A low-stress graphite growth ring, guide tube and silicon carbide single crystal growth method

By pre-treating the graphite growth ring and guide tube to form a pyrolytic or glassy carbon coating, combined with a multiple barrier structure, the problem of erosion of the graphite growth ring and guide tube at high temperatures is solved, and the growth of silicon carbide single crystal is improved. speed and quality, reducing cost and operational complexity.

CN118529732BActive Publication Date: 2024-10-11LINGFENG INVESTMENT (SHANTOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410998916.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-11
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

In the existing silicon carbide single crystal growth method, the graphite growth ring and flow guide tube are easily eroded by SixCy gas at high temperatures, resulting in low efficiency and high cost of the crystal growth device, and the operation is complicated. It is difficult to avoid carbon particles entering the growth area and affecting the crystal quality. .

Method used

Pretreatment methods of low-stress graphite growth rings and guide tubes are used, including sandblasting, ultrasonic cleaning, vacuum coating of phenolic resin glue, low-temperature curing and high-temperature carbonization to form pyrolytic carbon or glassy carbon coatings, combined with multiple Barrier structure to isolate SixCy gas and impurities to ensure the stability and purity of the growth environment.

Benefits of technology

The thermal stress of the crystal growth device is reduced, the growth rate and quality of silicon carbide single crystals are improved, the density of carbon inclusions and impurities is reduced, and the cost and operational complexity are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118529732B_ABST
    Figure CN118529732B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-stress graphite growth ring, a guide tube and a silicon carbide single crystal growth method, comprising the following steps: (1) pre-treating the two graphite parts of the graphite growth ring and the guide tube; (2) performing high-temperature carbonization treatment on the graphite parts; (3) loading high-purity silicon carbide powder into the inner cavity of the growth container; loading the entire growth container into a growth furnace; (4) evacuating the inner cavity of the growth container and replacing high-purity argon gas twice in the middle; starting to slowly increase the temperature; then slowly increasing the growth temperature to above 2300°C, and slowly reducing the pressure to the growth pressure of the single crystal, so that the high-purity silicon carbide powder passes through the powder filter, the guide tube, the graphite growth ring, and the graphite support from bottom to top in sequence, and then grows into a low-stress silicon carbide single crystal on a seed wafer. The present invention has low cost, simple operation, and can increase the growth rate of the crystal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor materials, and in particular to a low-stress graphite growth ring, a guide tube and a silicon carbide single crystal growth method. Background Art

[0002] In the efficient and fast-paced information society, high temperature, high pressure, high frequency and high power have become a threshold that we must overcome in our development. As the representative of the third-generation wide-bandgap semiconductor materials, silicon carbide, due to its material structural characteristics, can almost perfectly match the above advantages in application. Especially in recent years, the emerging new energy market has initially witnessed its highlight moment.

[0003] Since silicon carbide does not exist in a stoichiometric melt at room temperature and pressure, it cannot be prepared and produced using a mature and efficient Czochralski method. At present, the most commonly used and mature method for preparing silicon carbide single crystals at home and abroad is the physical vapor transport (PVT) method. It is under the protection of high-purity dynamic inert gas, in a suitable temperature field established by induction heating or graphite resistance heating, after the high-purity silicon carbide powder is decomposed and sublimated in the high-temperature source material area of ​​the growth cavity, it is transported to the low-temperature seed crystal guide area under the action of the thermal field temperature gradient and the material gas phase concentration gradient, and rearranged in an atomic-level regular manner in the low-temperature seed crystal guide area and crystallized and grown.

[0004] The entire PVT single crystal growth process is carried out in a high-temperature, low-pressure, closed chamber. As the high temperature continues, the high-purity silicon carbide powder will decompose and sublimate to produce high-temperature dynamic Si concentrated near the wafer. x C y Gas, Si x C y The gas will not only continuously erode the graphite growth ring and guide tube of the loose or porous carbon structure around the wafer, but also directly react with the silicon-rich atmosphere to cause the crystal edge to be wetted and adhered, disrupting the carbon-silicon atmosphere balance ratio. x C y The gas may contain carbon particles, which may directly enter the growing crystal, destroying the multiple filtration structures of the crystal growth device and causing the filtration of the crystal growth device to fail. x C y Gas, currently two structures are commonly used: one is to use a high-temperature refractory metal TaC coating structure applied to the graphite growth ring and guide tube in the growth chamber. The high-temperature refractory metal TaC coating can protect the graphite material from being Si at high temperatures. x C yGas erosion and destruction; second, the use of pyrolytic carbon or pyrolytic graphite buffer transition layer structure applied to the low-temperature seed crystal guide area of ​​the growth cavity as the substrate for the silicon carbide growth crystal to provide good growth conditions for the crystal. Although the above-mentioned high-temperature refractory metal TaC coating structure can be used to prevent graphite from being directly exposed to the silicon-rich atmosphere and reduce the corrosion and contamination of the surrounding graphite substrate to the silicon-carbon atmosphere and crystals, the cost of TaC coating is high, and the thermal expansion coefficient of TaC coating and the base carbon material is quite different, which is prone to delamination and peeling during use. At the same time, the use of TaC coating will partially change the thermal field structure and reduce the growth rate of silicon carbide growth crystals. The use of pyrolytic carbon or pyrolytic graphite buffer transition layer structure can largely avoid the decomposition and sublimation of high-temperature dynamic Si x C y Gas, but its operation process is complicated and it is easily corroded by silicon. Summary of the invention

