A seamless metal composite pipe perforation rolling method and perforation rolling equipment

By utilizing liquid metal filling and space die technology in the piercing and rolling method of seamless metal composite pipes, the problems of low forming efficiency and weak bonding strength in the existing technology are solved, and efficient and customized seamless metal pipes are realized. Composite tube forming improves the accuracy and bonding strength of the finished product.

CN118543659BActive Publication Date: 2024-10-11HAI AN & TAIYUAN UNIV OF TECH ADVANCED MFG & INTELLIGENT EQUIP IND RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028961.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing seamless metal composite pipe preparation technology has problems such as low forming efficiency, weak bonding strength, poor component performance, and long process flow. It is difficult to meet the needs of modern industry for efficient continuous formability and controllable forming.

Method used

The seamless metal composite pipe piercing and rolling method is used to process grooves or protrusions on the inner surface of the solid outer metal or the outer surface of the solid inner metal, fill the liquid inner metal or pour the liquid outer metal, and taper the A space die is installed on the shaped roller and the tapered head to increase the contact area, and the shape, size, distribution, and position of the space die are adjusted to achieve customization of the composite interface space structure.

Benefits of technology

It significantly improves the forming efficiency and bonding strength, realizes efficient customization of composite interfaces, improves equipment service life and product accuracy, reduces energy consumption, and can produce seamless metal composite pipes with a variety of structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118543659B_ABST
    Figure CN118543659B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of seamless metal composite pipe forming, and provides a seamless metal composite pipe perforation rolling method, which includes the following steps: S1, matching and designing component metals; S2, designing a spatial composite interface; S3, prefabricating a composite blank; S4, heating the composite blank; S5, perforating and rolling composite; S6, collecting the final product. In the seamless metal composite pipe perforation rolling equipment provided by the present invention, the background unit drives the conical mandrel to move forward along the rolling axis through the mandrel, and the pusher sends the prefabricated composite blank along the guide tube into the deformed hole formed by the conical roller, the guide device and the conical mandrel for perforation and rolling composite, thereby obtaining a seamless metal composite pipe. The present invention solves many problems of the prior art such as low forming efficiency, weak bonding strength, poor component performance, and long process flow, and has the advantages of simple and reliable equipment structure, high forming efficiency, high service life, high bonding strength of the composite interface, and customizable composite interface configuration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of seamless metal composite pipe forming, and in particular relates to a seamless metal composite pipe perforation rolling method and perforation rolling equipment thereof. Background Art

[0002] At the same time, with the increasing demand for production and manufacturing, seamless steel pipes made of a single material can no longer meet the performance requirements of special service environments in modern industrial engineering, so seamless metal composite pipes came into being. Seamless metal composite pipes refer to structural and functional integrated composite materials that are made of multiple layered component metal pipes through interface bonding to complete functional transformation. Because they have the excellent structural and functional characteristics of multiple component metal pipes, they can be widely used in aerospace, petrochemical, weapons and equipment, automobile manufacturing, marine engineering, pipeline engineering and other fields, thus having huge market demand.

[0003] Explosive bonding refers to a processing technology that uses the huge energy generated by the explosion of explosives to instantly weld and bond two or more different materials together. The use of this technology to prepare seamless metal composite pipes includes the following key steps: first, the base pipe is placed inside the covering pipe, second, explosives are laid inside the base pipe, and third, the instantaneous ultra-high pressure and ultra-high speed impact energy generated by the explosion of explosives are used to achieve metallurgical bonding between component metal layers, atomic diffusion and severe plastic deformation occur between metals, and periodic explosion waves form a wavy composite interface, which is conducive to increasing the bonding area and bonding strength. However, the disadvantages of explosive bonding are also very obvious. For example, seamless metal composite pipes are prone to cracks, there is serious noise and environmental pollution, and the forming efficiency is low, which restricts its subsequent development and application. Hydraulic expansion is a method that uses liquid pressure and molds to process seamless metal pipes into a certain shape. The process principle is simple but the processing efficiency is low. The hydraulic expansion machine needs to punch and process a pipe or pipe joint many times, which will lead to relatively low processing efficiency, especially in the expansion process of high-strength steel pipes or large-diameter steel pipes. The processing efficiency is even slower, and for seamless metal composite pipes, only mechanical bonding can be achieved, which cannot withstand thermal stress.

[0004] Therefore, existing preparation technologies such as explosive compounding and hydraulic expansion face many problems such as low forming efficiency, weak bonding strength, poor component performance, and long process flow. It is urgent to develop efficient, continuous, shape-controlled forming technology and equipment for seamless metal composite pipes. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a seamless metal composite pipe perforation rolling method and a perforation rolling device thereof. By machining grooves or protrusions on the inner surface of the solid outer metal or the outer surface of the solid inner metal, filling with liquid inner metal or pouring liquid outer metal, the forming efficiency can be significantly improved. At the same time, a spatial die head is arranged on the surface of the conical head or the conical roller, which can increase the contact area and strengthen the interface bonding between the inner metal and the outer metal. In addition, the shape, size, distribution, position and other rules of the spatial die head can be adjusted to realize the customization of the composite interface spatial structure, and obtain spiral and cross-shaped spatial composite interfaces, as well as various structural products such as outer surface corrugations and inner surface corrugations. The equipment has the advantages of simple and reliable structure and long service life.

[0006] The present invention provides a method for perforating and rolling a seamless metal composite pipe, which comprises the following steps:

[0007] S1. Determine the component metal: Determine the component metal information of the seamless metal composite pipe according to the working environment performance requirements of the target product;

[0008] S2. Determine the composite interface type: According to the working environment load requirements of the target product, the composite interface of the seamless metal composite pipe adopts a spatial corrugated composite interface;

[0009] S3. Determine the spatial corrugation composite interface: determine the combination type of the spatial corrugation composite interface of the seamless metal composite pipe and the structural parameters of the spatial corrugation composite interface;

[0010] S4. Determine the process for forming a spatial corrugated composite interface: the conical roller and the conical mandrel form a spatial corrugated composite interface;

[0011] S5. Determine the assembly method of the spatial corrugated composite interface prefabricated composite blank: determine whether the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method. If the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method, the outer metal or the inner metal is determined to be a solid metal, and solid-liquid composite assembly is performed by casting to form the prefabricated composite blank; if the assembly method of the prefabricated composite blank adopts the solid-solid composite assembly method, the outer metal and the inner metal are solid-phase packaged, and both ends of the solid-phase packaged package are sealed and vacuumed to form the prefabricated composite blank;

[0012] S6, heating the prefabricated composite blank: heating the prefabricated composite blank at the same temperature or at different temperatures, and waiting for piercing and rolling compounding after reaching the target piercing and rolling temperature;

[0013] S7, determining the spatial die: according to the determined spatial corrugation composite interface, an outer spatial die is arranged on the conical roller, an inner spatial die is arranged on the conical mandrel, or an outer spatial die and an inner spatial die are arranged on the conical roller and the conical mandrel respectively at the same time;

[0014] S8. Determine the deformed pass: determine the size of the seamless metal composite pipe according to the target size specification, start the push rod trolley to drive the conical mandrel to move forward along the rolling axis to a preset position, and adjust the installation positions of the conical roller and the guide device respectively, so that the conical roller, the guide device and the conical mandrel together form a deformed pass;

[0015] S9, conveying the composite blank: conveying the prefabricated composite blank along the guide tube into the deformed hole formed by the tapered roller, the guide device and the tapered head through the pusher;

[0016] S10, piercing and rolling composite: under the combined action of the internal piercing of the conical head, the edge guiding of the guide device and the external rolling of the conical roller, the wall thickness of the prefabricated composite billet is thinned and axially extended to obtain a seamless metal composite pipe with a spatial corrugated composite interface;

[0017] S11. Collecting final products: The prefabricated composite billet is subjected to perforation, rolling and composite to obtain a seamless metal composite pipe, and after cooling and sizing operations, a seamless metal composite pipe finished product of target size is finally obtained.

