High fatigue resistance high speed wheel steel, wheel and wheel manufacturing method

By optimizing the steelmaking and heat treatment process of high-speed wheel steel and controlling the element composition and organizational structure, the fatigue problem caused by high stress in high-speed wheels during high-speed operation is solved, the fatigue resistance and wear resistance of the wheel are improved, and the wear resistance is extended. service life and reduces the frequency of maintenance.

CN118531320BActive Publication Date: 2024-10-18MAANSHAN MAGANG JINXI RAIL TRANSPORT EQUIP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411016636.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-18
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

When high-speed railway wheels run at high speeds, the rolling contact stress between the wheels and rails is large, resulting in tread peeling and fine cracks, which reduces the service life of the wheels and increases the overall cost. The comprehensive performance of existing carbon steel wheels is close to the limit, and it is difficult to Further improvements are achieved through heat treatment processes.

Method used

High-fatigue high-speed wheel steel is used. Through steelmaking process control and rolling, combined with appropriate heat treatment processes, the elemental composition and organizational structure of the steel are controlled to improve the comprehensive performance of the wheel, including C, Si, Mn, Cr, V, The content and combination of elements such as Al, P, and S form optimized bainite and pearlite structures, increasing the stability and fracture toughness of supercooled austenite.

Benefits of technology

It achieves high fatigue resistance of the wheel, extends the service life, reduces the frequency of maintenance, improves the anti-rolling contact fatigue performance and wear resistance, reduces the resistance to peeling and falling off, and improves the service stability of the wheel throughout its life cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118531320B_ABST
    Figure CN118531320B_ABST
Patent Text Reader

Abstract

The present invention provides a high fatigue resistance high speed wheel steel, a wheel and a wheel manufacturing method, the components include C, Si, Mn, Cr, V and Al, P is controlled to be ≤0.008%, S: 0.001-0.009%, TO: ≤10ppm, [H]: ≤1.5ppm, [N]: 30-80ppm. The components meet: P1=300-260×C-45×Mn-12×Si-25.2×Cr-20×V≥108; 1.7≤P2=(5.04×Al / 3+2.76×V) / (15×[N])≤3.8, and the ultimate Brinell hardness Y value=4.5×[98×C+12×(Si+Mn / 3+1.2×Cr+V)]≥285. The present invention improves the comprehensive performance of the wheel by optimizing the design of wheel components and matching appropriate heat treatment processes, thereby improving the service performance of the wheel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of railway wheel preparation, and specifically relates to a high fatigue resistance high-speed wheel steel and a production method thereof, a wheel and a wheel manufacturing method, which are used for the production of high fatigue resistance ≥250 km grade wheels. Background Art

[0002] High-speed railway lines are long, trains run at high speeds for a long time, the temperature difference between the north and the south is large, and the service conditions between the east and the west vary greatly. High-speed wheels show obvious inadaptability in service, especially for high-speed trains with speeds ≥ 250 kilometers per hour. There are many damage problems such as wheel tread peeling and multiple changes. This greatly increases the frequency of wheel inspections, reduces the service life of the wheels, and increases the overall cost.

[0003] When the wheel is running at high speed, the rolling contact stress between the wheel and rail is large and changes alternately, causing plastic deformation of the subsurface of the wheel rim tread during operation. Also, due to the presence of brittle phases such as inclusions and cementite in the steel, it is easy for micro cracks to initiate on the rim. These micro cracks will cause peeling and other damage under the action of rolling contact fatigue during wheel operation.

[0004] Judging from the probability of polygons occurring in high-speed wheels and the statistical results of wheel hardness, increasing hardness can reduce the occurrence of polygons. It can be seen that increasing the hardness level can improve the service performance of the wheel. In addition, from the perspective of the relationship between wheel-rail hardness matching, the wheel hardness cannot be higher than the rail hardness. Of course, under normal circumstances, after the hardness is increased, the yield strength and tensile strength of the material are also increased accordingly, which can reduce the effect of plastic deformation of the surface layer of the wheel under the wheel-rail contact stress, thereby reducing the source of microcracks. However, the increase in strength and hardness is bound to lead to a decrease in toughness indicators, affecting the risk of vehicle operation.

