A method and device for determining time coefficient of accelerated test of coastal concrete structure

By simulating the salt spray erosion environment of coastal concrete structures and calculating the accelerated test time coefficient, it solves the problem of difficulty in accurately simulating and accelerating the erosion of concrete structures in the existing technology, and achieves accurate research on the chloride ion erosion rules of concrete structures and life cycle safety. sexual assessment.

CN118518573BActive Publication Date: 2024-10-18SOUTHWEST JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411001240.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-18
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Existing technology is difficult to accurately simulate and accelerate the indoor salt spray erosion process of coastal concrete structures, and cannot effectively study the chloride ion erosion rules and life cycle safety of concrete structures.

Method used

By obtaining the real sea exposure environment information, setting the salt spray concentration, temperature and humidity of the salt spray test device, preprocessing and clamping the concrete samples, simulating the settlement and attached corrosion process, establishing a chloride ion concentration change curve, and fitting the formula to calculate The accelerated test time coefficient is used to characterize the corrosion acceleration degree of the test device.

Benefits of technology

It realizes the accelerated test of settlement and adherent corrosion of concrete structures, accurately calculates the accelerated test time coefficient, supports more accurate research on the laws of concrete erosion and deterioration, and provides important support for the safety evaluation of the entire life cycle of concrete structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118518573B_ABST
    Figure CN118518573B_ABST
Patent Text Reader

Abstract

The present invention provides a method and device for determining the time coefficient of an accelerated test of a coastal concrete structure, which relates to the field of testing technology and includes a main body module, a salt spray module and an environmental control module. The main body module includes a box body, and a fan, a horizontal rack and a heater are arranged in sequence from top to bottom inside the box body; a salt spray sedimentation measurement funnel is arranged at the center of the box body; and a plurality of clamping structures for clamping concrete samples are arranged on the rack. The salt spray module is connected to the main body module and is used to control the salt spray concentration and humidity inside the box body. The environmental control module is connected to the main body module and is used to monitor the salt spray concentration, temperature and humidity inside the box body. The present invention realizes the accelerated sedimentation corrosion test and the accelerated adhesion corrosion test of the concrete structure by pre-treating the concrete sample and cooperating with the clamping structure, and proposes a method for calculating the time coefficient of the accelerated test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of testing technology, and in particular to a method and a device for determining a time coefficient of an accelerated test of a coastal concrete structure. Background Art

[0002] Although the concrete building structures in coastal cities are not in direct contact with seawater, the salt-containing aerosols are carried to the surface of the concrete building structures by the sea breeze for sedimentation or attachment, and continue to erode the concrete. The erosion process is a long process from the outside to the inside, and indoor simulated accelerated tests are usually used to study its erosion laws. When using indoor simulated accelerated tests, it is necessary to scientifically and reasonably control environmental variables to restore the real service environment of the concrete structure, and it is also necessary to determine the multiple relationship between the actual sea exposure and the indoor simulated accelerated test time to explore the chloride ion erosion process in the concrete structure under various influencing factors. Summary of the invention

[0003] The purpose of the present invention is to provide a method and device for determining the time coefficient of the accelerated test of coastal concrete structures to solve the above problems. In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0004] On the one hand, the present application provides a method for determining a time factor of an accelerated test of a coastal concrete structure, comprising:

[0005] Acquire environmental information and first information of the actual sea exposure environment, wherein the environmental information includes salt spray concentration, temperature and humidity; the first information is the chloride ion concentration at a preset depth of the concrete structure under different exposure times;

[0006] Set the salt spray concentration, temperature and humidity of the salt spray test device according to the environmental information;

[0007] Pre-treating a plurality of concrete samples, and placing the plurality of pre-treated concrete samples into a set salt spray test device;

[0008] Different batches of concrete samples are taken out at different test times to obtain the average chloride ion concentration at a preset depth of each batch of concrete samples;

[0009] Establishing a first curve according to different test times and corresponding average chloride ion concentrations, and fitting the first curve by a preset function to obtain a fitting formula;

[0010] Establishing a second curve according to the first information, selecting multiple points from the rising stage of the second curve, obtaining the chloride ion concentration and exposure time corresponding to these points, wherein the abscissa of the second curve is the exposure time, and the ordinate is the chloride ion concentration, and the second curve is used to characterize the change of the chloride ion concentration of the concrete structure at a preset depth;

[0011] Substitute the chloride ion concentrations corresponding to these points into the fitting formula to obtain the test time corresponding to these points;

[0012] The exposure time corresponding to the same point is divided by the test time to obtain the acceleration factor of the point. The acceleration factors of all points are averaged to obtain the accelerated test time coefficient. The acceleration factor is used to characterize the degree of acceleration of corrosion of concrete structures by the salt spray test device.