[0018] Furthermore, the outer space die is arranged in the biting section or the sizing section of the tapered roller, which can form a concave-convex morphology on the outer surface of the seamless metal composite tube. When the height of the outer space die is higher than the maximum height of the sizing section, a seamless metal composite tube with a concave-convex morphology on the outer surface can be obtained. When the height of the outer space die is lower than the maximum height of the sizing section, the concave-convex morphology on the outer surface of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth outer surface and a spatial corrugated composite interface can be obtained.

[0019] Furthermore, the inner space die is arranged at the configuration section or the flattening section of the conical top head, and a concave-convex topography is formed on the inner surface of the seamless metal composite tube. When the height of the inner space die is higher than the maximum height of the finishing section, a seamless metal composite tube with a concave-convex topography on the inner surface can be obtained. When the height of the inner space die is lower than the maximum height of the finishing section, the concave-convex topography on the inner surface of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth inner surface but a spatial corrugated composite interface can be obtained.

[0020] The second aspect of the present invention provides a perforation rolling device for a seamless metal composite pipe perforation rolling method, which includes a main machine base unit, a main transmission unit, a front unit and a back unit, the front unit, the main machine base unit, the main transmission unit and the back unit are arranged in sequence along the rolling axis, the front unit is arranged at the entrance end of the main machine base unit, the front unit includes a pusher, a material receiving trough and a guide tube, and the pusher, the material receiving trough and the guide tube are arranged in sequence along the rolling axis; the main machine base unit includes a rolling mill frame, a tapered roller and a guide device, the tapered roller is a tapered structure with a gradually changing diameter, and along the center axis of the tapered roller A plurality of segmented cones are sequentially arranged from the inlet end to the outlet end of the line, and the plurality of segmented cones include a biting section, a sizing section and a diameter expansion section, and an outer arc surface of the tapered roller is provided with an outer space die head, the tapered roller and the guide device are arranged on the rolling mill frame, and are evenly arranged along the circumference of the rolling axis, and the tapered roller, the guide device and the tapered head together constitute a deformation hole type; the main transmission unit is arranged on both sides of the backstage unit, and the main transmission unit includes a main motor, a main reducer and a universal joint shaft, the output shaft of the main motor is connected to the input shaft of the main reducer, and the output shaft of the main reducer is connected to the tapered roller through the universal joint shaft; The backstage unit is arranged at the outlet end of the main machine base unit, and the backstage unit includes a backstage frame, a conical plug, a push rod, a push rod trolley and a plurality of centering machines. The conical plug is a conical structure with a gradually changing diameter, and a plurality of segmented cones are arranged in sequence from the inlet end to the outlet end along the central axis of the conical plug. The plurality of segmented cones include a top section, a configuration section, a flat section, a finishing section and an exit section, and the generatrix of the finishing section in the conical plug is parallel to the generatrix of the sizing section in the conical roller. An inner space die is arranged on the outer arc surface of the conical plug. The plurality of centering machines are arranged at the first end of the backstage frame, and the push rod trolley is slidingly arranged at the backstage frame. The second end of the table frame is connected, and the first end of the conical plug is connected to the first end of the push rod, and the second end of the push rod is connected to the push rod trolley. The push rod trolley can drive the conical plug to move along the rolling axis on the background frame through the push rod, and the conical plug and the push rod can rotate around the rolling axis; the prefabricated composite billet is placed in the receiving trough, and the pusher sends the prefabricated composite billet along the guide tube into the deformation hole formed by the conical roller, the guide device and the conical plug. The push rod trolley drives the conical plug to move forward along the rolling axis through the push rod, and perforation rolling is performed at the center of the prefabricated composite billet to obtain a seamless metal composite pipe.

[0021] Preferably, the angle between the projection of the tapered roller axis and the rolling axis on the main vertical plane is the feed angle β , and the input angle β The angle range is 0-15°, the projection angle between the tapered roller axis and the rolling axis on the rolling main plane is the rolling angle α, and the angle range of the rolling angle α is 0-20°.

[0022] Preferably, the angle between the generatrix of the biting section in the tapered roller and the projection of the rolling axis on the main rolling plane is the biting angle αIn The angle between the generatrix of the expansion section of the tapered roller and the projection of the rolling axis on the main rolling plane is the expansion angle α Out , and the angle between the generatrix of the biting section and the central axis of the tapered roller is the first angle α 1, and α 1= α + α In The angle between the generatrix of the sizing section and the center axis of the tapered roller is the second angle α 2, and α 2= α The angle between the generatrix of the expansion section and the center axis of the tapered roller is the third angle α 3. α 3= α 2- α Out , and the first angle α 1 is greater than the second angle α 2. Second angle α 2 is greater than the third angle α 3.

[0023] Preferably, the spatial structure of the outer space die head adopts a point structure, a linear structure or a ring structure, and the distribution method of the outer space die head adopts an axial distribution method along the central axis of the tapered roller on the outer arc surface of the tapered roller, a circumferential distribution method around the central axis of the tapered roller on the outer arc surface of the tapered roller, a spiral distribution method on the outer arc surface of the tapered roller, or a cross distribution method on the outer arc surface of the tapered roller.

[0024] Preferably, the angle between the generatrix of the top section in the conical plug and the central axis of the conical plug is the first plug angle, the angle between the generatrix of the configuration section in the conical plug and the central axis of the conical plug is the second plug angle, the angle between the generatrix of the flattening section in the conical plug and the central axis of the conical plug is the third plug angle, the angle between the generatrix of the finishing section in the conical plug and the central axis of the conical plug is the fourth plug angle, the angle between the generatrix of the exit section in the conical plug and the central axis of the conical plug is the fifth plug angle, and the first plug angle is greater than the second plug angle, the second plug angle is greater than the third plug angle, the third plug angle is greater than the absolute value of the fifth plug angle, and the absolute value of the fifth plug angle is greater than the fourth plug angle.

[0025] Preferably, the spatial structure of the inner space die head adopts a point structure, a linear structure or a ring structure, and the distribution method of the inner space die head adopts an axial distribution method along the central axis of the conical plug on the outer arc surface of the conical plug, a circumferential distribution method around the central axis of the conical plug on the outer arc surface of the conical plug, a spiral distribution method on the outer arc surface of the conical plug, or a cross distribution method on the outer arc surface of the conical plug.