[0005] The problem to be solved by the present invention is to provide a low stress graphite growth ring, a guide tube and a silicon carbide single crystal growth method. The low stress graphite growth ring, the guide tube and the silicon carbide single crystal growth method have low cost, simple operation and can improve the growth rate of the crystal.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A low stress graphite growth ring, a guide tube and a silicon carbide single crystal growth method, characterized by comprising the following steps:

[0008] (1) Pre-treatment of the two graphite parts, graphite growth ring and guide tube:

[0009] (1-1) sandblasting the inner surface of the graphite growth ring;

[0010] (1-2) Graphite parts purification: After degreasing the graphite parts, ultrasonic cleaning and low-temperature drying, the graphite parts are placed in a high-temperature furnace, inert gas is introduced under vacuum, and carbonization treatment is performed under high-temperature conditions;

[0011] (1-3) Vacuum spraying or dipping: Place the purified graphite parts into the inner cavity of the infiltration curing device, evacuate the inner cavity of the infiltration curing device, and when the vacuum degree is ≤5 Pa, spray the graphite parts with phenolic resin glue or modified phenolic resin glue; or dip the graphite parts with phenolic resin glue or modified phenolic resin glue;

[0012] (1-4) One-time vacuum infiltration: the surface and interior of the graphite part are completely infiltrated with phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours to obtain carbon glue;

[0013] (1-5) Primary low-temperature curing: After filling the inner cavity of the coating curing device with argon gas to 1 standard atmospheric pressure, open the lower glue leakage port of the coating curing device to release the carbon glue; after the residual glue on the surface of the graphite part is drained away, continuously circulate argon gas into the inner cavity of the coating curing device, and then heat and ventilate it to solidify the remaining carbon glue on the surface of the graphite part;

[0014] (1-6) Secondary coating: The surface and interior of the graphite part are completely infiltrated in phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours to obtain carbon glue;

[0015] (1-7) Secondary low-temperature curing: After filling the inner cavity of the coating curing device with argon gas to 1 standard atmospheric pressure, open the lower liquid discharge port of the coating curing device to release the carbon glue; after the residual glue on the surface of the graphite part is drained away, continuously circulate argon gas into the inner cavity of the coating curing device, and then heat and ventilate it to solidify the remaining carbon glue on the surface of the graphite part;

[0016] (2) High-temperature carbonization treatment: Place the graphite parts after the secondary low-temperature curing treatment into a vacuum pressure furnace, evacuate the inner cavity of the vacuum pressure furnace to below 5 Pa, fill it with 1.5Mpa-2.0Mpa high-purity argon gas, raise the temperature to 2200-2500°C at a rate of 0.05°C / m-0.5°C / m, and maintain the temperature for 8 hours-12 hours to complete the high-temperature carbonization, so as to obtain a graphite growth ring and a guide tube with a pyrolytic carbon coating or a glassy carbon coating on the surface, and take the graphite growth ring and the guide tube out of the inner cavity of the infiltration curing device for standby use;

[0017] (3) High-purity silicon carbide powder is loaded into the inner cavity of the growth container; the growth container is provided with a powder filter, a graphite holder and a seed wafer, the powder filter is horizontally installed in the inner cavity of the growth container, the guide tube, the graphite growth ring and the graphite holder are arranged in sequence from bottom to top above the powder filter and in the inner cavity of the growth container, and the seed wafer is bonded to the graphite holder; the entire growth container is loaded into the growth furnace;

[0018] (4) The inner cavity of the growth container is evacuated and replaced with high-purity argon twice; when the vacuum degree of the inner cavity of the growth container reaches 5×10 -4 pa or above, start to slowly heat up; when the inner cavity temperature of the growth container reaches 800℃-1000℃, continue to fill with 800mbar-900mbar argon, slowly increase the growth temperature to above 2300℃, and slowly reduce the pressure to the growth pressure of the single crystal 1mbar-5mbar, so that the high-purity silicon carbide powder passes through the powder filter, guide tube, graphite growth ring, and graphite support from bottom to top in sequence, and then grows into a low-stress silicon carbide single crystal on the seed wafer.

[0019] In a preferred embodiment, in step (1-1), the inner surface of the graphite growth ring is sandblasted with 10-200 mesh diamond sand and 1atm-5atm compressed air. Sandblasting can effectively improve the inner surface roughness of the graphite growth ring, increase the surface area of ​​the material, and effectively buffer the thermal stress of different materials at high temperatures.

[0020] In a further preferred embodiment, the surface sandblasting treatment in step (1-1) is as follows: the inner surface of the graphite growth ring is uniformly sandblasted using 60-80 mesh diamond sand and 2atm-3atm compressed air.

