A method for preparing a composite grounding wire
Through graphite additives and electromagnetic field-assisted processing technology, conductive and anti-corrosion layers are formed in stainless steel coated composite metal wires, which solves the problems of insufficient durability and corrosion resistance of traditional ground wires in extreme environments, and realizes efficient preparation of composite ground wires and excellent performance.
Patent Information
- Application Number
- CN202410993530.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Traditional grounding wires show problems of insufficient durability and performance in extreme environments such as high corrosion, high temperature, and high pressure, especially in strong acid, strong alkali environments or seaside conditions, and their electrolytic reaction with underground pipelines affects grounding. Effect.
Graphite additive, electromagnetic field-assisted processing and ultrasonic oscillation mixing technology are used to coat composite metal wires with stainless steel leather to form conductive and anti-corrosion layers, and multi-channel drawing and annealing treatment are carried out to optimize the material structure and performance.
It improves the conductivity and corrosion resistance of the composite grounding wire, reduces maintenance frequency and cost, and ensures stable operation and safety in harsh environments.
Smart Images

Figure CN118538470B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a grounding wire, in particular to a method for preparing a composite grounding wire. Background Art
[0002] Grounding wires play a vital role in electrical engineering. Their main function is to connect the metal casing or other conductive parts of electrical equipment to the ground to ensure that the charges that may be generated on the equipment can be safely guided to the ground, thereby maintaining the safety of people and equipment. Traditional grounding wires are mostly made of copper wires or copper-plated steel wires. Their working principle is based on using the conductive properties of the ground to effectively transfer the charges on the equipment to the ground to maintain the electrical potential stability of the electrical system.
[0003] With the continuous advancement of technology and the diversification of application scenarios, the performance of traditional grounding wires in certain special environments has gradually failed to meet the growing demand. For example, in extreme conditions such as highly corrosive environments, high temperatures, and high pressures, the durability and performance of traditional grounding wires may be significantly affected.
[0004] The composite grounding wires currently available on the market, such as hot-dip galvanized flat steel, copper-clad steel, zinc-clad steel, etc., are designed to provide anti-corrosion performance and good conductivity when buried underground through the characteristics of their composite materials. However, in actual applications, the anti-corrosion performance of these materials is still insufficient. Specifically, although the anti-corrosion effect of hot-dip galvanizing is widely recognized, its durability still needs to be improved; copper-clad steel has poor anti-corrosion performance in harsh environments such as strong acids and alkalis or seaside conditions; in addition, the electrolytic reaction that may occur between the grounding wire and the underground pipeline will also affect the grounding effect. As for zinc-clad steel, although it has certain anti-corrosion properties, the hardness of the material itself limits its bending ability in actual applications and affects its installation flexibility.
[0005] In view of this, the need to develop a new type of composite grounding wire is becoming increasingly urgent. This new product needs to reduce the frequency and cost of maintenance while ensuring long-term stable use. The ideal new grounding wire should have excellent corrosion resistance and conductivity to adapt to the challenges of various harsh environments. At the same time, the product should also consider the interaction with underground pipelines to avoid the adverse effects of electrolytic reactions on the grounding effect.
[0006] The research and development of new composite grounding wires is of great significance to the field of electrical engineering. It is expected to provide a more stable and reliable grounding solution, thereby improving the safety and reliability of the entire electrical system. Summary of the invention
[0007] In order to solve the above problems in the prior art, the present invention proposes a method for preparing a composite grounding wire, comprising the following steps:
[0008] Step 1: adding graphite agent to metal wire through graphite additive adding device to mix to obtain composite metal wire, sending stainless steel skin and the composite metal wire into a coating machine for processing and pressing, so that the stainless steel skin is coated on the outside of the composite metal wire to form a coating layer, and promoting the orderly arrangement of molecules of the composite metal wire after coating under the action of electromagnetic field of preset frequency and preset intensity through electromagnetic field assisted processing technology, twisting the composite metal wire after pressing and electromagnetic processing, laser welding the side seams of the coating layer, and then sending it into a polishing machine for polishing to form a composite grounding wire core;
[0009] Step 2: performing a first-stage drawing process on the composite grounding wire core;
[0010] Step 3: performing a first-stage annealing treatment on the composite grounding wire core after the first-stage drawing treatment, with the annealing temperature being 300-400° C.;
[0011] Step 4: performing a second-stage drawing process on the composite grounding wire core after the first-stage annealing process;
[0012] Step 5: performing a second-stage annealing treatment on the composite grounding wire core after the second-stage drawing treatment, with the annealing temperature being 200-250° C.;
[0013] Step 6: performing single-filament forming on the composite grounding wire core after the second-stage annealing treatment, that is, forming the composite grounding wire.