[0026] A third aspect of the present invention provides a method for piercing and rolling a seamless metal composite pipe, comprising the following steps:

[0027] S1. Determine the component metal: Determine the component metal information of the seamless metal composite pipe according to the working environment performance requirements of the target product;

[0028] S2. Determine the composite interface type: according to the target product working environment load requirement, determine whether the composite interface of the seamless metal composite pipe adopts a spatial corrugated composite interface. If the composite interface of the seamless metal composite pipe adopts a spatial corrugated composite interface, execute step S4; if the composite interface of the seamless metal composite pipe adopts a spatial smooth composite interface, execute step S3;

[0029] S3, determining the assembly method of the prefabricated composite blank with a spatially smooth composite interface: according to the working environment performance requirements of the target product, judging whether the assembly method of the prefabricated composite blank adopts a solid-liquid composite assembly method; if the assembly method of the prefabricated composite blank adopts a solid-liquid composite assembly method, the outer metal or the inner metal is determined to be a solid metal, and a solid-liquid composite assembly is performed by casting to form a prefabricated composite blank; if the assembly method of the prefabricated composite blank adopts a solid-solid composite assembly method, the outer metal and the inner metal are solid-phase packaged, and both ends of the solid-phase packaged assembly are sealed and vacuumed to form a prefabricated composite blank; after the prefabricated composite blank is completed, step S8 is executed;

[0030] S4. Determine the spatial corrugation composite interface: determine the combination type of the spatial corrugation composite interface of the seamless metal composite pipe and the structural parameters of the spatial composite interface;

[0031] S5, determining the spatial corrugated composite interface forming process: judging whether the spatial corrugated composite interface is formed by rolling with a conical roller and a conical mandrel; if the spatial corrugated composite interface is formed by rolling with a conical roller and a conical mandrel, a prefabricated composite blank of a spatial smooth composite interface is used, and step S7 is executed; if the spatial corrugated composite interface is not formed by rolling with a conical roller and a conical mandrel, a prefabricated composite blank of a spatial corrugated composite interface is used, and step S6 is executed;

[0032] S6. Determine the assembly method of the prefabricated composite blank of the spatial corrugated composite interface: determine whether the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method according to the working environment performance requirements of the target product. If the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method, the outer metal or the inner metal is determined to be a solid metal; if the outer metal is determined to be solid, a concave-convex morphology is set on the inner surface of the outer metal; if the inner metal is determined to be solid, a concave-convex morphology is set on the outer surface of the inner metal. The prefabricated composite blank is formed by solid-liquid composite assembly through casting; if the prefabricated composite blank is assembled by solid-solid composite assembly, a concave-convex morphology is set on the inner surface of the outer metal, a concave-convex morphology is set on the outer surface of the inner metal, or a concave-convex morphology is set on the inner surface of the outer metal and the outer surface of the inner metal at the same time, and the outer metal and the inner metal are solid-phase packaged, and both ends of the solid-phase packaged blank are sealed and vacuumed to form a prefabricated composite blank. After the prefabricated composite blank is completed, step S8 is executed;

[0033] S7, determining the assembly method of the prefabricated composite blank with a spatially smooth composite interface: judging whether the assembly method of the prefabricated composite blank adopts a solid-liquid composite assembly method; if the assembly method of the prefabricated composite blank adopts a solid-liquid composite assembly method, the outer metal or the inner metal is determined to be a solid metal, and solid-liquid composite assembly is performed by casting to form a prefabricated composite blank; if the assembly method of the prefabricated composite blank adopts a solid-solid composite assembly method, the outer metal and the inner metal are solid-phase packaged, and both ends of the solid-phase packaged assembly are sealed and vacuumed to form a prefabricated composite blank. After the prefabricated composite blank is completed, step S8 is executed;

[0034] S8, heating the composite blank: heating the prefabricated composite blank at the same temperature or at different temperatures, and waiting for piercing and rolling composite after reaching the target piercing and rolling temperature;

[0035] S9, piercing and rolling compounding: start the push rod trolley to drive the conical mandrel to move forward to the preset position along the rolling axis, adjust the installation positions of the conical roller and the guide device respectively, and perform piercing and rolling compounding on the prefabricated composite billet in the deformed hole formed by the conical roller, the guide device and the conical mandrel;

[0036] S10, collecting final products: the prefabricated composite billet is subjected to perforation, rolling and composite to obtain a seamless metal composite pipe, and after cooling and sizing operations, a seamless metal composite pipe finished product of target size is finally obtained.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] 1. The seamless metal composite pipe piercing and rolling method and piercing and rolling equipment provided by the present invention have a simple and reliable equipment structure and a long service life. Under the condition that the structure of the tapered roller and the tapered head is not changed, a segmented gradual change treatment is performed. The tapered roller includes a bite section, a sizing section, and a diameter expansion section. The tapered head includes a top section, a configuration section, a flattening section, a finishing section, and an exit section. Through the gradual segmented treatment, the metal flow law is improved, and the wear and consumption of the tapered head is reduced, thereby increasing the service life of the equipment, and further improving the size accuracy and shape accuracy of the seamless metal composite pipe blank after piercing and rolling.

[0039] 2. The perforation and rolling method of seamless metal composite pipes and the perforation and rolling equipment provided by the present invention can be flexibly assembled to improve the forming efficiency. The inner surface of the solid outer metal or the outer surface of the solid inner metal is processed with grooves or protrusions, and the liquid inner metal is filled or the liquid outer metal is poured. The problems of high requirements for coaxiality, cylindricity, cleanliness, etc. in traditional solid-solid composite assembly can be avoided. The high temperature of the solid-liquid interface promotes the diffusion of interface elements and realizes metallurgical bonding, which can significantly improve the forming efficiency. The mutual meshing effect of the spatial composite interface can significantly improve the coordinated deformation ability. The prefabricated composite blank obtained after the liquid metal solidifies is still in a high temperature state and directly enters the heating furnace for heating, which can significantly reduce energy consumption.

[0040] 3. The perforation and rolling method of a seamless metal composite pipe and the perforation and rolling equipment provided by the present invention can increase the contact area and strengthen the interface bonding. The inner space die of the configuration section of the conical head can form an internal surface concave-convex morphology on the seamless metal composite blank, which is then rolled flat in the flattening section to obtain a smooth internal surface morphology, and finally the target size is obtained through the finishing section. However, there is a macroscopic or microscopic spatial composite interface between the component metals, which can significantly increase the bonding area and enhance the bonding strength. In addition, when the height of the inner space die is higher than the flattening section, the internal surface concave-convex morphology cannot be rolled flat in the flattening section, thereby retaining the internal surface concave-convex morphology to obtain a seamless metal composite pipe with an internal surface concave-convex morphology.

[0041] 4. The seamless metal composite pipe perforation rolling method and perforation rolling equipment provided by the present invention, the outer space die head of the biting section of the tapered roller can form an external surface concave-convex morphology on the seamless metal composite billet, which is then flattened in the sizing section to obtain a smooth external surface morphology, and finally the target size is obtained through the diameter expansion section, but there is a macroscopic or microscopic spatial composite interface between the component metals, which can significantly increase the bonding area and enhance the bonding strength. In addition, when the height of the outer space die head is higher than the sizing section, the external surface concave-convex morphology cannot be flattened in the sizing section, thereby retaining the external surface concave-convex morphology to obtain a seamless metal composite pipe with an external surface concave-convex morphology.