[0021] In a preferred embodiment, in step (1-2), the graphite piece is placed in a high-temperature furnace, argon gas is introduced under a vacuum environment, and carbonization treatment is performed at a high temperature of 2500° C. to 2800° C. for 60 min to 120 min.

[0022] Typically, the degreasing step in step (1-2) is as follows: use a suitable solvent or detergent to remove grease and dirt on the surface of the graphite part.

[0023] Generally, the ultrasonic cleaning step in step (1-2) is as follows: the graphite piece is placed in an ultrasonic cleaning device, and the surface of the graphite piece is cleaned using high-frequency sound wave vibration. This ultrasonic cleaning can enhance the cleaning effect on the surface of the graphite piece and remove the dirt and impurities remaining on the surface of the graphite piece.

[0024] Generally, the low-temperature drying step in step (1-2) is as follows: drying the surface of the cleaned graphite piece at a low temperature of 100°C-110°C to ensure that the surface of the graphite piece is dry. This low-temperature drying can maintain temperature stability and an appropriate drying time, so that the moisture on the surface of the graphite piece evaporates, but will not affect the thermal stress of the graphite piece, thus preparing for subsequent purification treatment.

[0025] In the above steps (1-2), during the purification process, it is necessary to control parameters such as vacuum degree, gas flow rate and temperature so that impurities can be volatilized or reacted to be removed to ensure that the graphite parts reach the required purity and performance.

[0026] The graphite parts in the above step (2) are vacuum dip-coated or spray-coated with phenolic resin or modified phenolic resin, and slowly heated and carbonized to obtain graphite growth rings and guide tubes with pyrolytic carbon coatings or glassy carbon coatings on the surface. These pyrolytic carbon coatings or glassy carbon coatings can effectively isolate Si x C y Gas, reducing its erosion and damage to graphite parts, thereby maintaining a good carbon-silicon atmosphere balance ratio, which is conducive to crystal growth.

[0027] In the above step (3), the powder filter, guide tube, graphite growth ring, graphite support and seed plate are reasonably arranged to form multiple barriers, reduce the possibility of impurities and carbon particles entering the growth area, improve the purity and quality of the crystal, ensure the uniform distribution and stability of the airflow during the growth process, and prevent the adverse effects of airflow disturbance on crystal growth. The above powder filter can effectively filter out impurities and large particles in the silicon carbide powder, ensure that the powder entering the growth area is purer, and is conducive to the high-quality growth of the crystal.

[0028] The vacuuming in the above step (4) can remove the air and impurities inside the growth container, ensuring the formation of a stable carbon-silicon atmosphere at high temperature; replacing the high-purity argon gas twice in the middle can further remove the residual gas and impurities, ensuring the purity of the final growth environment; slowly increasing the temperature can help to uniformly heat and avoid structural damage caused by thermal stress; slowly reducing the pressure to the growth pressure of the single crystal can help to form a high-quality low-stress silicon carbide single crystal and avoid the formation of bubbles and defects.

[0029] In a preferred embodiment, in the steps (1-5), after the residual glue on the surface of the graphite piece is drained away for 2 to 5 hours, argon gas at 150°C to 250°C is continuously circulated into the inner cavity of the diffusion coating and curing device for 50 to 100 hours of heating and ventilation to cure the remaining carbon glue on the surface of the graphite piece.

[0030] In a preferred embodiment, in the step (1-7), after the residual glue on the surface of the graphite part is drained away for 2 to 5 hours, argon gas at 150°C to 250°C is continuously circulated into the inner cavity of the diffusion coating and curing device for 50 to 100 hours of heating and ventilation to cure the remaining carbon glue on the surface of the graphite part.

[0031] In the preferred embodiment, the coating and curing device in the step (1-3) comprises a vacuum glue storage chamber, a glue draining basket, a hair dryer and a gas heater, a glue injection port and a pressure relief port are provided on the top of the vacuum glue storage chamber, a glue leakage port and an air inlet are provided on the bottom of the vacuum glue storage chamber, a vacuum port and an air outlet are provided on the side wall of the vacuum glue storage chamber, the glue injection port, the pressure relief port, the glue leakage port, the air inlet, the vacuum port and the air outlet are all connected to the inner cavity of the vacuum glue storage chamber, and the glue injection port, the pressure relief port, the glue leakage port, the air inlet, the vacuum port and the air outlet are all provided with a first switch valve; the hair dryer and the gas heater are both arranged on the outside of the vacuum glue storage chamber and are sequentially connected between the air outlet and the air inlet, the gas heater is provided with a first air inlet, and the first air inlet is provided with a second switch valve; the glue draining basket Installed in the lower part of the inner cavity of the vacuum glue storage chamber, the glue draining basket is provided with a plurality of glue draining holes on the bottom and side walls; first open the vacuum glue storage chamber, put the graphite parts on the glue draining basket and close the vacuum glue storage chamber; then, open the first switch valve, use an external vacuum pump to evacuate the inner cavity of the entire vacuum glue storage chamber through the vacuum port, and exhaust the gas inside the graphite parts. When the vacuum degree is ≤5pa, inject phenolic resin or modified phenolic resin glue from the glue injection port, and inject solvent from the glue injection port at the same time; then, use an external glue liquid supply device to inject glue liquid into the inner cavity of the vacuum glue storage chamber through the glue injection port. When the graphite parts are infiltrated with glue, the residual glue on the surface of the graphite parts will drain out, and the drained residual glue will be collected at the bottom of the vacuum glue storage chamber through the plurality of glue draining holes on the glue draining basket.