[0014] Preferably, the first-stage drawing treatment, the first-stage annealing treatment, the second-stage drawing treatment and the second-stage annealing treatment are performed in an environment of protective gas.
[0015] Preferably, the protective gas is nitrogen.
[0016] Preferably, in step 1, the graphite additive adding device comprises an adding box and a discharge conduit connected to the outlet of the adding box, and the discharge conduit is located above the running wheels of the laminating machine.
[0017] Preferably, in step 1, the graphite agent and the metal wire are mixed using ultrasonic oscillation technology.
[0018] Preferably, the steps of the ultrasonic oscillation technology include: putting the graphite agent and the metal wire into a mixing container according to a preset ratio, using an ultrasonic oscillation mixing device to generate ultrasonic oscillation waves, so that the graphite agent and the metal wire in the mixing container are subjected to uniform ultrasonic oscillation;
[0019] The ultrasonic oscillation wave has a sound wave frequency of 20 kHz to 100 kHz, an energy density of 0.1 to 2 W / cm², and an oscillation time of 5 min to 30 min.
[0020] Preferably, in step 1, a functional layer is formed outside the coating layer, and the functional layer includes a conductive layer and an anti-corrosion layer in sequence from the inside to the outside.
[0021] Preferably, in step 1, the conductive layer comprises 10%-30% by mass of metal wires; and the anti-corrosion layer comprises 5%-20% by mass of corrosion-resistant materials.
[0022] Preferably, the step of promoting the orderly arrangement of molecules under the action of an electromagnetic field of a preset frequency and a preset intensity by electromagnetic field assisted processing technology comprises the following steps:
[0023] a. Determine the electromagnetic field parameters: the preset frequency range is 100 Hz to 10 kHz, and the preset intensity range is 0.1 to 2 Tesla;
[0024] b. Design an electromagnetic field assisted processing device: The electromagnetic field assisted processing device includes an electromagnetic field generator, a coil and a control system, wherein the electromagnetic field generator is used to provide power to the coil and the control system, the coil is used to generate an electromagnetic field with adjustable frequency and intensity, and the control system is used to adjust and monitor the electromagnetic field parameters generated by the coil;
[0025] c. After the stainless steel skin and the composite metal wire are fed into the coating machine, an electromagnetic field-assisted processing device is used to cause the coated composite metal wire to be arranged in an orderly manner under the action of an electromagnetic field of a preset frequency and a preset intensity.
[0026] Preferably, the control system is used to monitor the electromagnetic field parameters in real time, and the crystallinity and conductivity performance indicators of the composite grounding wire are tested in real time, and the electromagnetic field parameters are adjusted and optimized in real time according to the crystallinity and conductivity performance indicators.
[0027] The beneficial effects of the present invention include:
[0028] By using graphite additive adding device, electromagnetic field assisted processing technology and ultrasonic oscillation mixing technology, rapid and uniform mixing of composite materials is achieved, the uniformity and stability of the composite materials are improved, making the preparation process more efficient and stable.
[0029] By controlling the proportion and layout of each layer of material and optimizing the material structure and performance, precise regulation of the performance of the composite material is achieved, thereby improving the conductivity of the composite grounding wire.
[0030] The anti-corrosion layer material is evenly covered or centrally laid out, and multiple drawing and annealing treatments are performed to further optimize the material structure and performance of the composite grounding wire, thereby improving its corrosion resistance.
[0031] After multiple drawing and annealing treatments, the finished single-filament cored product is obtained, i.e., the prepared composite grounding wire product, which ensures the smooth completion of the preparation process and the high quality of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present application, but do not constitute an improper limitation of the present invention. In the drawings:
[0033] Figure 1 The present invention is a flow chart of a method for preparing a composite grounding wire. DETAILED DESCRIPTION
[0034] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments, wherein the illustrative embodiments and descriptions are only used to explain the present invention but are not intended to limit the present invention.