[0042] 5. The perforation rolling method and perforation rolling equipment for seamless metal composite pipes provided by the present invention can achieve efficient forming and customized interface structure. The conical rollers and conical head are integrated in design. Segmented cones with gradually changing diameters are sequentially arranged along the rolling axis from the inlet side to the outlet side. The forming process and the flattening process of the concave and convex surface are highly concentrated. The spatial structure of the composite interface can be customized by adjusting the shape, size, distribution, position and other rules of the spatial die head, and various structural products such as spiral and cross-shaped spatial composite interfaces, as well as outer surface corrugations and inner surface corrugations can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a flow chart of using a conical roller and a conical mandrel to pierce and roll a composite blank in the spatial corrugation composite process of the present invention;

[0044] Figure 2 It is a flow chart of the method for perforating and rolling a smooth composite interface and spatial corrugated composite seamless metal composite pipe of the present invention;

[0045] Figure 3 It is a schematic diagram of the structure of the solid outer metal processing space groove in the present invention;

[0046] Figure 4 It is a schematic diagram of the structure of the solid inner metal processing space protrusion in the present invention;

[0047] Figure 5 The prefabricated composite blank with a spatial composite interface obtained in the present invention;

[0048] Figure 6 It is a schematic diagram of the overall structure of the seamless metal composite pipe perforating and rolling equipment of the present invention;

[0049] Figure 7 It is a schematic diagram of the deformation zone of the seamless metal composite pipe piercing and rolling equipment of the present invention;

[0050] Figure 8 It is a schematic diagram of the arrangement of the tapered roller partitions and feed angles of the present invention;

[0051] Fig. 9 It is a schematic diagram of the arrangement of the tapered roller partitions and rolling angles of the present invention;

[0052] Fig.10 It is a schematic diagram of the partitioning of the conical plug of the present invention;

[0053] Fig.11 It is a schematic diagram of the structure of a tapered roller with an outer space die head of the present invention;

[0054] Fig.12 The present invention adopts Fig.11 Schematic diagram of the structure of a seamless metal composite pipe that can be obtained when the outer space die head of the middle tapered roller is lower than the sizing section;

[0055] Fig.13 The present invention adopts Fig.11 Schematic diagram of the structure of a seamless metal composite pipe that can be obtained when the outer space die head of the middle tapered roller is higher than the sizing section;

[0056] Fig.14 It is a schematic diagram of the structure of a conical mandrel with an inner space die head of the present invention;

[0057] Fig.15 The present invention adopts Fig.14 Schematic diagram of the seamless metal composite pipe structure that can be obtained when the inner space die head of the middle conical head is lower than the flat section;

[0058] Fig.16 The present invention adopts Fig.14 Schematic diagram of the seamless metal composite pipe structure that can be obtained when the inner space die head of the middle conical head is higher than the flat section;

[0059] Fig.17 It is a schematic diagram of the structure of a conical mandrel with three spatial dies of the present invention;

[0060] Fig.18 The present invention adopts Fig.17 Schematic diagram of the seamless metal composite pipe structure that can be obtained with a medium tapered plug.

[0061] Main reference numerals:

[0062] 1. Main machine base unit; 101. Rolling mill frame; 102. Conical roller; 1021. Biting section; 1022. Sizing section; 1023. Expansion section; 1024. Outer space die head; 103. Guide device; 2. Main transmission unit; 201. Main motor; 202. Main reducer; 203. Universal joint shaft; 3. Front unit; 301. Pusher; 302. Receiving trough; 303. Guide tube; 4. , backstage unit; 401, conical top; 4011, top section; 4012, configuration section; 4013, flat section; 4014, finishing section; 4015, exit section; 4016, inner space die head; 402, ejector; 403, ejector trolley; 404, centering machine; 405, thrust seat; 406, backstage frame; 5, outer metal; 51, groove; 6, inner metal; 61, protrusion. DETAILED DESCRIPTION

[0063] In order to fully describe the technical content, structural features, objectives and effects of the present invention, the following will be described in detail with reference to the accompanying drawings.

[0064] The present invention provides a method for perforating and rolling a seamless metal composite pipe. Figure 1 As shown, it includes the following steps:

[0065] S1. Determine the component metal: Determine the component metal information of the seamless metal composite pipe according to the working environment performance requirements of the target product;

[0066] S2. Determine the composite interface type: According to the working environment load requirements of the target product, the composite interface of the seamless metal composite pipe adopts a spatial corrugated composite interface;

[0067] S3. Determine the spatial corrugation composite interface: determine the combination type of the spatial corrugation composite interface of the seamless metal composite pipe and the structural parameters of the spatial corrugation composite interface;

[0068] S4, determining the process for forming a spatial corrugated composite interface: using a conical roller 102 and a conical mandrel 401 to form a spatial corrugated composite interface;

[0069] S5. Determine the assembly method of the spatial corrugated composite interface prefabricated composite blank: determine whether the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method. If the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method, the outer metal or the inner metal is determined to be a solid metal, and solid-liquid composite assembly is performed by casting to form the prefabricated composite blank; if the assembly method of the prefabricated composite blank adopts the solid-solid composite assembly method, the outer metal and the inner metal are solid-phase packaged, and both ends of the solid-phase packaged package are sealed and vacuumed to form the prefabricated composite blank;

[0070] S6, heating the composite blank: heating the prefabricated composite blank at the same temperature or at different temperatures, and waiting for piercing and rolling composite after reaching the target piercing and rolling temperature;

[0071] S7, determine the spatial die: according to the determined spatial corrugation composite interface, set the outer spatial die 1024 on the conical roller 102, set the inner spatial die 4016 on the conical head 401, or simultaneously set the outer spatial die 1024 and the inner spatial die 4016 on the conical roller 102 and the conical head 401 respectively;

[0072] S8, determining the deformed pass: according to the size of the seamless metal composite pipe of the target size specification, start the push rod trolley 403 to drive the conical mandrel 401 to move forward to the preset position along the rolling axis, and adjust the installation positions of the conical roller 102 and the guide device 103 respectively, so that the conical roller 102, the guide device 103 and the conical mandrel 401 together form a deformed pass;

[0073] S9, conveying the prefabricated composite blank: conveying the prefabricated composite blank along the guide tube 303 into the deformed hole formed by the tapered roller 102, the guide device 103 and the tapered plug 401 through the pusher 301;

[0074] S10, piercing and rolling composite: under the combined action of the internal piercing of the conical plug 401, the edge guiding of the guide device 103 and the external rolling of the conical roller 102, the wall thickness of the prefabricated composite blank is thinned and axially extended, so as to obtain a seamless metal composite pipe with a spatial corrugated composite interface;

[0075] S11. Collecting final products: The prefabricated composite billet is subjected to perforation, rolling and composite to obtain a seamless metal composite pipe, and after cooling and sizing operations, a seamless metal composite pipe finished product of target size is finally obtained.

[0076] like Figure 8 and Fig. 9 As shown, the outer diameter of the seamless metal composite pipe is d The outer space die 1024 can be arranged at the biting section 1021 and the sizing section 1022 of the tapered roller 102. When the outer space die 1024 is arranged at the biting section 1021, a concave-convex shape can be formed on the outer surface of the seamless metal composite tube. When the height of the outer space die 1024 is higher than the maximum height of the sizing section 1022, the concave-convex shape of the outer surface of the seamless metal composite tube cannot be rolled flat, and a seamless metal composite tube with a concave-convex shape on the outer surface can be obtained. When the height of the outer space die 1024 is lower than the maximum height of the sizing section 1022, the concave-convex shape of the outer surface of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth outer surface and a spatial corrugated composite interface can be obtained. When the outer space die 1024 is set in the sizing section 1022, a concave-convex morphology can be formed on the outer surface of the seamless metal composite tube. When the height of the outer space die 1024 is higher than the maximum height of the sizing section 1022, the concave-convex morphology of the outer surface of the seamless metal composite tube cannot be rolled flat, and a seamless metal composite tube with a concave-convex morphology on the outer surface can be obtained. When the height of the outer space die 1024 is lower than the maximum height of the sizing section 1022, the concave-convex morphology of the outer surface of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth outer surface and a spatial corrugated composite interface can be obtained.