[0032] In a further preferred embodiment, the solvent is one of acetone, ethanol, furfuryl alcohol or propylene glycol methyl ether acetate, but is not limited to the above ingredients. The above propylene glycol methyl ether acetate is a high-grade industrial solvent with excellent performance, which has a strong solubility for both polar and non-polar substances and is suitable for solvents of various polymers in high-grade coatings and inks.

[0033] In a further preferred embodiment, in the steps (1-4), after the surface and interior of the graphite part are completely infiltrated in the phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours, the pressure relief port at the top of the vacuum glue storage chamber is slowly opened, and after argon gas is filled into the inner cavity of the vacuum glue storage chamber to 1 standard atmospheric pressure, the glue leakage port at the bottom of the vacuum glue storage chamber is opened to discharge the leaked residual glue from the glue leakage port.

[0034] In a further preferred embodiment, in the step (1-5), after the residual glue is exhausted, the air inlet at the bottom of the vacuum glue storage chamber and the first air inlet of the gas heater are opened, argon gas is introduced from the first air inlet of the gas heater, the argon gas is heated to 150°C-250°C by the gas heater, and then the heated argon gas is transported to the vacuum glue storage chamber through the air inlet by a hair dryer to perform a primary curing treatment on the carbon glue on the graphite part.

[0035] In a further preferred embodiment, in the step (1-7), after the residual glue on the surface of the graphite part has been drained away for 2 to 5 hours, the first air inlet of the gas heater is closed, and the air inlet and the air outlet at the bottom of the vacuum glue storage chamber are opened respectively, so that the air outlet, the heater, the hair dryer, the air inlet and the inner cavity of the vacuum glue storage chamber are connected in sequence, and the argon gas coming out of the air outlet is heated to 150°C-250°C by the gas heater, and then the heated argon gas is continuously circulated and transported to the vacuum glue storage chamber through the air inlet by the hair dryer, so as to perform a secondary curing treatment on the graphite part.

[0036] Compared with the prior art, the present invention has the following advantages:

[0037] The present invention pre-treats two graphite parts, a graphite growth ring and a guide tube, performs vacuum degassing, automatic glue infiltration, automatic glue leaching, and automatic low-temperature curing treatments on the graphite parts, and then performs high-temperature carbonization treatment on the graphite parts. This can increase the continuous stability of the crystal growth environment, improve the growth rate of the crystal, reduce the thermal stress of the crystal during continuous high-temperature growth, and reduce the density of carbon inclusions and other impurities or defects in the crystal at a lower cost and with lower porosity and specific surface area. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a structural schematic diagram of a penetration coating and curing device in a specific embodiment of the present invention;

[0039] Figure 2 It is a schematic diagram of the structure of a growth furnace and a growth container in a specific embodiment of the present invention. DETAILED DESCRIPTION

[0040] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0041] like Figure 1-2 As shown, the low stress graphite growth ring, guide tube and silicon carbide single crystal growth method in this embodiment include the following steps:

[0042] (1) Pre-treating the two graphite parts, graphite growth ring 5 and guide tube 6:

[0043] (1-1) performing sandblasting on the inner surface of the graphite growth ring 5;

[0044] (1-2) Graphite parts purification: After degreasing the graphite parts, ultrasonic cleaning and low-temperature drying, the graphite parts are placed in a high-temperature furnace, inert gas is introduced under vacuum, and carbonization treatment is performed under high-temperature conditions;

[0045] (1-3) Vacuum spraying or dipping: Place the purified graphite parts into the inner cavity of the infiltration curing device, evacuate the inner cavity of the infiltration curing device, and when the vacuum degree is ≤5 Pa, spray the graphite parts with phenolic resin glue or modified phenolic resin glue; or dip the graphite parts with phenolic resin glue or modified phenolic resin glue;

[0046] (1-4) One-time vacuum infiltration: the surface and interior of the graphite part are completely infiltrated with phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours to obtain carbon glue;

[0047] (1-5) Primary low-temperature curing: After filling the inner cavity of the coating curing device with argon gas to 1 standard atmospheric pressure, the lower glue leakage port 13 of the coating curing device is opened to release the carbon glue; after the residual glue on the surface of the graphite part is drained away, argon gas is continuously circulated into the inner cavity of the coating curing device, and then heating and ventilation are performed to solidify the remaining carbon glue on the surface of the graphite part;

[0048] (1-6) Secondary coating: The surface and interior of the graphite part are completely infiltrated in phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours to obtain carbon glue;