[0005] After decades of research, the comprehensive performance of carbon steel wheels has basically reached its limit, and it is difficult to further improve it through optimization of heat treatment process. Adding other elements and alloying have become the most direct and effective methods to improve wheel performance.

[0006] The patent with publication number CN103741047A published on April 23, 2014 discloses medium carbon steel wheel steel for railway locomotives with improved fracture toughness and a wheel preparation method. Its composition is: C0.46-0.53%, Si0.20-0.37%, Mn0.70-0.85%, Ni0.10-0.25%, Cr0.24-0.32%, Als0.020-0.040%, P≤0.008%, S≤0.008%, and the rest are Fe and unavoidable impurity elements. The composition design idea of ​​this patent is to improve the hardness and toughness of the material by adding Cr (0.24-0.32%) and Ni (0.10-0.25%), which is relatively costly. Summary of the invention

[0007] The purpose of the present invention is to provide a high fatigue resistance high-speed wheel steel and a production method thereof, by controlling the steelmaking process and rolling, controlling the inclusions in the steel, improving the performance of the steel, and using it for the production of high fatigue resistance ≥ 250 km grade wheels to improve the comprehensive performance of the wheels.

[0008] Another object of the present invention is to provide a wheel and a wheel manufacturing method, using the above-mentioned high fatigue resistance and high-speed wheel steel to produce the wheel, matching the appropriate heat treatment process, to improve the comprehensive performance of the wheel, thereby improving the service performance of the wheel.

[0009] The specific technical solutions of the present invention are as follows:

[0010] A high fatigue resistance high speed wheel steel, comprising the following components in percentage by mass:

[0011] C: 0.52-0.60%, Si: 0.25-0.40%, Mn: 0.65-0.80%, Cr: 0.12-0.30%, V: 0.00-0.15%, Al: 0.010-0.030%, P≤0.008%, S: 0.001-0.009%, TO: ≤10ppm, [H]: ≤1.5ppm, [N]: 30-80ppm, the rest are Fe and unavoidable impurity elements.

[0012] The composition of the high fatigue resistance high speed wheel steel also meets the following requirements:

[0013] P1=300-260×C-45×Mn-12×Si-25.2×Cr-20×V, P1≥108;

[0014] The combination of Mn, Si, Cr, V and C slows down the diffusion of C, slows down the transformation of bainite, increases the incubation period, and increases the depth of bainite under the tread. The present invention controls P1≥108, the bainite structure obtained on the wheel tread is ≤6mm, and the spacing between the pearlite lamellae is small, which has good plasticity and toughness.

[0015] P2=(5.04×Al / 3+2.76×V) / (15×[N]), 1.7≤ P2≤3.8; by adjusting the content of elements such as Cr and V, the stability of supercooled austenite is improved, the supercooling degree in the cooling phase transformation stage is increased, and a relatively fine pearlite plate spacing is obtained. With the goal of pinning the grain boundaries with AlN particles, the contents of V, Al, N, etc. are strictly controlled to promote the effective combination of Als and N to form AlN and VN second phases. Due to its good thermal stability, it has a significant effect of pinning the grain boundaries, and can effectively hinder the growth and coarsening of austenite grains during hot working, thereby obtaining high hardness while also having good fracture toughness.

[0016] The ultimate Brinell hardness Y value of the present invention is ≥285, Y=4.5×[98×C+12×(Si+Mn / 3+1.2×Cr+V)]. In order to make the wheel obtain high strength and high toughness under appropriate heat treatment process and meet the service conditions of high resistance to heat damage, according to the role of alloy elements in steel, Y is an index evaluated by weighting and adding the influence of each element on the Brinell hardness of quenched and tempered steel.

[0017] When calculating in the above formula, each element is expressed as its mass percentage content × 100.