[0077] like Fig.10As shown, the inner space die 4016 can be arranged in the configuration section 4012 and the flat section 4013 of the conical head 401. When the inner space die 4016 is arranged in the configuration section 4012, a concave-convex morphology can be formed on the inner surface of the seamless metal composite tube. When the height of the inner space die 4016 is higher than the maximum height of the flat section 4013, the concave-convex morphology of the inner surface of the seamless metal composite tube cannot be rolled flat, and a seamless metal composite tube with a concave-convex morphology on the inner surface can be obtained. When the height of the inner space die 4016 is lower than the maximum height of the flat section 4013, the concave-convex morphology of the inner surface of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth inner surface but a spatial corrugated composite interface can be obtained. When the inner space die 4016 is set in the flattening section 4013, a concave-convex morphology can be formed on the inner surface of the seamless metal composite tube. When the height of the inner space die 4016 is higher than the maximum height of the flattening section 4013, the concave-convex morphology on the inner surface of the seamless metal composite tube cannot be rolled flat, and a seamless metal composite tube with a concave-convex morphology on the inner surface can be obtained. When the height of the inner space die 4016 is lower than the maximum height of the flattening section 4013, the concave-convex morphology on the inner surface of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth inner surface but a spatial corrugated composite interface can be obtained.

[0078] A second aspect of the present invention provides a method for piercing and rolling a seamless metal composite pipe, such as Figure 2 As shown, it includes the following steps:

[0079] S1. Determine the component metal: Determine the component metal information of the seamless metal composite pipe according to the working environment performance requirements of the target product, such as the component metal material matching, size specifications, layer thickness ratio, and arrangement information;

[0080] S2. Determine the type of composite interface: according to the load requirements of the working environment of the target product, determine whether the composite interface of the seamless metal composite pipe adopts a spatial corrugated composite interface. If the composite interface of the seamless metal composite pipe adopts a spatial corrugated composite interface, that is, the seamless metal composite pipe needs to have excellent radial bending resistance, axial shear resistance, circumferential torsion resistance and other comprehensive bearing properties, then execute step S4; if the composite interface of the seamless metal composite pipe adopts a smooth composite interface, then execute step S3;

[0081] S3, determine the prefabricated composite blank with a smooth composite interface: according to the working environment performance requirements of the target product, determine whether the prefabricated composite blank is assembled in a solid-liquid composite manner; if the prefabricated composite blank is assembled in a solid-liquid composite manner, the outer metal 5 or the inner metal 6 is determined to be a solid metal, and solid-liquid composite assembly is performed by casting to form the prefabricated composite blank; if the prefabricated composite blank is assembled in a solid-solid composite manner, the outer metal 5 and the inner metal 6 are assembled in a solid phase, and both ends of the solid phase assembly are sealed and vacuumed to form the prefabricated composite blank; after the prefabricated composite blank is completed, execute step S8;

[0082] S4. Determine the spatial corrugation composite interface: determine the spatial corrugation composite interface combination type of the seamless metal composite tube and the structural parameters of the spatial composite interface, wherein the spatial composite interface combination type is sine, cosine, arc, spline curve, triangle, spiral, etc.;

[0083] S5, determine the spatial corrugation composite interface forming process: determine whether the spatial corrugation composite interface is formed by rolling with the conical roller 102 and the conical head 401. If the spatial corrugation composite interface is formed by rolling with the conical roller 102 and the conical head 401, execute step S7; if the spatial corrugation composite interface is not formed by rolling with the conical roller 102 and the conical head 401, execute step S6, that is, when the seamless metal composite pipe has a spatial corrugation composite interface, it is necessary to determine whether the spatial corrugation composite interface is formed between the outer metal 5 and the inner metal 6 when the seamless metal composite blank is prefabricated, or whether the spatial corrugation composite interface is obtained by setting a spatial die on the conical roller 102 and the conical head 401 in the piercing and rolling composite process;

[0084] S6. Determine the prefabricated composite blank of the spatial corrugated composite interface: According to the working environment performance requirements of the target product, determine whether the prefabricated composite blank is assembled in a solid-liquid composite manner. If the prefabricated composite blank is assembled in a solid-liquid composite manner, determine the outer metal 5 or the inner metal 6 as a solid metal; if the outer metal 5 is determined to be solid, set a concave-convex morphology on the inner surface of the outer metal, such as Figure 3 As shown, a groove 51 is provided on the inner surface of the outer metal 5; if the inner metal 6 is determined to be solid, a concave-convex morphology is provided on the outer surface of the inner metal, such as Figure 4As shown, a protrusion 61 is provided on the outer surface of the inner metal 6, and a solid-liquid composite blank is formed by casting to form a prefabricated composite blank; if the prefabricated composite blank is assembled by solid-solid composite assembly, a concave-convex morphology is provided on the inner surface of the outer metal 5, a concave-convex morphology is provided on the outer surface of the inner metal 6, or concave-convex morphologies are provided on the inner surface of the outer metal 5 and the outer surface of the inner metal 6 at the same time, and the outer metal 5 and the inner metal 6 are respectively assembled by solid phase assembly, and both ends of the solid phase assembly are sealed and vacuumed to form a prefabricated composite blank. After the prefabricated composite blank is completed, step S8 is executed;

[0085] S7, determining the assembly method of the spatial corrugated composite interface prefabricated composite blank: judging whether the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method, if the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method, the outer metal or the inner metal is determined to be a solid metal, and the solid-liquid composite assembly is performed by casting to form the prefabricated composite blank; if the assembly method of the prefabricated composite blank adopts the solid-solid composite assembly method, the outer metal and the inner metal are solid-phase packaged, and the two ends of the solid-phase packaged assembly are sealed and vacuumed to form the prefabricated composite blank. After the prefabricated composite blank is completed, step S8 is executed;

[0086] S8, heating the composite blank: heating the prefabricated composite blank at the same temperature or at different temperatures, and waiting for piercing and rolling composite after reaching the target piercing and rolling temperature;

[0087] S9, piercing and rolling compounding: starting the mandrel trolley 403 to drive the conical mandrel 401 to move forward to a preset position along the rolling axis, adjusting the installation positions of the conical roller 102 and the guide device 103 respectively, and performing piercing and rolling compounding on the prefabricated composite billet in the deformed pass formed by the conical roller 102, the guide device 103 and the conical mandrel 401;

[0088] S10, collecting the final product: the prefabricated composite billet is subjected to perforation and rolling to obtain a seamless metal composite pipe, and after cooling and sizing, a seamless metal composite pipe finished product of target size is finally obtained. Figure 5 It is a schematic diagram of the prefabricated composite blank with a spatial composite interface obtained in the present invention.

[0089] The third aspect of the present invention provides a piercing and rolling device for a seamless metal composite pipe piercing and rolling method, such as Figure 6~Figure 10 As shown, it includes a main base unit 1, a main transmission unit 2, a front unit 3 and a back unit 4.

[0090] like Figure 6As shown, the front unit 3, the main machine base unit 1, the main transmission unit 2 and the back unit 4 are arranged in sequence along the rolling axis OX, the front unit 3 is arranged at the entrance end of the main machine base unit 1, the front unit 3 includes a pusher 301, a material receiving trough 302 and a conduit 303, and the pusher 301, the material receiving trough 302 and the conduit 303 are arranged in sequence along the rolling axis.