[0049] (1-7) Secondary low-temperature curing: After filling the inner cavity of the coating curing device with argon gas to 1 standard atmospheric pressure, open the lower liquid discharge port of the coating curing device to release the carbon glue; after the residual glue on the surface of the graphite part is drained away, continuously circulate argon gas into the inner cavity of the coating curing device, and then heat and ventilate it to solidify the remaining carbon glue on the surface of the graphite part;

[0050] (2) High-temperature carbonization treatment: the graphite parts after the secondary low-temperature curing treatment are placed in a vacuum pressure furnace, the inner cavity of the vacuum pressure furnace is evacuated to below 5 Pa, and filled with 1.5Mpa-2.0Mpa high-purity argon gas, and the temperature is raised to 2200°C-2500°C at a rate of 0.05°C / m-0.5°C / m, and the high-temperature carbonization is completed at a constant temperature for 8 hours-12 hours, so that the graphite growth ring 5 and the guide tube 6 with a pyrolytic carbon coating or a glassy carbon coating on the surface are obtained, and the graphite growth ring 5 and the guide tube 6 are taken out from the inner cavity of the infiltration curing device for standby use;

[0051] (3) High-purity silicon carbide powder 9 is loaded into the inner cavity of the growth container 7; the growth container 7 is provided with a powder filter 71, a graphite holder 72 and a seed chip 73, the powder filter 71 is horizontally installed in the inner cavity of the growth container 7, the guide tube 6, the graphite growth ring 5 and the graphite holder 72 are arranged in sequence from bottom to top above the powder filter 71 and in the inner cavity of the growth container 7, and the seed chip 73 is bonded to the graphite holder 72; the entire growth container 7 is loaded into the growth furnace 8;

[0052] (4) The inner cavity of the growth container 7 is evacuated and replaced with high-purity argon twice; when the vacuum degree of the inner cavity of the growth container 7 reaches 5×10 -4 pa or more, start to slowly heat up; when the inner cavity temperature of the growth container 7 reaches 800℃-1000℃, continue to fill with 800mbar-900mbar argon, slowly increase the growth temperature to above 2300℃, and slowly reduce the pressure to the growth pressure of the single crystal 1mbar-5mbar, so that the high-purity silicon carbide powder 9 passes through the powder filter 71, the guide tube 6, the graphite growth ring 5, and the graphite support 72 from bottom to top, and then grows into a low stress silicon carbide single crystal on the seed chip 73.

[0053] The surface sandblasting treatment in step (1-1) is as follows: 60-80 mesh diamond sand and 2atm-3atm compressed air are used to uniformly sandblast the inner surface of the graphite growth ring 5. Sandblasting can effectively improve the inner surface roughness of the graphite growth ring 5, increase the surface area of ​​the material, and effectively buffer the thermal stress of different materials at high temperatures.

[0054] In step (1-2), the graphite piece is placed in a high-temperature furnace, argon gas is introduced under a vacuum environment, and carbonization treatment is performed at a high temperature of 2500° C. to 2800° C. for 60 min to 120 min.

[0055] Typically, the degreasing step in step (1-2) is as follows: use a suitable solvent or detergent to remove grease and dirt on the surface of the graphite part.

[0056] Generally, the ultrasonic cleaning step in step (1-2) is as follows: the graphite piece is placed in an ultrasonic cleaning device, and the surface of the graphite piece is cleaned using high-frequency sound wave vibration. This ultrasonic cleaning can enhance the cleaning effect on the surface of the graphite piece and remove the dirt and impurities remaining on the surface of the graphite piece.

[0057] Generally, the low-temperature drying step in step (1-2) is as follows: drying the surface of the cleaned graphite piece at a low temperature of 100°C-110°C to ensure that the surface of the graphite piece is dry. This low-temperature drying can maintain temperature stability and an appropriate drying time, so that the moisture on the surface of the graphite piece evaporates, but will not affect the thermal stress of the graphite piece, thus preparing for subsequent purification treatment.

[0058] In the above steps (1-2), during the purification process, it is necessary to control parameters such as vacuum degree, gas flow rate and temperature so that impurities can be volatilized or reacted to be removed to ensure that the graphite parts reach the required purity and performance.

[0059] The graphite piece in the above step (2) is vacuum dip-coated or spray-coated with phenolic resin or modified phenolic resin, and slowly heated and carbonized to obtain a graphite growth ring 5 and a guide tube 6 with a pyrolytic carbon coating or a glassy carbon coating on the surface. These pyrolytic carbon coatings or glassy carbon coatings can effectively isolate Si x C y Gas, reducing its erosion and damage to graphite parts, thereby maintaining a good carbon-silicon atmosphere balance ratio, which is conducive to crystal growth.

[0060] In the above step (3), the powder filter 71, the guide tube 6, the graphite growth ring 5, the graphite support 72 and the seed chip 73 are reasonably arranged to form multiple barriers, reduce the possibility of impurities and carbon particles entering the growth area, improve the purity and quality of the crystal, ensure the uniform distribution and stability of the airflow during the growth process, and prevent the adverse effects of airflow disturbance on crystal growth. The above powder filter 71 can effectively filter out impurities and large particles in the silicon carbide powder 9, ensure that the powder entering the growth area is purer, and is conducive to the high-quality growth of the crystal.