[0035] Example 1
[0036] Combined with Figure 1 A method for preparing a composite grounding wire of the present invention comprises the following steps:
[0037] Step 1:
[0038] Gathering Ingredients:
[0039] In the preparation process of the present invention, the following raw materials are prepared: metal wire and a pre-prepared stainless steel skin. The metal wire includes but is not limited to copper wire, aluminum wire, and steel core wire;
[0040] Preparation of composite grounding core:
[0041] The graphite agent is added to the metal wire through a graphite additive adding device to mix and obtain a composite metal wire, the stainless steel skin and the composite metal wire are sent to a coating machine for processing and pressing, so that the stainless steel skin is coated on the outside of the composite metal wire to form a coating layer, and the electromagnetic field assisted processing technology is used to promote the orderly arrangement of molecules of the composite metal wire after coating under the action of an electromagnetic field of a preset frequency and a preset intensity, the composite metal wire after pressing and electromagnetic processing is twisted, the coating layer is laser welded at the side seam, and then sent to a polishing machine for polishing, and after polishing, it is sent to a twisting machine again for twisting, and finally a composite grounding wire core is formed;
[0042] Wherein, the graphite additive adding device comprises an adding box and a discharge conduit connected to the outlet of the adding box, and the discharge conduit is located above the running wheel of the laminating machine.
[0043] Step 2: First stage drawing process:
[0044] Performing a first-stage drawing process on the composite grounding wire core;
[0045] During the first stage of drawing, a protective gas is required to prevent oxidation, and nitrogen is used as the protective gas.
[0046] Step 3: First stage annealing treatment:
[0047] The composite grounding wire core after the first stage drawing treatment is subjected to the first stage annealing treatment, and the annealing temperature is 300-400° C.;
[0048] Step 4: Second stage drawing process:
[0049] Performing a second-stage drawing process on the composite grounding wire core after the first-stage annealing process;
[0050] During the second stage drawing process, it is also necessary to fill in a protective gas to protect the material from oxidation, and the protective gas is still nitrogen.
[0051] Step 5: Second stage annealing treatment:
[0052] The composite grounding wire core after the second stage drawing treatment is subjected to a second stage annealing treatment, and the annealing temperature is 200-250° C.;
[0053] Step 6: Finished product of monofilament core collection:
[0054] The composite grounding wire core after the second stage annealing treatment is subjected to single-filament forming to form the composite grounding wire.
[0055] Example 2
[0056] Based on the above embodiment, in step 2, when laminating the stainless steel skin and the composite metal wire in the laminating machine, the electromagnetic field assisted processing technology is introduced. By adjusting the electromagnetic field parameters, such as frequency and intensity, the order of the material molecular arrangement can be promoted, and the crystallinity and electrical conductivity of the composite material can be improved.
[0057] The step of promoting the orderly arrangement of molecules under the action of an electromagnetic field of a preset frequency and a preset intensity by electromagnetic field-assisted processing technology specifically comprises the following steps:
[0058] a. Determine the electromagnetic field parameters: the preset frequency range is 100 Hz to 10 kHz, and the preset intensity range is 0.1 to 2 Tesla; the frequency and intensity depend on the characteristics of the composite metal wire and the processing conditions;
[0059] b. Design electromagnetic field assisted processing device to be used with laminating machine:
[0060] The electromagnetic field assisted processing device includes an electromagnetic field generator, a coil and a control system, wherein the electromagnetic field generator is used to provide power to the coil and the control system, the coil is used to generate an electromagnetic field with adjustable frequency and intensity, and the control system is used to adjust and monitor the electromagnetic field parameters generated by the coil to ensure the stability and consistency of the processing process.
[0061] c. After the stainless steel skin and the composite metal wire are fed into the laminating machine, the electromagnetic field assisted processing device is started, and the device generates an electromagnetic field with a preset frequency and intensity, which acts on the metal wire and graphite agent in the composite metal wire, and promotes the molecular arrangement of the composite metal wire after lamination under the action of the electromagnetic field of the preset frequency and preset intensity. By adjusting the electromagnetic field parameters and controlling the microstructure of the material, the crystallinity and conductivity of the material can be effectively improved.
[0062] During the processing, the electromagnetic field parameters can be monitored in real time by the control system, and the electromagnetic field parameters can be adjusted in real time according to the monitoring results to ensure the stability and consistency of the processing process to meet the requirements of composite material processing; finally, the crystallinity and conductive performance indicators of the composite grounding wire are tested in real time, and the electromagnetic field parameters are further optimized by real-time adjustment according to the evaluation results of the crystallinity and conductive performance indicators to improve the performance of the composite grounding wire.
[0063] Through the above-mentioned electromagnetic field-assisted processing process, the microstructure of the composite grounding wire can be effectively controlled, its crystallinity and conductivity can be improved, and reliable technical support can be provided for the preparation of high-quality composite grounding wires.