[0013] On the one hand, the present application also provides a device for determining the time coefficient of the accelerated test of coastal concrete structures, including a main body module, a salt spray module and an environmental control module. The main body module includes a box body, and the inside of the box body is provided with a fan, a horizontal rack and a heater from top to bottom in sequence; a salt spray deposition measurement funnel is provided at the center of the box body; and a plurality of clamping structures for clamping concrete samples are provided on the rack. The salt spray module is connected to the main body module and is used to control the salt spray concentration and humidity inside the box body. The environmental control module is connected to the main body module and is used to monitor the salt spray concentration, temperature and humidity inside the box body.

[0014] The beneficial effects of the present invention are:

[0015] The present invention realizes the accelerated sedimentation corrosion test and the accelerated adhesion corrosion test of the concrete structure by pre-treating the concrete sample and cooperating with the clamping structure. The present invention calculates the accelerated test time coefficient by the accelerated test time required for the concrete sample to reach a certain amount of chloride ion concentration and the required actual sea exposure time. The accelerated test time coefficient can be used to more accurately study the corrosion and degradation law of concrete, and provide important support for accurately and scientifically evaluating the safety and reliability of concrete structures throughout their life cycle.

[0016] Other features and advantages of the present invention will be set forth in the following description, and in part will become apparent from the description, or may be understood by practicing embodiments of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 It is a three-dimensional schematic diagram of the device of the present invention;

[0019] Figure 2 is a schematic cross-sectional view of the device of the present invention;

[0020] Figure 3It is a three-dimensional schematic diagram of the clamping structure of the present invention;

[0021] Figure 4 It is a front view of the clamping structure of the present invention;

[0022] Figure 5 It is the first curve fitted in Example 2 of the present invention.

[0023] Markings in the figure:

[0024] 1. Main module; 2. Salt spray module; 3. Environmental control module; 4. Clamping structure; 41. Straight plate; 42. Fasteners; 5. Storage rack; 6. Fan; 7. Heater; 8. Heating water tank; 9. Pipeline; 10. Spray tower; 11. Salt spray deposition measurement funnel; 12. Salt spray compressor; 13. Transparent salt spray box cover. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention generally described and shown in the drawings herein can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings. At the same time, in the description of the present invention, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.

[0027] Embodiment 1:

[0028] like Figure 1 and Figure 2 As shown, this embodiment provides a device for determining the time coefficient of the accelerated test of coastal concrete structures, including: a main body module 1, a salt spray module 2 and an environment control module 3.

[0029] The main module 1 includes a box body, and a fan 6, a horizontal rack 5 and a heater 7 are arranged inside the box body from top to bottom in sequence; a salt spray deposition measurement funnel 11 is arranged at the center of the box body; and a plurality of clamping structures 4 for clamping concrete samples are arranged on the rack 5. The upper part of the box body is a detachable transparent salt spray box cover 13, which is convenient for observing the test conditions of the concrete samples and taking out the concrete samples. The main module 1 is used to construct a salt spray environment and complete the injection and discharge of salt spray. The fan 6 is used for the circulation of air in the box body. The heater 7 is used to control the temperature in the box body. The salt spray deposition measurement funnel 11 is used to collect the settled salt spray and obtain the salt spray deposition per unit area.

[0030] The salt spray module 2 is connected to the main body module 1 and is used to control the salt spray concentration and humidity inside the box. The salt spray module 2 includes a heating water tank 8, a spray tower 10 and a salt spray compressor 12. The heating water tank 8 and the salt spray compressor 12 are connected and arranged outside the box, and the spray tower 10 is arranged inside the box. The spray tower 10 is connected to the salt spray compressor 12 through a pipeline 9. A salt solution of a certain concentration is stored in the heating water tank 8, and the heating water tank 8 can control the temperature of the salt solution. The salt solution is converted into salt spray gas by the cooperation of the salt spray compressor 12 and the spray tower 10, and the salt spray gas is sprayed into the box.

[0031] The environmental control module 3 is connected to the main body module 1 and is used to monitor the salt spray concentration, temperature and humidity inside the box. The environmental control module 3 includes a concentration sensor, a temperature sensor and a humidity sensor arranged inside the box and a control unit arranged outside the box, and the concentration sensor, the temperature sensor and the humidity sensor are electrically connected to the control unit.