[0018] When the C content is between 0.52≤C content≤0.56%, the preferred other components are Si: 0.30-0.35%, Mn: 0.70-0.80%, Cr: 0.18-0.30%, V: 0.08-0.15%, Al: 0.020-0.025%, S: 0.001-0.005%; [N]: 60-80ppm.

[0019] When the C content is between 0.56<C content≤0.60, the preferred other components are Si: 0.25-0.30%, Mn: 0.65-0.70%, Cr: 0.12-0.18%, V: 0.00-0.08%, Al: 0.010-0.020%, S: 0.005-0.009%; [N]: 30-60ppm.

[0020] A production method for high fatigue resistance high speed wheel steel comprises the following process flow: electric arc furnace smelting - LF refining - RH vacuum treatment - continuous casting - heating - rolling - slow cooling.

[0021] The electric arc furnace smelting: in the electric furnace blowing process, oxygen, nitrogen and argon mixed gas are blown by an oxygen lance from the late melting period, and slag-making materials are added in time to reduce the decarburization reaction rate in the dephosphorization process under the condition of effectively ensuring the thermodynamics and kinetics of dephosphorization, so that the carbon content in the electric furnace terminal steel is higher, the phosphorus content of slag-free steel is P≤0.06%, and the steel tapping temperature is ≥1600°C;

[0022] The LF refining adopts a successive deoxidation mechanism, and carbon powder, silicon-containing alloys and materials are used for primary deoxidation during steel tapping and refining. The active oxygen in the molten steel can be controlled to 20-30ppm at the end of refining. The RH process uses the vacuum carbon deoxidation principle to further reduce the active oxygen in the steel. The active oxygen in the steel can be controlled to about 10ppm before adding aluminum for final deoxidation in the late RH period. Aluminum is added for final deoxidation before the RH end point, and the deoxidation TO is less than or equal to 6ppm. The tapping temperature is 1640-1660°C.

[0023] The RH vacuum treatment: RH vacuum cycle degassing to set H≤1.0ppm, precise control of N: 30-80ppm;

[0024] The continuous casting: The continuous casting process design appropriately increases the superheat of the molten steel in the tundish, the primary cooling rate of the strong cooling process of the billet: the molten steel temperature in the tundish is 1500-1530°C, the primary cooling rate of the strong cooling process is 4000-4500l / min, the secondary cooling water volume is 0.18-0.20 L / kg, and the casting speed is 0.25-0.35m / min, so that the rim corresponds to the billet and forms dense columnar crystals, improves the density of the organization, and promotes the fine MnS precipitated at the solidification end of the secondary dendrite to be distributed in a uniform and dispersed form, thereby improving the uniformity and dispersion of the MnS inclusions in the billet and reducing the size of the MnS inclusions. The billet entry slow cooling temperature is ≥500°C, and the slow cooling time is ≥24h; the billet exit slow cooling temperature is ≥160°C.

[0025] For the heating, the steel billet is preheated at 700-1100°C for 1-1.5 hours and then heated to 1310-1330°C with the furnace. The heating period is 1-1.5 hours. The steel billet then enters the soaking section of the heating furnace. The temperature control range of the soaking section is 1240-1250°C and the heating time is 0.5-1.0 hour. The steel billet is kept warm at this temperature. The total time for preheating, heating and soaking is controlled not to exceed 4 hours.

[0026] The rolling process has a starting temperature of 1155-1170° C. and a final rolling temperature of ≥870° C., in order to avoid decomposition and phase transformation of austenite during rolling.

[0027] The slow cooling comprises slow cooling in a pit at a temperature not lower than 500° C. after rolling, and the slow cooling time is ≥6h.

[0028] The high fatigue resistance high speed wheel steel has aluminum oxide inclusions of ≤2 μm, total oxygen stability in the steel of ≤6 ppm, a casting structure of uniformly grown columnar crystal structure, and an austenite grain size of the steel of 11.0 or above.