[0091] like Figure 6 and Figure 7 As shown, the main machine base unit 1 includes a rolling mill frame 101, a tapered roller 102 and a guide device 103. The tapered roller 102 is a tapered structure with a gradually changing diameter, and a plurality of segmented cones are sequentially arranged along the central axis of the tapered roller 102 from the inlet end to the outlet end. The plurality of segmented cones include a biting section 1021, a sizing section 1022 and a diameter expansion section 1023, and an outer arc surface of the tapered roller 102 is provided with an outer space die head 1024. The tapered roller 102 and the guide device 103 are arranged on the rolling mill frame 101 and are evenly distributed circumferentially along the rolling axis to jointly constitute a deformation hole type.

[0092] like Figure 6 As shown, the main transmission unit 2 is arranged on both sides of the backstage unit 4, and the main transmission unit 2 includes a main motor 201, a main reducer 202 and a universal joint 203, the output shaft of the main motor 201 is connected to the input shaft of the main reducer 202, and the output shaft of the main reducer 202 is transmission-connected to the conical roller 102 through the universal joint 203.

[0093] like Figure 6 As shown, the backstage unit 4 is arranged at the outlet end of the main machine base unit 1, and the backstage unit 4 includes a backstage frame 406, a conical plug 401, a push rod 402, a push rod trolley 403 and a plurality of centering machines 404. The conical plug 401 is a conical structure with a gradually changing diameter, and a plurality of segmented cones are sequentially arranged along the central axis of the conical plug 401 from the inlet end to the outlet end. The plurality of segmented cones include a top section 4011, a configuration section 4012, a flattening section 4013, a finishing section 4014 and an exit section 4015, and the busbar of the finishing section 4014 in the conical plug 401 is the same as the busbar of the sizing section 1022 in the conical roller 102. The lines are parallel, the outer arc surface of the conical plug 401 is provided with an inner space die 4016, a plurality of centering machines 404 are evenly arranged at the first end of the backstage frame 406, a push rod trolley 403 is slidably arranged at the second end of the backstage frame 406, a thrust seat 405 is arranged at the front end of the push rod trolley 403, and the first end of the conical plug 401 is connected to the first end of the push rod 402, and the second end of the push rod 402 is connected to the push rod trolley 403, the push rod trolley 403 can drive the conical plug 401 to move along the rolling axis on the backstage frame 406 through the push rod 402, and the conical plug 401 and the push rod 402 can rotate around the rolling axis.

[0094] The prefabricated composite blank is placed in the receiving trough 302, and the pusher 301 sends the prefabricated composite blank along the guide tube 303 into the deformation hole formed by the conical roller 102, the guide device 103 and the conical mandrel 401. The push rod trolley 403 drives the conical mandrel 401 to move forward along the rolling axis through the push rod 402, and piercing and rolling are performed at the center of the prefabricated composite blank to obtain a seamless metal composite pipe.

[0095] like Figure 8 and Fig. 9 As shown, the central axis of the tapered roller 102 OB With rolling axis OX The projection angle on the main vertical plane is the feed angle β , and the angle range of the feed angle is β =0-15°, the central axis of the tapered roller 102 OB With rolling axis OX The projection angle on the main rolling plane is the rolling angle α, and the angle range of the rolling angle is α=0-20°.

[0096] like Fig. 9 As shown, the line segment of the biting segment 1021 in the tapered roller 102 L ZG-1 The angle between the rolling axis OX and the projection on the main rolling plane is the bite angle. α In , the contour line of the expanded diameter section 1023 in the tapered roller 102 L ZG-3 The angle between the projection of the rolling axis OX on the main rolling plane is the expansion angle α Out , bite into the contour line of segment 1021 L ZG-1 and the central axis of the tapered roller 102 OB The angle between is the first angle α 1. The angle range of the first angle is α 1= α + α In , the contour line of the sizing section 1022 L ZG-2 and the central axis of the tapered roller 102 OB The angle between is the second angle α 2, and the angle range of the second angle is α 2= α , the contour line of the expanded diameter section 1023 L ZG-3 and the central axis of the tapered roller 102 OB The angle between them is the third angle α 3. The angle range of the third angle is α 3=α 2- α Out , and the first angle α 1 is greater than the second angle α 2. Second angle α 2 is greater than the third angle α 3.

[0097] like Fig.10 As shown, the contour line of the top section 4011 in the conical head 401 L XB-1 With the center axis of the conical head 401 OA The angle between them is the first head angle, and the contour line of the configuration section 4012 in the conical head 401 L XB-2 With the center axis of the conical head 401 OA The angle between them is the second head angle, and the contour line of the flat section 4013 in the conical head 401 L XB-3 With the center axis of the conical head 401 OA The angle between them is the third plug angle, and the contour line of the finishing section 4014 in the conical plug 401 L XB-4 With the center axis of the conical head 401 OA The angle between them is the fourth head angle, and the profile of the exit section 4015 in the conical head 401 is L XB-5 Line and center axis of conical plug 401 OA The angle between them is the fifth head angle, and the first head angle is greater than the second head angle, the second head angle is greater than the third head angle, the third head angle is greater than the absolute value of the fifth head angle, and the absolute value of the fifth head angle is greater than the fourth head angle.

[0098] like Figure 11~Figure 13 As shown, the spatial structure of the outer space die head 1024 adopts a point structure, a line structure or a ring structure, and the distribution method of the outer space die head 1024 adopts an axial distribution method along the central axis of the conical roller 102 on the outer arc surface of the conical roller 102, a circumferential distribution method around the central axis of the conical roller 102 on the outer arc surface of the conical roller 102, a spiral distribution method on the outer arc surface of the conical roller 102, or a cross distribution method on the outer arc surface of the conical roller 102.

[0099] like Fig.11 As shown, the outer arc surface of the tapered roller 102 is provided with an outer space die head 1024 distributed circumferentially around the central axis of the tapered roller 102 .

[0100] like Fig.12 As shown, the Fig.11Schematic diagram of the seamless metal composite pipe structure that can be obtained when the outer space die head of the middle tapered roller is lower than the sizing section.

[0101] like Fig.13 As shown, the Fig.11 Schematic diagram of the seamless metal composite pipe structure that can be obtained when the outer space die head of the middle tapered roller is higher than the sizing section.

[0102] Fig.12 The present invention adopts Fig.11 Schematic diagram of the structure of the seamless metal composite tube that can be obtained when the outer spatial die of the middle tapered roller is lower than the sizing section. When the height of the outer spatial die is lower than the maximum height of the sizing section, the outer surface concave-convex morphology of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth outer surface and a spatial corrugated composite interface can be obtained.

[0103] Fig.13 The present invention adopts Fig.11 Schematic diagram of the structure of the seamless metal composite tube that can be obtained when the outer space die of the middle tapered roller is higher than the sizing section. When the height of the outer space die is higher than the maximum height of the sizing section, the concave-convex morphology of the outer surface of the seamless metal composite tube cannot be rolled flat, and a seamless metal composite tube with a concave-convex morphology on the outer surface can be obtained.

[0104] like Figure 14~Figure 18 As shown, the spatial structure of the inner space die 4016 adopts a point structure, a line structure or a ring structure, and the distribution mode of the inner space die 4016 adopts an axial distribution mode along the central axis of the conical head 401 on the outer arc surface of the conical head 401, a circumferential distribution mode around the central axis of the conical head 401 on the outer arc surface of the conical head 401, a spiral distribution mode on the outer arc surface of the conical head 401, or a cross distribution mode on the outer arc surface of the conical head 401.