[0064] In addition, in the process of mixing the graphite agent and the metal wire, ultrasonic oscillation mixing technology is used. Under the action of ultrasonic waves, the dispersion and uniform mixing of the graphite agent can be accelerated, and the uniformity and stability of the composite material can be improved.
[0065] In the step 1, the graphite agent and the metal wire are mixed by using ultrasonic oscillation technology.
[0066] The steps of the ultrasonic oscillation mixing technology specifically include: putting the graphite agent and the metal wire into a mixing container according to a preset ratio, starting the ultrasonic oscillation mixing equipment to generate ultrasonic oscillation waves, so that the graphite agent and the metal wire in the mixing container are subjected to uniform ultrasonic oscillation; the frequency of the ultrasonic wave is 20 kHz to 100 kHz, the energy density is 0.1 to 2 W / cm², and the oscillation time is 5 min to 30 min.
[0067] Among them, in terms of ultrasonic oscillation mixing technology, it is necessary to select suitable equipment suitable for mixing graphite agent and metal wire to ensure that it can provide sufficient oscillation frequency and energy density. Secondly, the graphite agent and metal wire are mixed. This includes putting the graphite agent and metal wire into a mixing container in a certain proportion, and starting the ultrasonic oscillation mixing equipment to generate ultrasonic oscillation waves, so that the graphite agent and metal wire are uniformly subjected to ultrasonic oscillation in the mixing container.
[0068] In the mixing operation of graphite agent and metal wire, first of all, the ratio of graphite agent and metal wire should be determined according to the specific requirements and application scenarios of the prepared composite material, and this ratio varies in the mass ratio range of 1:5 to 1:20. Secondly, the parameters need to be controlled in detail, mainly including the frequency, energy density and time of ultrasonic oscillation. When selecting the frequency and energy density, factors such as the particle size, density of the graphite agent and metal wire and the size of the mixing container should be considered comprehensively. Usually, the energy density is adjusted between 0.1 and 2 W / cm² within the frequency range of 20 kHz to 100 kHz. The control of oscillation time should be ensured to be in the range of 5 minutes to 30 minutes to ensure that the graphite agent can be fully dispersed and evenly mixed during the mixing process.
[0069] Finally, during the mixing process, it is necessary to monitor and control the parameters in real time to ensure that the mixing effect meets the requirements. The performance of the mixed composite material is tested, including the evaluation of indicators such as uniformity and stability, and then the ultrasonic oscillation mixing parameters are optimized according to the test results to further improve the mixing effect and the quality of the composite material.
[0070] Through the above ultrasonic oscillation mixing technology implementation plan, rapid and uniform mixing can be achieved in the mixing process of graphite agent and metal wire, the uniformity and stability of the composite material can be improved, and an efficient and reliable technical means is provided for the preparation of composite grounding wires.
[0071] Furthermore, the composite grounding wire of the embodiment of the present invention is designed with a multi-layer structure. During the composite process of the stainless steel skin and the metal wire, the proportion and layout of each layer of material are controlled to achieve precise control of the performance of the composite material, thereby achieving better conductivity and corrosion resistance.
[0072] When designing multi-layered composite materials, it is necessary to consider the interactions between different material layers as well as the proportion and layout of each layer of material in order to precisely control the performance of the composite materials and achieve better conductivity and corrosion resistance.
[0073] First, determine the base layer and functional layer of the composite grounding wire. The base layer is the coating formed by the stainless steel skin on the outside of the composite grounding wire. The good mechanical properties and corrosion resistance of the stainless steel skin provide a solid foundation for the composite material. The functional layer is a protective layer formed outside the coating layer. The hierarchical structure of different functions is designed according to the needs. For example, the functional layer can include a conductive layer and an anti-corrosion layer from the inside to the outside, but it is not limited to this structure.
[0074] Secondly, the proportion of each layer of material needs to be controlled. For the conductive layer, determine the content of the metal wire and ensure its uniform distribution and conductivity; for the anti-corrosion layer, select a material with good corrosion resistance and determine its content and distribution. In the embodiment of the present invention, the conductive layer preferably includes 10%-30% of metal wire by mass; the anti-corrosion layer includes 5%-20% of corrosion-resistant material by mass.