[0061] The vacuuming in the above step (4) can remove the air and impurities inside the growth container 7, ensuring the formation of a stable carbon-silicon atmosphere at high temperature; replacing the high-purity argon gas twice in the middle can further remove the residual gas and impurities, ensuring the purity of the final growth environment; slowly heating up can help to heat evenly and avoid structural damage caused by thermal stress; slowly reducing the pressure to the growth pressure of the single crystal can help to form a high-quality low-stress silicon carbide single crystal and avoid the formation of bubbles and defects.

[0062] In step (1-5), after the residual glue on the surface of the graphite part is drained away for 2 to 5 hours, argon gas at 150°C to 250°C is continuously circulated into the inner cavity of the diffusion coating and curing device for 50 to 100 hours of heating and ventilation to cure the remaining carbon glue on the surface of the graphite part.

[0063] In step (1-7), after the residual glue on the surface of the graphite part is drained away for 2 to 5 hours, argon gas at 150°C to 250°C is continuously circulated into the inner cavity of the diffusion coating and curing device for 50 to 100 hours of heating and ventilation to solidify the remaining carbon glue on the surface of the graphite part.

[0064] The coating curing device in step (1-3) comprises a vacuum glue storage chamber 1, a glue draining basket 2, a hair dryer 3 and a gas heater 4. The top of the vacuum glue storage chamber 1 is provided with a glue injection port 11 and a pressure relief port 12, the bottom of the vacuum glue storage chamber 1 is provided with a glue leakage port 13 and an air inlet 14, and the side wall of the vacuum glue storage chamber 1 is provided with a vacuum port 15 and an air outlet 16. The glue injection port 11, the pressure relief port 12, the glue leakage port 13, the air inlet 14, the vacuum port 15, and the air outlet 16 are all connected to the inner cavity of the vacuum glue storage chamber 1, and the glue injection port 11, the pressure relief port 12, the glue leakage port 13, the air inlet 14, the vacuum port 15, and the air outlet 16 are all provided with a first switch valve 17; the hair dryer 3 and the gas heater 4 are both arranged on the outside of the vacuum glue storage chamber 1 and are sequentially connected between the air outlet 16 and the air inlet 14; the gas heater 4 is provided with a first air inlet 41, and the first air inlet 41 A second switch valve 42 is provided; the glue draining basket 2 is installed in the lower part of the inner cavity of the vacuum glue storage chamber 1, and a plurality of glue draining holes 21 are provided on the bottom and side walls of the glue draining basket 2; first open the vacuum glue storage chamber 1, put the graphite part on the glue draining basket 2 and close the vacuum glue storage chamber 1; then, open the first switch valve 17, and use an external vacuum pump to evacuate the inner cavity of the entire vacuum glue storage chamber 1 through the vacuum port 15 to exhaust the gas inside the graphite part. When the vacuum degree is ≤5pa, inject phenolic resin or modified phenolic resin glue from the glue injection port 11, and inject solvent from the glue injection port 11 at the same time; then, use an external glue liquid supply device to inject glue liquid into the inner cavity of the vacuum glue storage chamber 1 through the glue injection port 11. When the graphite part is infiltrated with glue, the residual glue on the surface of the graphite part will drain out, and the drained residual glue will pass through the plurality of glue draining holes 21 on the glue draining basket 2 and gather at the bottom of the vacuum glue storage chamber 1.

[0065] The solvent is propylene glycol methyl ether acetate. The above propylene glycol methyl ether acetate is a high-grade industrial solvent with excellent performance, which has a strong solubility for both polar and non-polar substances and is suitable for solvents of various polymers in high-grade coatings and inks.

[0066] In step (1-4), after the surface and interior of the graphite part are completely infiltrated in the phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours, the pressure relief port 12 at the top of the vacuum glue storage chamber 1 is slowly opened, and argon gas is filled into the inner cavity of the vacuum glue storage chamber 1 to 1 standard atmospheric pressure. Then, the glue leakage port 13 at the bottom of the vacuum glue storage chamber 1 is opened to allow the leaked residual glue to be discharged from the glue leakage port 13.

[0067] In step (1-5), after the residual glue is exhausted, the air inlet 14 at the bottom of the vacuum glue storage chamber 1 and the first air inlet 41 of the gas heater 4 are opened, and argon gas is introduced from the first air inlet 41 of the gas heater 4. The argon gas is heated to 150°C-250°C by the gas heater 4, and then the heated argon gas is transported to the vacuum glue storage chamber 1 through the air inlet 14 by the hair dryer 3 to perform a primary curing treatment on the carbon glue on the graphite part.