[0105] like Fig.14 As shown, the outer arc surface of the conical head 401 is provided with a dot-shaped protruding inner space die 4016.

[0106] like Fig.15 As shown, the Fig.14 Schematic diagram of the structure of the seamless metal composite tube that can be obtained when the inner space die 4016 of the middle conical head 401 is lower than the flattening section 4013. Because the inner space die 4016 is lower than the flattening section 4013, a spiral corrugation is first formed on the inner surface of the seamless metal composite tube blank during the piercing and rolling process. However, as the seamless metal composite tube blank moves forward, after passing through the flattening section 4013 and the finishing section 4014, the spiral corrugation on the inner surface is flattened, but a spiral space composite interface is formed, which significantly increases the composite interface bonding area and bonding strength of the seamless metal composite tube.

[0107] like Fig.16 As shown, the Fig.14 Schematic diagram of the structure of a seamless metal composite tube that can be obtained when the inner space die 4016 of the middle conical head 401 is higher than the flattening section 4013. Because the inner space die 4016 is higher than the flattening section 4013, a spiral corrugation is first formed on the inner surface of the seamless metal composite tube billet during the piercing and rolling process. However, as the seamless metal composite tube billet moves forward, after passing through the flattening section 4013 and the finishing section 4014, the spiral corrugation on the inner surface cannot be flattened. The seamless metal composite tube with the spiral corrugation on the inner surface can significantly increase the specific area of ​​the inner surface of the seamless metal composite tube, increase the contact area with the fluid, improve the fluid flow state, and can be used in heat exchange pipelines.

[0108] like Fig.17 As shown, the outer arc surface of the conical head 401 is axially distributed with three dot-shaped protruding inner space dies 4016 along the central axis of the conical head 401. The sizes of the three inner space dies 4016 can be changed, and the positions and spacings can be different.

[0109] like Fig.18 As shown, the Fig.17 Schematic diagram of the seamless metal composite tube structure that can be obtained by the middle conical head 401. By adjusting the size, shape, spacing and other arrangements of the three inner space dies 4016, a seamless metal composite tube with a spatial composite interface with a corresponding distribution pattern can be obtained. At this time, due to the increase in the number of corrugations, the connection function of the corrugations in the seamless metal composite tube is highlighted, and a mechanical locking similar to a bolt connection is formed between the inner and outer tubes, thereby increasing the interface bonding strength of the seamless metal composite tube.

[0110] The equipment of the present invention has a simple and reliable structure and a long service life. Under the condition that the structures of the tapered roller and the tapered plug are not changed, a segmented gradual change treatment is performed. The tapered roller includes a bite section, a sizing section, and a diameter expansion section. The tapered plug includes a top section, a configuration section, a flattening section, a finishing section, and an exit section. Through the gradual segmented treatment, the metal flow law is improved, and the wear and tear of the tapered plug is reduced, thereby increasing the service life of the equipment and improving the size accuracy and shape accuracy of the seamless metal composite tube blank after piercing and rolling. At the same time, it can flexibly assemble the blanks to improve the forming efficiency. The inner surface of the solid outer metal or the outer surface of the solid inner metal can be processed with grooves or protrusions, and filled with liquid inner metal or liquid outer metal. This can avoid the high requirements of coaxiality, cylindricity, cleanliness and other matching requirements of traditional solid-solid composite blanks. The high temperature of the solid-liquid interface promotes the diffusion of interface elements and realizes metallurgical bonding, which can significantly improve the forming efficiency. The mutual meshing effect of the spatial composite interface can significantly improve the coordinated deformation ability. The seamless metal composite blank obtained after the inner metal solidifies is still in a high temperature state and directly enters the heating furnace for heating, which can significantly reduce energy consumption. In addition, the contact area can be increased and the interface bonding can be strengthened. The inner space die of the configuration section of the conical head can form an internal surface concave-convex morphology on the seamless metal composite blank, and then it is rolled flat in the flattening section to obtain a smooth internal surface morphology. Finally, the target size is obtained through the finishing section, but there is a macroscopic or microscopic spatial composite interface between the component metals, which can significantly increase the bonding area and enhance the bonding strength. In addition, when the height of the inner space die is higher than the flattening section, the internal surface concave-convex morphology cannot be rolled flat in the flattening section, so the internal surface concave-convex morphology is retained to obtain a seamless metal composite tube with an internal surface concave-convex morphology. Similarly, the outer space die of the bite section of the tapered roller can form an external surface concave-convex morphology on the seamless metal composite blank, which is then rolled flat in the sizing section to obtain a smooth external surface morphology, and finally the target size is obtained through the expansion section. However, there is a macroscopic or microscopic spatial composite interface between the component metals, which can significantly increase the bonding area and enhance the bonding strength. In addition, when the height of the outer space die is higher than the sizing section, the external surface concave-convex morphology cannot be rolled flat in the sizing section, so the external surface concave-convex morphology is retained to obtain a seamless metal composite tube with an external surface concave-convex morphology. Finally, efficient forming and customized interface structure can be achieved, the tapered roller and the tapered head are integrated, and a segmented cone with a gradually changing diameter is sequentially set from the inlet side to the outlet side along the rolling axis. The forming process of the concave-convex surface and the rolling process are highly concentrated. The composite interface space structure customization can be achieved by adjusting the shape, size, distribution, position and other rules of the space die, and a variety of structural products such as spiral and cross-shaped spatial composite interfaces, as well as external surface corrugations and internal surface corrugations can be obtained.