[0029] A wheel manufacturing method uses the above-mentioned high fatigue resistance high-speed wheel steel to manufacture the wheel, including heat treatment, wherein the heat treatment method is: heating and heat preservation, quenching, and tempering.

[0030] The heating and heat preservation means that the wheel is first heated to 860-900°C in the heating section of the heat treatment furnace and heated to 840-870°C in the soaking section. The total heating time is 2.0-3.0h, of which the soaking section time is 0.5-1.0h.

[0031] Heating according to the above method ensures uniform austenitization of the internal structure of the wheel, eliminates the uneven structure of rolling, and partially dissolves and homogenizes V, Cr, etc. The shorter insulation time of 0.5-1.0 is to inhibit the coarsening of austenite grains and precipitated MX (M: C, N) particles.

[0032] In the quenching, the tread strong spray nozzle starts to spray the wheel tread, the rim cooling rate is 3-5℃ / s, the metal inside the rim quickly passes through the Ar3~Ar1 temperature range, inhibiting the precipitation of proeutectoid ferrite and preventing the internal structure from transforming to bainite. Cooling to the temperature of the transition area between the rim and the web is below 600℃.

[0033] The tempering is performed at 480-520° C. for a period of ≥3.0 hours.

[0034] A wheel is manufactured by adopting the above manufacturing method.

[0035] The wheel fracture toughness is ≥90MPa.m 1 / 2 , -60℃ impact KV≥5J, -40℃ impact KV≥12J, -20℃ impact KV≥18J, rim tensile strength 900-980MPa, yield strength ≥700MPa, rim wear limit Brinell hardness ≥285HBW (5 / 750), high contact fatigue resistance and wear performance, and good matching of strength, hardness and toughness, the organization is ferrite and pearlite, the pearlite sheet spacing is 0.09-0.12μm; the grain size is finer than 10 levels, thus obtaining better comprehensive mechanical properties, and at the same time, the wheel has good wear resistance and contact fatigue resistance. Wheel rim sampling threshold value △Kth≥9.1 MPa.m 1 / 2 .

[0036] The circumferential residual stress compression value on the wheel running surface is controlled at (-150MPa) - (-80MPa), and the compressive stress value of the rim in the area between the wheel wear limit and 15 mm below the wear limit (35mm-50mm below the tread) is zero. At the same time, it has excellent resistance to rolling contact fatigue and wear resistance, thereby reducing peeling and falling off, and further improving the service stability of the wheel throughout its life cycle.

[0037] The design ideas of the present invention are as follows:

[0038] C: C is necessary for steel to obtain high strength and hardness. The C content in traditional wheel steel is relatively high.

[0039] Although high C content is beneficial to the strength and hardness of steel, it is extremely detrimental to the plasticity and toughness of steel, and reduces the yield strength ratio, increases the decarburization sensitivity, and deteriorates the fatigue resistance and processing performance of steel. Therefore, the C content in steel is appropriately reduced to improve the plasticity and toughness of steel, but too low C content will affect the strength of steel. Combined with the addition of other elements, it is controlled at 0.52-0.60%.

[0040] Si: Si is the main deoxidizing element in steel, has a strong solid solution strengthening effect, and can also improve the hardenability of wheel steel. However, too high Si content will reduce the plasticity and toughness of steel, increase the activity of C, promote the decarburization and graphitization tendency of steel during rolling and heat treatment, make smelting difficult and easy to form inclusions, and deteriorate the fatigue resistance of steel. Therefore, the Si content is controlled to 0.25-0.40%.

[0041] Mn: Mn is an element that improves the quenching characteristics without inhibiting low temperature toughness. In addition, Mn can act synergistically with Si, and part of the dissolved oxygen captured by Mn and Si can be distributed among elements other than Al, thereby limiting the risk of forming large clusters of alumina inclusions. However, when added in an amount greater than 0.80%, the center segregation that occurs not only reduces the low temperature toughness but also improves the hardenability of the steel. Since Mn center segregation is a factor that causes hydrogen cracking, it is preferred to limit the content to 0.65% to 0.80%.