[0032] like Figure 3 and Figure 4 As shown, the clamping structure 4 includes two straight plates 41 and a plurality of fasteners 42 ; the two straight plates 41 are parallel to each other and connected by the fasteners 42 ; the straight plates 41 are perpendicular to the storage rack 5 .

[0033] It should be noted that the existing test devices usually place the test samples directly on the rack. This placement method can only simulate the sedimentation and corrosion process of the test samples in the real service environment, and the concrete structure will also be affected by pressure in the real service environment. Therefore, the factors considered by the existing test devices are still not comprehensive enough. The clamping structure 4 of this embodiment makes the bottom of the concrete sample suspended in the air after clamping the concrete sample. Therefore, this application can simulate the sedimentation and corrosion process of the top of the concrete structure in the real service environment, and can also simulate the adhesion and corrosion process of the bottom of the concrete structure in the real service environment. In addition, pressure can be applied to both ends of the concrete sample through the clamping structure 4 to simulate the stress conditions of the concrete structure in the real service environment and highly restore the real service environment of the concrete structure.

[0034] Embodiment 2:

[0035] This embodiment provides a method for determining the time coefficient of the accelerated test of coastal concrete structures, using the above-mentioned device, including the steps of:

[0036] S1. Acquire environmental information and first information of a real sea exposure environment, wherein the environmental information includes salt spray concentration, temperature and humidity; the first information is the chloride ion concentration at a preset depth of a concrete structure under different exposure times.

[0037] In this embodiment, the salt spray concentration of the environmental information is 18.0 μg / m 3 , temperature is 20.5℃, and humidity is 87.2%.

[0038] S2. Set the salt spray concentration, temperature and humidity of the salt spray test device according to the environmental information.

[0039] In some specific embodiments, step S2 includes:

[0040] S21, setting the salt spray concentration inside the salt spray test device to be greater than the salt spray concentration in the actual sea exposure environment as the first setting;

[0041] S22, setting the temperature inside the salt spray test device to be greater than the temperature in the actual sea exposure environment as the second setting;

[0042] S23, setting the humidity inside the salt spray test device to be greater than the humidity in the actual sea exposure environment as the third setting;

[0043] S24, selecting one or more of the first setting, the second setting or the third setting to set the salt spray test device.

[0044] It should be noted that after the salt spray test device is set, it is necessary to record the salt spray concentration corresponding to the first setting, the temperature corresponding to the second setting, and the humidity corresponding to the third setting. In this embodiment, a salt solution with a pre-configured concentration of 10% is placed in the heating water tank 8, and the salt spray box environment temperature is set to 35° C. and the humidity is set to 95%.

[0045] S3. Pre-treat a plurality of concrete samples, and place the plurality of pre-treated concrete samples into a set salt spray test device.

[0046] In this embodiment, the concrete sample is a cubic block of 100×100×100 mm, which is used to simulate the concrete structure in the real sea exposure environment.

[0047] In some specific embodiments, step S3 includes:

[0048] S31. Select one surface of the concrete sample as the corrosion surface.

[0049] S32. Grind the corroded surface with an angle grinder to remove the surface slurry, which is used to remove the attachments on the corroded surface of the concrete sample, making different concrete samples more comparable and improving the reliability of the test results. In addition, the attachments may contain substances that affect the corrosion process and cause test errors.

[0050] S33. The non-corrosive surface of the concrete sample is sealed with paraffin to prevent corrosion of the non-corrosive surface during the test. The chloride ion content inside the concrete sample increases, affecting the accuracy and reliability of the test results.

[0051] S34, placing the concrete sample between two straight plates 41, making the non-corroded surface contact the straight plates 41, and tightening the fasteners 42 to make the concrete sample suspended in the air.

[0052] Specifically, step S34 includes:

[0053] S341. Determine the stress of concrete structures in real sea exposure environment;

[0054] S342. By changing the rotation angle of the nut in the fastener 42 or by using other pressure devices to control the stress of the concrete sample, the stress of the concrete sample is made the same as that of the concrete structure in the actual sea exposure environment.

[0055] The stress on the concrete structure will affect the speed of the corrosion process. In the early stage of service, a passivation layer is formed due to the high alkalinity of the pore fluid in the concrete, which effectively prevents the steel bars from being corroded. However, the carbonization of the concrete and the chloride ion erosion in the later stage will lead to the destruction of the passivation film and cause corrosion of the concrete structure. The chloride ion invasion corrosion area is small but the corrosion depth is large, which can easily cause structural stress concentration and brittle failure without warning. When the concrete structure is subjected to external loads, the corrosion process will be aggravated. Steps S341 and S342 simulate the pressure conditions of the concrete structure in the actual sea exposure environment, so that the accelerated test is closer to the actual sea exposure environment.