[0068] In step (1-7), after the residual glue on the surface of the graphite part is drained away for 2 hours to 5 hours, the first air inlet 41 of the gas heater 4 is closed, and the air inlet 14 and the air outlet 16 at the bottom of the vacuum glue storage chamber 1 are opened respectively, so that the air outlet 16, the heater, the hair dryer 3, the air inlet 14 and the inner cavity of the vacuum glue storage chamber 1 are connected in sequence, and the argon gas coming out of the air outlet 16 is heated to 150°C-250°C by the gas heater 4, and then the heated argon gas is continuously circulated and transported to the vacuum glue storage chamber 1 through the air inlet 14 by the hair dryer 3, so as to perform a secondary curing treatment on the graphite part.

[0069] In addition, it should be noted that the names of the various parts of the specific embodiments described in this specification may be different, and any equivalent or simple changes made based on the structure, features and principles described in the patent concept of the present invention are included in the protection scope of the patent of the present invention. The technicians in the technical field of the present invention can make various modifications or supplements to the specific embodiments described or replace them in a similar manner, as long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A low stress graphite growth ring, a guide tube and a silicon carbide single crystal growth method, characterized in that The steps include: (1) Pre-treatment of the two graphite parts, graphite growth ring and guide tube: (1-1) sandblasting the inner surface of the graphite growth ring; (1-2) Graphite parts purification: After degreasing the graphite parts, ultrasonic cleaning and low-temperature drying, the graphite parts are placed in a high-temperature furnace, inert gas is introduced under vacuum, and carbonization treatment is performed under high-temperature conditions; In the step (1-2), the graphite piece is placed in a high temperature furnace, argon gas is introduced under a vacuum environment, and carbonization treatment is performed at a high temperature of 2500° C. to 2800° C. for 60 min to 120 min; (1-3) Vacuum spraying or dipping: Place the purified graphite parts into the inner cavity of the infiltration curing device, evacuate the inner cavity of the infiltration curing device, and when the vacuum degree is ≤5 Pa, spray the graphite parts with phenolic resin glue or modified phenolic resin glue; or dip the graphite parts with phenolic resin glue or modified phenolic resin glue; The coating and curing device includes a vacuum glue storage chamber, a glue draining basket, a hair dryer and a gas heater. A glue injection port and a pressure relief port are provided on the top of the vacuum glue storage chamber, a glue leakage port and an air inlet are provided on the bottom of the vacuum glue storage chamber, and a vacuum port and an air outlet are provided on the side wall of the vacuum glue storage chamber. The glue injection port, the pressure relief port, the glue leakage port, the air inlet, the vacuum port and the air outlet are all connected with the inner cavity of the vacuum glue storage chamber, and the glue injection port, the pressure relief port, the glue leakage port, the air inlet, the vacuum port and the air outlet are all provided with a first switch valve; the hair dryer and the gas heater are both arranged on the outside of the vacuum glue storage chamber and are sequentially connected between the air outlet and the air inlet; the gas heater is provided with a first air inlet, and the first air inlet is provided with a second switch valve; the glue draining basket is installed in the vacuum glue storage chamber The bottom and side walls of the glue draining basket are provided with a plurality of glue draining holes at the lower part of the inner cavity; firstly, the vacuum glue storage chamber is opened, the graphite piece is placed on the glue draining basket and the vacuum glue storage chamber is closed; then, the first switch valve is opened, and an external vacuum pump is used to evacuate the inner cavity of the entire vacuum glue storage chamber through the vacuum extraction port to exhaust the gas inside the graphite piece, and when the vacuum degree is ≤5pa, phenolic resin or modified phenolic resin glue is injected from the glue injection port, and the solvent is injected from the glue injection port at the same time; then, an external glue liquid supply device is used to inject glue liquid into the inner cavity of the vacuum glue storage chamber through the glue injection port, and when the graphite piece is completely infiltrated with glue, the residual glue on the surface of the graphite piece will be drained out, and the drained residual glue is collected at the bottom of the vacuum glue storage chamber through the plurality of glue draining holes on the glue draining basket; (1-4) One-time vacuum infiltration: completely infiltrate the surface and interior of the graphite part into phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours to obtain carbon glue; (1-5) Primary low-temperature curing: After filling the inner cavity of the coating curing device with argon gas to 1 standard atmospheric pressure, open the lower glue leakage port of the coating curing device to release the carbon glue; after the residual glue on the surface of the graphite part is drained away, continuously circulate argon gas into the inner cavity of the coating curing device, and then heat and ventilate it to solidify the remaining carbon glue on the surface of the graphite part; (1-6) Secondary coating: The surface and interior of the graphite part are completely infiltrated in phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours to obtain carbon glue; (1-7) Secondary low-temperature curing: After filling the inner cavity of the coating curing device with argon gas to 1 standard atmospheric pressure, open the lower liquid discharge port of the coating curing device to release the carbon glue; after the residual glue on the surface of the graphite part is drained away, continuously circulate argon gas into the inner cavity of the coating curing device, and then heat and ventilate it to solidify the remaining carbon glue on the surface of the graphite part; (2) High-temperature carbonization treatment: Place the graphite parts after the secondary low-temperature curing treatment into a vacuum pressure furnace, evacuate the inner cavity of the vacuum pressure furnace to below 5 Pa, fill it with 1.5Mpa-2.0Mpa high-purity argon gas, raise the temperature to 2200-2500°C at a rate of 0.05°C / m-0.5°C / m, and maintain the temperature for 8 hours-12 hours to complete the high-temperature carbonization, so as to obtain a graphite growth ring and a guide tube with a pyrolytic carbon coating or a glassy carbon coating on the surface, and take the graphite growth ring and the guide tube out of the inner cavity of the infiltration curing device for standby use; (3) High-purity silicon carbide powder is loaded into the inner cavity of the growth container; the growth container is provided with a powder filter, a graphite holder and a seed wafer, the powder filter is horizontally installed in the inner cavity of the growth container, the guide tube, the graphite growth ring and the graphite holder are arranged in sequence from bottom to top above the powder filter and in the inner cavity of the growth container, and the seed wafer is bonded to the graphite holder; the entire growth container is loaded into the growth furnace; (4) The inner cavity of the growth container is evacuated and replaced with high-purity argon twice; when the vacuum degree of the inner cavity of the growth container reaches 5×10 -4 pa or above, start to slowly heat up; when the inner cavity temperature of the growth container reaches 800℃-1000℃, continue to fill with 800mbar-900mbar argon, slowly increase the growth temperature to above 2300℃, and slowly reduce the pressure to the growth pressure of the single crystal 1mbar-5mbar, so that the high-purity silicon carbide powder passes through the powder filter, guide tube, graphite growth ring, and graphite support from bottom to top in sequence, and then grows into a low-stress silicon carbide single crystal on the seed wafer.