[0042] S: Sulfur easily forms MnS inclusions with manganese in steel, making the steel hot brittle. However, adding a small amount of S will significantly improve the cutting performance of wheel steel without affecting product performance, and MnS also has the effect of refining grains. The uniform and dispersed precipitation of MnS during the solidification process requires appropriate [S] in the steel. The standards of wheel customers have strict requirements on the rating of MnS inclusions. Therefore, the needs of both aspects should be comprehensively considered in the process design. Through comparison and analysis of previous data, the optimal value of [S] in molten steel for the inclusion plasticization process is determined to be controlled at 0.001-0.009%.

[0043] P is an element with a strong tendency to segregate, which increases the cold brittleness of steel, reduces plasticity, and is harmful to the uniformity of product structure and performance. P is controlled to be ≤ 0.008%. However, if you want to reduce the P content too much, the refining cost will increase excessively. Therefore, considering the usual industrial production, the preferred lower limit of the P content is 0.005%.

[0044] Cr: Cr can improve the hardenability and strength of steel. Cr can also reduce the activity of C, reduce the decarburization tendency of the steel surface during heating, rolling and heat treatment, and can be used to obtain high fatigue resistance. At the same time, as the Cr content increases, the average transformation temperature of pearlite decreases, the CCT curve moves to the lower right, the spacing between pearlite lamellae becomes smaller, and the hardness increases. In addition, Cr and V can be combined to obtain an extremely fine dispersed phase, which improves the wear resistance of the wheel. Therefore, the Cr content cannot be lower than 0.10%. However, too high Cr will reduce the toughness of the steel and increase the depth of abnormal organization of the wheel tread. For economic considerations, the Cr content should not be higher than 0.14%. The Cr content is controlled at 0.10-0.14%.

[0045] Al: Al is an effective deoxidizer and can form AlN to refine grains. When the Al content is lower than 0.016%, the effect is not obvious. When it is higher than 0.030%, it is easy to form coarse inclusions, which deteriorates the impact properties of steel. Therefore, the Al content should be controlled at 0.016-0.030%.

[0046] V: Vanadium is an important strong carbonitride forming element in wheel steel. Through heating dissolution and cooling precipitation, interstitial VC, V4C3 and nitrogen-rich V (C, N) second phase particles can be formed in the steel, resulting in strong precipitation strengthening and fine grain strengthening, which plays a role in significantly improving the yield strength. In addition, the formation of vanadium-containing second phase particles, the micro-region around the particles, due to the carbon deficiency and the small lattice mismatch with ferrite, promotes the formation of proeutectoid ferrite, which plays a role in moderately increasing the wear rate, thereby achieving the purpose of coordinating the competitive relationship between contact fatigue and wear and improving the surface contact fatigue resistance of the wheel. The present invention sets the vanadium content range to 0.00% to 0.06%, because, on the one hand, when the vanadium content exceeds 0.06%, a higher heating temperature must be used to produce a significant strengthening effect, otherwise, due to the dual factors of low solid solution V content and low matrix carbon content, the effect of V microalloying on improving strength will be greatly limited, and even a negative effect will be produced. At the same time, with the increase of V content, the average transformation temperature of pearlite is also reduced, the CCT curve moves to the lower right, and the pearlite lamella spacing and hardness increase. When the V content exceeds 0.06%, the effect becomes weaker.

[0047] TO and [H]: TO forms oxide inclusions in steel, so control TO≤10ppm; [H] forms white spots in steel, which seriously affects product performance, so control [H]≤1.5ppm.

[0048] When P1 is less than 108, the toughness of the pearlite structure is insufficient. In addition, during heat treatment and quenching, the bainite structure is deeper, and it is not easy to eliminate the bainite structure under the same processing allowance design.

[0049] When P2 is less than 1.7, the wheel toughness index is significantly reduced. When P2 is greater than 3.8, the wheel toughness index is reduced and the strength and hardness index will also decrease.