[0056] S35, placing the clamping structure 4 with the installed concrete sample into the set salt spray test device.

[0057] It should be noted that adhesion corrosion is the process in which corrosion ions are adsorbed to the bottom surface of the concrete structure without the influence of gravity to cause corrosion, and sedimentation corrosion is the process in which corrosion ions settle to the upper surface of the concrete structure under the influence of gravity to cause corrosion. The accumulated amount of corrosion ions on different surfaces of the concrete structure is different, resulting in different corrosion rates. In this embodiment, when the corrosion surface of the concrete sample in the box is placed upward, it is used to simulate the sedimentation corrosion process of the top of the concrete structure in the real service environment; when the corrosion surface of the concrete sample in the box is placed downward, it is used to simulate the adhesion corrosion process of the bottom of the concrete structure in the real service environment.

[0058] Concrete structures are usually irregular in shape, and inclined surfaces often experience both sedimentation corrosion and adhesion corrosion. Therefore, the corrosion surface can also be installed in the clamping structure 4 with an inclined upward direction to simultaneously simulate the sedimentation corrosion process and adhesion corrosion process of the concrete structure in a real service environment.

[0059] S4. Take out different batches of concrete samples after different test times, and obtain the average chloride ion concentration of each batch of concrete samples at a preset depth.

[0060] In this embodiment, the preset depth is 30 mm. A batch of concrete samples is taken out every 10 days, and multiple drillings are performed on each concrete sample at a depth of 30 mm vertically away from the corrosion surface, so that the error of each drilling depth is strictly controlled within one millimeter. The multiple drillings of the same concrete sample are mixed, dried, ground, sieved, weighed and dissolved to determine the chloride ion concentration of the concrete sample. The average value of the chloride ion concentration of the same batch of concrete samples at a depth of 30 mm is taken as the average chloride ion concentration of the batch of concrete samples at a depth of 30 mm.

[0061] S5. Establish a first curve according to different test times and corresponding average chloride ion concentrations, and obtain a fitting formula by fitting the first curve through a preset function.

[0062] The default functions are:

[0063]

[0064] Wherein, C represents the chloride ion concentration; t represents the test time; t0 represents the time when the first curve reaches the peak value; dX represents the parameter related to the chloride ion diffusion rate; A1 represents the low peak value of the first curve; A2 represents the high peak value of the first curve; and e represents a natural constant.

[0065] It should be noted that the curve formed by the preset function is flat and rising, which is consistent with the changing trend of chloride ion concentration at a certain depth of the concrete structure, and the fitting effect of the preset function is good.

[0066] In this embodiment, after different test times, the chloride ion concentrations at different depths of the concrete samples are obtained as shown in Table 1.

[0067] Table 1

[0068]

[0069] The first curve fitted according to the data of 30 mm depth in Table 1 is as follows Figure 5 As shown, the fitting formula is:

[0070]

[0071] Wherein, C represents the chloride ion concentration; t represents the test time; and e represents a natural constant.

[0072] S6. Establish a second curve based on the first information, randomly select multiple points from the rising stage of the second curve, and obtain the chloride ion concentration and exposure time corresponding to these points. The abscissa of the second curve is the exposure time, and the ordinate is the chloride ion concentration. The second curve is used to characterize the change of chloride ion concentration of the concrete structure at a preset depth.

[0073] In this embodiment, one of the points is a concrete sample that has been exposed to the sea for 18 years, and the chloride ion concentration at a depth of 30 mm is 0.1123%.

[0074] S7. Substitute the chloride ion concentrations corresponding to these points into the fitting formula to obtain the test times corresponding to these points.

[0075] In this embodiment, 0.1123% is substituted into the fitting formula, and the test time at this point is calculated to be 62 days.

[0076] S8. Divide the exposure time and test time corresponding to a point to obtain the acceleration factor of the point, and average the acceleration factors of all points to obtain the accelerated test time coefficient. The acceleration factor is used to characterize the degree of acceleration of corrosion of a concrete structure by the salt spray test device.

[0077] In this embodiment, the acceleration factor at this point = 18 years / 62 days = 105.96.