[0075] In the composite grounding wire structure, the conductive layer and the anti-corrosion layer are crucial components, which play the important roles of providing conductivity and anti-corrosion functions respectively. First of all, as the core of the composite grounding wire, the main function of the conductive layer is to ensure effective conductivity to ensure the normal operation of the grounding wire. In order to achieve the best conductivity, it is necessary to reasonably control the content of metal wire (copper wire, aluminum wire or steel core wire) and ensure the uniform distribution of metal wire in the composite material. Metal wire materials include high-purity copper wire, aluminum wire and steel core copper wire. In the entire composite grounding wire, the metal wire content of the conductive layer is in the range of 10%-30%, and the specific content can be adjusted according to actual needs and conductivity requirements. Through appropriate process control and material mixing methods, the uniform distribution of metal wires in the composite material is ensured to avoid the occurrence of local uneven conductivity.
[0076] The anti-corrosion layer plays a key role in protecting metal materials from corrosion in composite grounding wires. The selection and content of the anti-corrosion layer directly affect the long-term stable operation of the grounding wire. The anti-corrosion layer materials include polymers, ceramics, etc., which have good chemical stability and corrosion resistance. The content of the anti-corrosion layer is usually in the range of 5%-20%, and the specific content can be adjusted according to the actual use environment and the degree of corrosion. Through appropriate coating, spraying or dipping and other process means, the anti-corrosion material is evenly covered on the surface of the conductive layer to ensure that the metal material is fully protected. By reasonably controlling the content and distribution of the conductive layer and the anti-corrosion layer, the conductivity and corrosion resistance of the composite grounding wire can be effectively improved to ensure its stable operation under different environmental conditions.
[0077] In terms of layout design, staggered stacking or layered arrangement is adopted to ensure close integration of different material layers, thereby enhancing the overall performance of the composite material. For the conductive layer, grid-like, criss-crossing and other layout methods can increase the connectivity of the conductive path; while for the anti-corrosion layer, uniform coverage or concentrated layout is adopted to ensure that the entire stainless steel skin can be effectively protected from corrosion.
[0078] In the layout design, the staggered stacking or layered arrangement is first adopted to ensure that the layers of materials of the composite grounding wire are closely combined, thereby enhancing its mechanical properties and stability. This layout method effectively reduces the stratification phenomenon between material layers and improves the overall strength and durability of the composite grounding wire.
[0079] For the layout design of the conductive layer, a grid-like, criss-cross, and other methods are used to increase the connectivity of the conductive path. Through a reasonably designed grid structure or staggered arrangement, the metal wires form multiple conductive paths in the composite material, which improves the conductive performance and uniformity and ensures the effective conduction of the grounding wire.
[0080] For the layout design of the anti-corrosion layer, a uniform covering or centralized layout is adopted to ensure that the entire stainless steel skin is effectively protected against corrosion. By uniformly coating or centralized spraying of anti-corrosion materials, a complete anti-corrosion layer is formed, which effectively prevents environmental corrosion from invading the grounding wire and improves its corrosion resistance and service life.
[0081] Through the above layout design, the close combination of the various layers of the composite grounding wire can be achieved, the overall performance is improved, and the effective realization of the conductive layer and the anti-corrosion layer is ensured. This provides a guarantee for the reliable operation of the composite grounding wire in various environments.
[0082] Finally, in terms of processing technology, processing parameters such as temperature, pressure, speed, etc. are strictly controlled to ensure that each layer of material can be evenly compacted and combined.
[0083] The embodiment of the present invention provides a novel method for preparing a composite grounding wire, and the technical problem solved by the method mainly includes how to prepare the composite grounding wire and ensure that the composite grounding wire has good electrical conductivity and corrosion resistance.
[0084] Through the preparation method provided by the embodiment of the present invention, first, in the raw material collection stage, copper wire, aluminum wire, steel core wire and reserved stainless steel skin are used as raw materials to ensure that the composite grounding wire has excellent electrical conductivity and corrosion resistance. Secondly, in the preparation process of the composite material, the graphite agent is added to the stainless steel skin by the graphite additive adding device, and the rapid and uniform mixing of the graphite agent and the metal wire is achieved by combining the electromagnetic field assisted processing technology and the ultrasonic oscillation mixing technology, thereby improving the uniformity and stability of the composite material. In terms of multi-level structural design, by controlling the proportion and layout of each layer of material, the precise regulation of the performance of the composite material is further achieved, ensuring that the composite grounding wire has better electrical conductivity and corrosion resistance. Finally, in the preparation process, after multiple drawing and annealing treatments, it is ensured that the material structure and performance of the composite grounding wire are further optimized and stabilized, and finally a single-wire core collection product is obtained, that is, a prepared composite grounding wire product. In summary, the technical solution of the embodiment of the present invention achieves the goal of high efficiency and stability in the preparation process of the composite grounding wire, and improves the electrical conductivity and corrosion resistance of the composite grounding wire.