[0050] Compared with the prior art, the present invention achieves better comprehensive performance by controlling the steelmaking process, rolling and heat treatment processes, and realizing effective matching of microalloys, playing a strengthening role to improve strength and hardness, and playing a grain refinement role to improve strength and toughness matching. The wheel has excellent rolling contact fatigue resistance and wear resistance, thereby reducing the phenomenon of peeling and falling off, and further improving the service stability of the wheel throughout its life cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is the wheel rim structure of Example 1. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] Example 1-Example 3

[0054] A production method for high fatigue resistance high speed wheel steel comprises the following process flow: electric arc furnace smelting-LF refining-RH vacuum treatment-continuous casting-heating-rolling-slow cooling.

[0055] The electric arc furnace smelting: in the electric furnace blowing process, oxygen, nitrogen and argon mixed gas are blown by an oxygen lance from the late melting period, and slag-making materials are added in time to reduce the decarburization reaction rate in the dephosphorization process under the condition of effectively ensuring the thermodynamics and kinetics of dephosphorization, so that the carbon content in the electric furnace terminal steel is higher, the phosphorus content of slag-free steel is P≤0.06%, and the steel tapping temperature is ≥1600°C;

[0056] The LF refining adopts a successive deoxidation mechanism, and carbon powder, silicon-containing alloys and materials are used for primary deoxidation during steel tapping and refining. The active oxygen in the molten steel can be controlled to 20-30ppm at the end of refining. The RH process uses the vacuum carbon deoxidation principle to further reduce the active oxygen in the steel. The active oxygen in the steel can be controlled to about 10ppm before adding aluminum for final deoxidation in the late RH period. Aluminum is added for final deoxidation before the RH end point, and the deoxidation TO is less than or equal to 6ppm. The tapping temperature is 1640-1660°C.

[0057] The RH vacuum treatment: RH vacuum cycle degassing to set H≤1.0ppm, precise control of N: 30-80ppm;

[0058] The continuous casting: the continuous casting process design appropriately increases the superheat of the molten steel in the tundish, the primary cooling rate of the strong cooling process of the billet: the molten steel temperature in the tundish is 1500-1530°C, the primary cooling rate of the strong cooling process is 4000-4500l / min, the secondary cooling water volume is 0.18-0.20 L / kg, the pouring and pulling speed is 0.25-0.35m / min, and the rim corresponds to the billet to form dense columnar crystals, improve the density of the organization, promote the fine MnS precipitated at the solidification end of the secondary dendrite to be distributed in a uniform and dispersed form, improve the uniformity and dispersion of the MnS inclusions in the billet, and reduce the size of the MnS inclusions. The billet entry slow cooling temperature is ≥500°C, the slow cooling time is ≥24h; the billet exit slow cooling temperature is ≥160°C.

[0059] For the heating, the steel billet is preheated at 700-1100°C for 1-1.5 hours and then heated to 1310-1330°C with the furnace. The heating period is 1-1.5 hours. The steel billet then enters the soaking section of the heating furnace. The temperature control range of the soaking section is 1240-1250°C and the heating time is 0.5-1.0 hour. The steel billet is kept warm at this temperature. The total time for preheating, heating and soaking is controlled not to exceed 4 hours.

[0060] The rolling process has a starting temperature of 1155-1170° C. and a final rolling temperature of ≥870° C., in order to avoid decomposition and phase transformation of austenite during rolling.

[0061] The slow cooling comprises slow cooling in a pit at a temperature not lower than 500° C. after rolling, and the slow cooling time is ≥6h.

[0062] Comparative Example 1-Comparative Example 5

[0063] A method for producing high fatigue resistance high speed wheel steel is carried out in the same manner as in the embodiment except for different parameters and components.

[0064] The specific parameters of each embodiment and comparative example are shown in Table 1 and Table 3.

[0065] .

[0066] The specific composition of the steels smelted in the embodiments and comparative examples is shown in Table 2. The remainder not shown in Table 2 is Fe and unavoidable impurities.

[0067] .