[0111] The embodiments described above are only descriptions of the preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for perforating and rolling a seamless metal composite pipe, It is characterized in that It includes the following steps: S1. Determine the component metal: Determine the component metal information of the seamless metal composite pipe according to the working environment performance requirements of the target product; S2. Determine the composite interface type: According to the working environment load requirements of the target product, the composite interface of the seamless metal composite pipe adopts a spatial corrugated composite interface; S3. Determine the spatial corrugation composite interface: determine the combination type of the spatial corrugation composite interface of the seamless metal composite pipe and the structural parameters of the spatial corrugation composite interface; S4. Determine the process for forming a spatial corrugated composite interface: the conical roller and the conical mandrel form a spatial corrugated composite interface; S5. Determine the assembly method of the spatial corrugated composite interface prefabricated composite blank: determine whether the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method. If the assembly method of the prefabricated composite blank adopts the solid-liquid composite assembly method, the outer metal or the inner metal is determined to be a solid metal, and solid-liquid composite assembly is performed by casting to form the prefabricated composite blank; if the assembly method of the prefabricated composite blank adopts the solid-solid composite assembly method, the outer metal and the inner metal are solid-phase packaged, and both ends of the solid-phase packaged package are sealed and vacuumed to form the prefabricated composite blank; S6, heating the prefabricated composite blank: heating the prefabricated composite blank at the same temperature or at different temperatures, and waiting for piercing and rolling compounding after reaching the target piercing and rolling temperature; S7, determining the spatial die: according to the determined spatial corrugation composite interface, an outer spatial die is arranged on the conical roller, an inner spatial die is arranged on the conical mandrel, or an outer spatial die and an inner spatial die are arranged on the conical roller and the conical mandrel respectively at the same time; S8. Determine the deformed pass: determine the size of the seamless metal composite pipe according to the target size specification, start the push rod trolley to drive the conical mandrel to move forward along the rolling axis to a preset position, and adjust the installation positions of the conical roller and the guide device respectively, so that the conical roller, the guide device and the conical mandrel together form a deformed pass; S9, conveying the prefabricated composite blank: conveying the prefabricated composite blank along the guide tube into the deformed hole formed by the tapered roller, the guide device and the tapered head through the pusher; S10, piercing and rolling composite: under the combined action of the internal piercing of the conical head, the edge guiding of the guide device and the external rolling of the conical roller, the wall thickness of the prefabricated composite billet is thinned and axially extended to obtain a seamless metal composite pipe with a spatial corrugated composite interface; S11. Collecting final products: The prefabricated composite billet is subjected to perforation, rolling and composite to obtain a seamless metal composite pipe, and after cooling and sizing, a seamless metal composite pipe finished product of target size is finally obtained; The outer space die is arranged at the biting section or the sizing section of the tapered roller, and can form a concave-convex shape on the outer surface of the seamless metal composite pipe. When the height of the outer space die is higher than the maximum height of the sizing section, a seamless metal composite pipe with a concave-convex shape on the outer surface can be obtained. When the height of the outer space die is lower than the maximum height of the sizing section, the concave-convex shape on the outer surface of the seamless metal composite pipe can be rolled flat, and a seamless metal composite pipe with a smooth outer surface and a spatial corrugated composite interface can be obtained. The inner space die is arranged at the configuration section or the flat section of the conical top head to form a concave-convex morphology on the inner surface of the seamless metal composite tube. When the height of the inner space die is higher than the maximum height of the flat section, a seamless metal composite tube with a concave-convex morphology on the inner surface can be obtained. When the height of the inner space die is lower than the maximum height of the flat section, the concave-convex morphology on the inner surface of the seamless metal composite tube can be rolled flat, and a seamless metal composite tube with a smooth inner surface but a spatial corrugated composite interface can be obtained.

2. A piercing and rolling device for the piercing and rolling method for seamless metal composite pipes according to claim 1, It is characterized in that It includes a main base unit, a main transmission unit, a front unit and a back unit. The front unit, the main machine base unit, the main transmission unit and the back unit are arranged in sequence along the rolling axis. The front unit is arranged at the entrance end of the main machine base unit. The front unit includes a pusher, a material receiving trough and a guide tube, and the pusher, the material receiving trough and the guide tube are arranged in sequence along the rolling axis. The main machine base unit includes a rolling mill frame, a tapered roller and a guide device. The tapered roller is a tapered structure with a gradually changing diameter, and a plurality of segmented cones are sequentially arranged along the central axis of the tapered roller from the inlet end to the outlet end. The plurality of segmented cones include a biting section, a sizing section and a diameter expansion section. An outer space die head is arranged on the outer arc surface of the tapered roller. The tapered roller and the guide device are arranged on the rolling mill frame and are evenly arranged along the circumferential direction of the rolling axis. The tapered roller, the guide device and the tapered head together constitute a deformation pass type. The main transmission unit is arranged on both sides of the backstage unit, and the main transmission unit includes a main motor, a main reducer and a universal joint shaft. The output shaft of the main motor is connected to the input shaft of the main reducer, and the output shaft of the main reducer is connected to the tapered roller through the universal joint shaft. The backstage unit is arranged at the outlet end of the main machine base unit, and the backstage unit includes a backstage frame, a conical plug, a push rod, a push rod trolley and a plurality of centering machines. The conical plug is a conical structure with a gradually changing diameter, and a plurality of segmented cones are arranged in sequence from the inlet end to the outlet end along the central axis of the conical plug. The plurality of segmented cones include a top section, a configuration section, a flattening section, a finishing section and an exit section, and the generatrix of the finishing section in the conical plug is parallel to the generatrix of the sizing section in the conical roller. The outer arc surface of the conical plug is provided with an inner space die head, and the plurality of centering machines are arranged at the first end of the backstage frame. The push rod trolley is slidably arranged at the second end of the backstage frame, and the first end of the conical plug is connected to the first end of the push rod, and the second end of the push rod is connected to the push rod trolley. The push rod trolley can drive the conical plug to move along the rolling axis on the backstage frame through the push rod, and the conical plug and the push rod can rotate around the rolling axis. The prefabricated composite blank is placed in the receiving trough, and the pusher sends the prefabricated composite blank along the guide tube into the deformation hole formed by the conical roller, the guide device and the conical plug. The ejector trolley drives the conical plug to move forward along the rolling axis through the ejector, and performs piercing and rolling at the center of the prefabricated composite blank to obtain a seamless metal composite pipe. The angle between the projection of the tapered roller axis and the rolling axis on the main vertical plane is the feed angle. β , and the input angle β The angle range is 0-15°, the projection angle between the axis of the tapered roller and the rolling axis on the main rolling plane is the rolling angle α, and the angle range of the rolling angle α is 0-20°; The angle between the generatrix of the biting section of the tapered roller and the projection of the rolling axis on the main rolling plane is the biting angle. α In The angle between the generatrix of the expansion section of the tapered roller and the projection of the rolling axis on the main rolling plane is the expansion angle α Out , and the angle between the generatrix of the biting section and the central axis of the tapered roller is the first angle α 1 ,and α 1 = α + α In The angle between the generatrix of the sizing section and the center axis of the tapered roller is the second angle α 2 ,and α 2 = α The angle between the generatrix of the expansion section and the center axis of the tapered roller is the third angle α 3 , α 3 = α 2 - α Out , and the first angle α 1 Greater than the second angle α 2 , the second angle α 2 Greater than the third angle α 3 .

3. The piercing and rolling equipment according to claim 2, It is characterized in that The spatial structure of the outer space die head adopts a point structure, a linear structure or a ring structure, and the distribution method of the outer space die head adopts an axial distribution method along the central axis of the tapered roller on the outer arc surface of the tapered roller, a circumferential distribution method around the central axis of the tapered roller on the outer arc surface of the tapered roller, a spiral distribution method on the outer arc surface of the tapered roller, or a cross distribution method on the outer arc surface of the tapered roller.

4. The piercing and rolling equipment according to claim 2, It is characterized in that The angle between the generatrix of the top section in the conical plug and the central axis of the conical plug is the first plug angle, the angle between the generatrix of the configuration section in the conical plug and the central axis of the conical plug is the second plug angle, the angle between the generatrix of the flat section in the conical plug and the central axis of the conical plug is the third plug angle, the angle between the generatrix of the finishing section in the conical plug and the central axis of the conical plug is the fourth plug angle, the angle between the generatrix of the exit section in the conical plug and the central axis of the conical plug is the fifth plug angle, and the first plug angle is greater than the second plug angle, the second plug angle is greater than the third plug angle, the third plug angle is greater than the absolute value of the fifth plug angle, and the absolute value of the fifth plug angle is greater than the fourth plug angle.

5. The piercing and rolling equipment according to claim 2, It is characterized in that The spatial structure of the inner space die head adopts a point structure, a linear structure or a ring structure, and the distribution mode of the inner space die head adopts an axial distribution mode along the central axis of the conical plug on the outer arc surface of the conical plug, a circumferential distribution mode around the central axis of the conical plug on the outer arc surface of the conical plug, a spiral distribution mode on the outer arc surface of the conical plug, or a cross distribution mode on the outer arc surface of the conical plug.