[0085] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.
Claims
1. A method for preparing a composite grounding wire, characterized in that: The following steps are involved: Step 1: adding graphite agent to metal wire through graphite additive adding device to mix to obtain composite metal wire, sending stainless steel skin and the composite metal wire into a coating machine for processing and pressing, so that the stainless steel skin is coated on the outside of the composite metal wire to form a coating layer, and promoting the orderly arrangement of molecules of the composite metal wire after coating under the action of electromagnetic field of preset frequency and preset intensity through electromagnetic field assisted processing technology, twisting the composite metal wire after pressing and electromagnetic processing, laser welding the side seams of the coating layer, and then sending it into a polishing machine for polishing to form a composite grounding wire core; Step 2: performing a first-stage drawing process on the composite grounding wire core; Step 3: performing a first-stage annealing treatment on the composite grounding wire core after the first-stage drawing treatment, with the annealing temperature being 300-400° C.; Step 4: performing a second-stage drawing process on the composite grounding wire core after the first-stage annealing process; Step 5: performing a second-stage annealing treatment on the composite grounding wire core after the second-stage drawing treatment, with the annealing temperature being 200-250° C.; Step 6: performing single-filament forming on the composite grounding wire core after the second stage annealing treatment, that is, forming the composite grounding wire; The graphite agent and the metal wire are mixed by using ultrasonic oscillation technology; The steps of the ultrasonic oscillation technology include: putting the graphite agent and the metal wire into a mixing container according to a preset ratio, using an ultrasonic oscillation mixing device to generate ultrasonic oscillation waves, so that the graphite agent and the metal wire in the mixing container are subjected to uniform ultrasonic oscillation; The electromagnetic field assisted processing technology is used to promote the orderly arrangement of molecules of the composite metal wire after coating under the action of an electromagnetic field of a preset frequency and a preset intensity, and includes the following steps: a. Determine the electromagnetic field parameters: the preset frequency range is 100 Hz to 10 kHz, and the preset intensity range is 0.1 to 2 Tesla; b. Design an electromagnetic field assisted processing device: The electromagnetic field assisted processing device includes an electromagnetic field generator, a coil and a control system, wherein the electromagnetic field generator is used to provide power to the coil and the control system, the coil is used to generate an electromagnetic field with adjustable frequency and intensity, and the control system is used to adjust and monitor the electromagnetic field parameters generated by the coil; c. After the stainless steel skin and the composite metal wire are fed into the coating machine, an electromagnetic field-assisted processing device is used to cause the coated composite metal wire to be arranged in an orderly manner under the action of an electromagnetic field of a preset frequency and a preset intensity.
2. The method for preparing a composite grounding wire according to claim 1, characterized in that: The first-stage drawing treatment, the first-stage annealing treatment, the second-stage drawing treatment and the second-stage annealing treatment are performed in an environment of protective gas.
3. The method for preparing the composite grounding wire according to claim 2, characterized in that: The protective gas is nitrogen.
4. The method for preparing a composite grounding wire according to claim 1, characterized in that: In the step 1, the graphite additive adding device includes an adding box and a discharge conduit connected to the outlet of the adding box, and the discharge conduit is located above the running wheels of the laminating machine.
5. The method for preparing the composite grounding wire according to claim 1, characterized in that: The ultrasonic oscillation wave has a sound wave frequency of 20 kHz to 100 kHz, an energy density of 0.1 to 2 W / cm², and an oscillation time of 5 min to 30 min.
6. The method for preparing a composite grounding wire according to claim 1, characterized in that: In the step 1, a functional layer is formed outside the coating layer, and the functional layer includes a conductive layer and an anti-corrosion layer in sequence from the inside to the outside.
7. The method for preparing the composite grounding wire according to claim 6, characterized in that: In step 1, the conductive layer comprises 10%-30% by mass of metal wires; and the anti-corrosion layer comprises 5%-20% by mass of corrosion-resistant materials.
8. The method for preparing a composite grounding wire according to claim 1, characterized in that: The control system is used to monitor the electromagnetic field parameters in real time, and the crystallinity and conductivity performance indicators of the composite grounding wire are tested in real time, and the electromagnetic field parameters are adjusted and optimized in real time according to the crystallinity and conductivity performance indicators.