[0068] The wheel rolling processes of the embodiments of the present invention and the comparative examples are shown in Table 3.

[0069] .

[0070] The wheel steels of the above-mentioned embodiments and comparative examples are used to manufacture wheels, including heat treatment, wherein the heat treatment method is: heating and heat preservation, quenching, and tempering.

[0071] The heating and heat preservation means that the wheel is first heated to 860-900°C in the heating section of the heat treatment furnace and heated to 840-870°C in the soaking section. The total heating time is 2.0-3.0h, of which the soaking section time is 0.5-1.0h.

[0072] In the quenching, the tread strong spray nozzle starts to spray the wheel tread, the rim cooling rate is 3-5℃ / s, the metal inside the rim quickly passes through the Ar3~Ar1 temperature range, the precipitation of proeutectoid ferrite is suppressed, and the internal structure is prevented from transforming to bainite, and the temperature of the transition area between the rim and the web is cooled to below 600℃.

[0073] The tempering is performed at 480-520° C. for a period of ≥3.0 hours.

[0074] The heat treatment parameters of each embodiment and comparative example are shown in Table 4.

[0075] .

[0076] The properties of the steels produced in the above embodiments and comparative examples are shown in Table 5.

[0077] .

[0078] Continued from the above table.

[0079] .

[0080] Cyclic plasticity experiments on ratcheting behavior of wheel materials.

[0081] A rod-shaped specimen was sampled 15 mm below the tread, and an axial cyclic tension and compression fatigue test with three stress amplitudes was carried out under constant average stress. The loading waveform was a sine wave with a frequency of 0.1 Hz. The test was stopped when the specimen broke. The test stress loading condition parameters are shown in Table 6, and the test results are shown in Table 7.

[0082] .

[0083] .

[0084] The wear performance and contact fatigue performance comparison tests were carried out on the MMS-2A microcomputer controlled testing machine in accordance with GB 10622 "Metallic Material Rolling Contact Fatigue Test Method" standard, and the test results are shown in Tables 8 and 9 respectively. During the test, the main sample is the wheel sample prepared in each embodiment or comparative example of the present invention, and the auxiliary sample is the U71Mn rail sample with the same hardness, and the diameter of the main sample and the auxiliary sample is 60mm. Wear test: a group of 3 sets of samples, the main sample speed is 360rpm, the auxiliary sample speed is 400rpm, the corresponding rotation slip rate is 0.75%, the contact stress is 1100MPa, and the number of cycles is 500,000 times. Contact fatigue test: a group of 6 sets of samples, the speed is 2000rpm, the corresponding rotation slip rate is 0.3%, the contact stress is 1100-1500MPa, and 20# engine oil is used for lubrication.

[0085] .

[0086] .

[0087] The surface hardness of the sample before and after the test was measured using a MVK-21 Vickers microhardness tester (average of 8-10 points on the circumference of the contact surface), and the surface hardening rate of the wheel sample was measured.

[0088] .

[0089] Hardening rate = (surface hardness after test - surface hardness before test) / surface hardness before test × 100%

[0090] After the test, the surface structure of the wheel specimens showed obvious plastic rheology. Under the same test parameters, the wheel material has a significant effect on the thickness of the plastic deformation layer. The measured results are shown in Table 11.

[0091] .

[0092] It can be seen from Tables 7 to 11 that the wheels of Examples 1 to 3 produced according to the composition and process of the present invention have excellent rolling contact fatigue resistance and wear resistance, and improve the service stability of the wheels throughout their life cycle. However, Comparative Examples 1 to 5 were not produced according to the composition and process of the present invention, and the wheels had poor rolling contact fatigue resistance and wear resistance.

[0093] The underlined data above do not meet the requirements of the present invention.