[0078] Calculate the acceleration ratios of other points, eliminate the acceleration ratios with errors greater than 20%, take the average of the multiple acceleration ratios after elimination, and obtain the acceleration test time coefficient.

[0079] Since different salt spray concentrations, temperatures and humidity are set inside the box, the accelerated test time coefficients are different. In some specific embodiments, step S9 is further included. Step S9 specifically includes:

[0080] S91, changing one or more of the salt spray concentration, temperature or humidity inside the salt spray test device, establishing different first curves, and obtaining a fitting formula corresponding to each first curve;

[0081] S92, substituting the chloride ion concentration corresponding to the point into the fitting formula corresponding to different first curves to obtain different test times corresponding to the point;

[0082] S93, dividing the exposure time corresponding to the point by the different test times corresponding to the point to obtain accelerated test time coefficients of different sizes;

[0083] S94. Record the salt spray concentration, temperature and humidity corresponding to each accelerated test time coefficient.

[0084] Step S9 can obtain the salt spray concentration, temperature and humidity corresponding to the accelerated test time coefficients of different sizes, laying a foundation for the subsequent study of the relationship between the salt spray concentration, temperature and humidity and the chloride ion corrosion law.

[0085] In some specific embodiments, this embodiment further includes step S10, and step S10 specifically includes:

[0086] S101, selecting an accelerated test time coefficient according to the required salt spray test time, and setting a salt spray test device according to the salt spray concentration, temperature and humidity corresponding to the selected accelerated test time coefficient;

[0087] S102, conducting a test according to the set salt spray test device to obtain the corresponding average chloride ion concentration at different times, wherein the average chloride ion concentration is the chloride ion concentration of multiple concrete samples at a preset depth;

[0088] S103, establishing a third curve according to the average chloride ion concentration corresponding to all the time periods, wherein the abscissa of the third curve is the time period and the ordinate is the average chloride ion concentration, and the third curve is used to characterize the change in chloride ion concentration of the concrete structure at a preset depth;

[0089] S104, obtaining the time corresponding to the point on the third curve that reaches the chloride ion concentration limit;

[0090] S105. Multiply the time corresponding to the point at which the chloride ion concentration limit is reached by the selected accelerated test time coefficient to obtain the predicted life of the concrete sample.

[0091] Step S10 provides a method for predicting the life of concrete samples. Based on the accelerated test time coefficient obtained in step S9 and the corresponding salt spray concentration, temperature and humidity, the life prediction of concrete samples becomes simple and easy to operate, and the prediction results are true and reliable, providing an important reference for engineering design and maintenance. In addition, selecting a large value of the accelerated test time coefficient can quickly predict the life of concrete samples.

[0092] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

[0093] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for determining the time coefficient of accelerated testing of coastal concrete structures, characterized in that: include: Acquire environmental information and first information of the actual sea exposure environment, wherein the environmental information includes salt spray concentration, temperature and humidity; the first information is the chloride ion concentration at a preset depth of the concrete structure under different exposure times; Set the salt spray concentration, temperature and humidity of the salt spray test device according to the environmental information; Pre-treating a plurality of concrete samples, and placing the plurality of pre-treated concrete samples into a set salt spray test device; Different batches of concrete samples are taken out at different test times to obtain the average chloride ion concentration at a preset depth of each batch of concrete samples; Establishing a first curve according to different test times and corresponding average chloride ion concentrations, and fitting the first curve by a preset function to obtain a fitting formula; A second curve is established according to the first information, and a plurality of points are randomly selected from the rising phase of the second curve to obtain the chloride ion concentration and exposure time corresponding to these points, wherein the abscissa of the second curve is the exposure time, and the ordinate is the chloride ion concentration, and the second curve is used to characterize the change of the chloride ion concentration of the concrete structure at a preset depth under the actual sea exposure environment; Substitute the chloride ion concentrations corresponding to these points into the fitting formula to obtain the test time corresponding to these points; Divide the exposure time and test time corresponding to a point to obtain the acceleration factor of the point, and average the acceleration factors of all points to obtain the accelerated test time coefficient. The acceleration factor is used to characterize the degree of acceleration of corrosion of a concrete structure by the salt spray test device; Among them, the salt spray concentration, temperature and humidity inside the salt spray test device are set according to the environmental information, including: The salt spray concentration inside the salt spray test device is set to be greater than the salt spray concentration in the actual sea exposure environment as the first setting; The temperature inside the salt spray test device is set to be greater than the temperature in the actual sea exposure environment as the second setting; The humidity inside the salt spray test device is greater than the humidity in the actual sea exposure environment as the third setting; Select one or more of the first setting, the second setting or the third setting to set the salt spray test device.