2. The low stress graphite growth ring, guide tube and silicon carbide single crystal growth method according to claim 1, characterized in that: In the step (1-1), the inner surface of the graphite growth ring is sandblasted using 10-200 mesh diamond sand and 1atm-5atm compressed air.

3. The low stress graphite growth ring, guide tube and silicon carbide single crystal growth method according to claim 2, characterized in that: The surface sandblasting treatment in the step (1-1) is as follows: the inner surface of the graphite growth ring is uniformly sandblasted using 60-80 mesh diamond sand and 2atm-3atm compressed air.

4. The low stress graphite growth ring, guide tube and silicon carbide single crystal growth method according to claim 1, characterized in that: In the step (1-5), after the residual glue on the surface of the graphite piece is drained away for 2 to 5 hours, argon gas at 150° C. to 250° C. is continuously circulated into the inner cavity of the diffusion coating and curing device for 50 to 100 hours of heating and ventilation to solidify the remaining carbon glue on the surface of the graphite piece; In the step (1-7), after the residual glue on the surface of the graphite piece is drained away for 2 to 5 hours, argon gas at 150° C. to 250° C. is continuously circulated into the inner cavity of the diffusion coating and curing device, and heating and ventilation are performed for 50 to 100 hours to solidify the remaining carbon glue on the surface of the graphite piece.

5. The low stress graphite growth ring, guide tube and silicon carbide single crystal growth method according to claim 1, characterized in that: The solvent is one of acetone, ethanol, furfuryl alcohol or propylene glycol methyl ether acetate.

6. The low stress graphite growth ring, guide tube and silicon carbide single crystal growth method according to claim 1, characterized in that: In the steps (1-4), after the surface and interior of the graphite part are completely infiltrated in the phenolic resin glue or modified phenolic resin glue for 0.5 hour to 2 hours, the pressure relief port at the top of the vacuum glue storage chamber is slowly opened, and argon gas is filled into the inner cavity of the vacuum glue storage chamber to 1 standard atmospheric pressure. Then, the glue leakage port at the bottom of the vacuum glue storage chamber is opened to discharge the leaked residual glue from the glue leakage port.

7. The low stress graphite growth ring, guide tube and silicon carbide single crystal growth method according to claim 6, characterized in that: In the steps (1-5), after the residual glue is exhausted, the air inlet at the bottom of the vacuum glue storage chamber and the first air inlet of the gas heater are opened, argon gas is introduced from the first air inlet of the gas heater, the argon gas is heated to 150°C-250°C by the gas heater, and then the heated argon gas is transported to the vacuum glue storage chamber through the air inlet by a hair dryer to perform a primary curing treatment on the carbon glue on the graphite part.

8. The low stress graphite growth ring, guide tube and silicon carbide single crystal growth method according to claim 7, characterized in that: In the steps (1-7), after the residual glue on the surface of the graphite part has been drained away for 2 hours to 5 hours, the first air inlet of the gas heater is closed, and the air inlet and the air outlet at the bottom of the vacuum glue storage chamber are opened respectively, so that the air outlet, the heater, the hair dryer, the air inlet and the inner cavity of the vacuum glue storage chamber are connected in sequence, and the argon gas coming out of the air outlet is heated to 150°C-250°C by the gas heater, and then the heated argon gas is continuously circulated and transported to the vacuum glue storage chamber through the air inlet by the hair dryer, so as to perform a secondary curing treatment on the graphite part.