[0094] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A high fatigue resistance high speed wheel steel, characterized in that: The high fatigue resistance high speed wheel steel comprises the following components in percentage by mass: C: 0.52-0.60%, Si: 0.25-0.40%, Mn: 0.65-0.80%, Cr: 0.12-0.30%, V: 0.00-0.15%, Al: 0.010-0.030%, P≤0.008%, S: 0.001-0.009%, TO: ≤10ppm, [H]: ≤1.5ppm, [N]: 30-80ppm, the rest are Fe and unavoidable impurity elements; The composition of the high fatigue resistance high speed wheel steel meets the following requirements: P1=300-260×C-45×Mn-12×Si-25.2×Cr-20×V, P1≥108; P2=(5.04×Al / 3+2.76×V) / (15×[N]), 1.7≤P2≤3.8; Ultimate Brinell hardness Y value≥285, Y=4.5×[98×C+12×(Si+Mn / 3+1.2×Cr+V)]; The process includes the following steps: electric arc furnace smelting - LF refining - RH vacuum treatment - continuous casting - heating - rolling - slow cooling; The electric arc furnace smelting: phosphorus content P≤0.06% for slag-free steelmaking, and steelmaking temperature≥1600°C; The LF refining: deoxidation TO≤6ppm, tapping temperature: 1640-1660°C; The RH vacuum treatment: RH vacuum cycle degassing to set H≤1.0ppm, precise control of N: 30-80ppm; The continuous casting: primary cooling speed: tundish molten steel temperature 1500-1530°C, strong cooling process primary cooling speed 4000-4500l / min, secondary cooling specific water volume: 0.18-0.20L / kg, casting speed: 0.25-0.35m / min, billet entry slow cooling temperature ≥500°C, slow cooling time ≥24h; billet exit slow cooling temperature ≥160°C; The heating is that the steel billet is preheated at 700-1100°C for 1-1.5 hours and then heated to 1310-1330°C with the furnace. The heating period is 1-1.5 hours. Then the steel billet enters the soaking section of the heating furnace. The temperature control range of the soaking section is 1240-1250°C. The heating time is 0.5-1.0 hours. The steel billet is kept warm at this temperature. The total time of preheating, heating and soaking is controlled not to exceed 4 hours. The rolling process has a starting temperature of 1155-1170°C and a final rolling temperature of ≥870°C; The slow cooling is carried out after rolling at a temperature not lower than 500°C and the slow cooling time is ≥ 6h; The high fatigue resistance high speed wheel steel has aluminum oxide inclusions of ≤2 μm, total oxygen stability in the steel of ≤6 ppm, a casting structure of uniformly grown columnar crystal structure, and an austenite grain size of the steel of 11.0 or above.

2. A method for manufacturing a wheel, characterized in that: The high fatigue resistance high speed wheel steel is manufactured using the high fatigue resistance high speed wheel steel according to claim 1, and the manufacturing method includes heating and heat preservation, quenching and tempering.

3. The manufacturing method according to claim 2, characterized in that: The heating and heat preservation means: firstly put the wheel into the heat treatment furnace, heat it at 860-900°C in the heating section, and heat it at 840-870°C in the soaking section. The total heating time is 2.0-3.0h, of which the soaking section time is 0.5-1.0h.

4. The manufacturing method according to claim 2 or 3, characterized in that: The quenching is performed by strong spraying on the tread, the nozzle sprays the wheel tread, and the cooling rate of the rim is 3-5°C / s.

5. A wheel manufactured by the manufacturing method according to any one of claims 2 to 4, characterized in that: The wheel fracture toughness is ≥90MPa.m 1 / 2 , -60℃ impact KV≥5J, -40℃ impact KV≥12J, -20℃ impact KV≥18J, rim tensile strength 900-980MPa, yield strength ≥700MPa, rim wear limit Brinell hardness ≥285HBW, wheel rim sampling threshold value △Kth≥9.1MPa.m 1 / 2 .

Citation Information

Patent Citations

  • Medium-carbon steel wheel steel having improved fracture toughness and used for railway locomotive and preparation method of wheel

    CN103741047A

  • Steel suitable for wheels of passenger locomotives in alpine regions, production method of steel, wheels and production method of wheels

    CN116623098A