2. The method for determining the time coefficient of the accelerated test of coastal concrete structures according to claim 1, characterized in that: Pre-treating a plurality of concrete samples, and placing the plurality of pre-treated concrete samples into a set salt spray test device, including: Select one surface of the concrete sample as the corrosion surface; Use an angle grinder to grind the corroded surface to remove the surface slurry; The non-corroded surface of the concrete specimens was sealed by paraffin wax; The concrete sample is placed between two straight plates (41) so that the non-corroded surface contacts the straight plates (41), and the fasteners (42) are tightened so that the concrete sample is suspended in the air; The clamping structure (4) with the concrete sample installed is placed into the set salt spray test device.

3. The method for determining the time coefficient of the accelerated test of coastal concrete structures according to claim 1, characterized in that: Also includes: Changing one or more of the salt spray concentration, temperature or humidity inside the salt spray test device, establishing different first curves, and obtaining a fitting formula corresponding to each first curve; Substituting the chloride ion concentration corresponding to the point into the fitting formula corresponding to different first curves to obtain different test times corresponding to the point; Divide the exposure time corresponding to the point by the different test times corresponding to the point to obtain accelerated test time coefficients of different sizes; Record the salt spray concentration, temperature and humidity corresponding to each accelerated test time coefficient.

4. The method for determining the time coefficient of the accelerated test of coastal concrete structures according to claim 3, characterized in that: Also includes: Select an accelerated test time coefficient according to the required salt spray test time, and set up the salt spray test device according to the salt spray concentration, temperature and humidity corresponding to the selected accelerated test time coefficient; Conducting a test according to the set salt spray test device to obtain the corresponding average chloride ion concentration at different times, wherein the average chloride ion concentration is the chloride ion concentration of multiple concrete samples at a preset depth; A third curve is established according to the average chloride ion concentration corresponding to all the times, wherein the abscissa of the third curve is the time and the ordinate is the average chloride ion concentration, and the third curve is used to characterize the change of the chloride ion concentration of the concrete structure at a preset depth; Obtaining the time corresponding to the point on the third curve where the chloride ion concentration limit is reached; The predicted life of the concrete sample is obtained by multiplying the time corresponding to the point where the chloride ion concentration limit is reached by the selected accelerated test time coefficient.

5. A device for determining the time coefficient of the accelerated test of coastal concrete structures, used to implement the method of claim 1, characterized in that: include: A main body module (1), the main body module (1) comprising a box body, wherein a fan (6), a horizontal storage rack (5) and a heater (7) are arranged in sequence from top to bottom inside the box body; a salt spray deposition measurement funnel (11) is arranged at the center of the box body; and a plurality of clamping structures (4) for clamping concrete samples are arranged on the storage rack (5); A salt spray module (2), the salt spray module (2) being connected to the main body module (1) and being used to control the salt spray concentration and humidity inside the box; An environmental control module (3), the environmental control module (3) being connected to the main body module (1) and being used to monitor the salt spray concentration, temperature and humidity inside the box; Wherein, the clamping structure (4) comprises two straight plates (41) and a plurality of fasteners (42); the two straight plates (41) are parallel to each other and connected via the fasteners (42); and the straight plates (41) are perpendicular to the storage rack (5).

6. The device for determining the time coefficient of the accelerated test of coastal concrete structures according to claim 5, characterized in that: The salt spray module (2) comprises a heating water tank (8), a spray tower (10) and a salt spray compressor (12); the heating water tank (8) and the salt spray compressor (12) are connected and arranged outside the box; the spray tower (10) is arranged inside the box; and the spray tower (10) is connected to the salt spray compressor (12) via a pipeline (9).

7. The device for determining the time coefficient of the accelerated test of coastal concrete structures according to claim 5, characterized in that: The environmental control module (3) comprises a concentration sensor, a temperature sensor and a humidity sensor arranged inside the box body, and a control unit arranged outside the box body, wherein the concentration sensor, the temperature sensor and the humidity sensor are all electrically connected to the control unit.

8. The device for determining the time coefficient of the accelerated test of coastal concrete structures according to claim 5, characterized in that: The upper part of the box body is a detachable transparent salt spray box cover (13).

Citation Information

Patent Citations

  • Method for rapidly predicting service life of reinforced concrete in chlorine salt environment

    CN103487480A

  • Reinforced concrete member service life prediction method based on chloride ion concentration monitoring

    CN112529255A