A polypropylene pearlescent film and its preparation method and application in composite express bags

By adding a special flame retardant to the polypropylene pearlescent film, its flame retardant performance is improved, which solves the problem of insufficient flame retardant performance of the existing polypropylene pearlescent film in composite express bags and achieves excellent flame retardant effects.

CN118544660BActive Publication Date: 2024-10-01烟台富利新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411021414.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing polypropylene pearlescent film has poor flame retardant properties in composite express bags and is difficult to meet application needs.

Method used

A multi-layer structure polypropylene pearlescent film composed of polypropylene, organic pearlescent masterbatch, titanium dioxide, calcium carbonate, flame retardant, antistatic agent and lignin is used to prepare a new type of pearlescent film through specific raw material ratio and process treatment. Flame retardants are added to polypropylene to improve flame retardant properties.

Benefits of technology

Significantly improves the flame retardant level of polypropylene pearlescent film. By containing a large number of nitrogen-containing groups and phosphate groups in the polymer main chain and graft structure, the gas phase and condensed phase flame retardant mechanisms are realized, achieving excellent flame retardant properties. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention discloses a polypropylene pearlescent film and a preparation method thereof and an application in a composite express bag, and belongs to the technical field of polypropylene pearlescent film. The polypropylene pearlescent film is composed of an outer layer, an intermediate layer and an inner layer, and the outer layer is composed of the following raw materials in parts by weight: polypropylene: 40-50 parts, organic pearlescent masterbatch 8-15 parts, titanium dioxide: 1-2 parts, calcium carbonate: 2-4 parts, flame retardant 3-5 parts, antistatic agent 2-3 parts, lignin 30-40 parts; the intermediate layer is composed of the following raw materials in parts by weight: polypropylene: 30-40 parts, titanium dioxide: 1-2 parts, lignin 10-20 parts; the raw materials and parts of the inner layer are the same as those of the outer layer. The present invention improves the flame retardant grade of the polypropylene pearlescent film by adding a prepared polymer flame retardant to polypropylene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polypropylene pearlescent films, and in particular to a polypropylene pearlescent film and a preparation method thereof and application thereof in composite express bags. Background Art

[0002] Polypropylene pearlescent film has many advantages, such as low carbon and environmental protection, low specific gravity, high strength, good weather resistance, good tear resistance, soft texture, excellent printing performance and durability. Polypropylene pearlescent film has been widely used in printing, packaging bags and other fields because it has the characteristics of both plastic and paper. With the increase in the application scenarios of polypropylene pearlescent film, more requirements are put forward for polypropylene pearlescent film. For example, when polypropylene pearlescent film is used in the field of composite express bags, it is required to have excellent flame retardant properties.

[0003] The Chinese invention patent application with publication number CN116574329A discloses a process for preparing a stretch-resistant polypropylene packaging film. The packaging film disclosed in the patent application has excellent tensile properties, but its flame retardant properties are relatively poor. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a polypropylene pearlescent film and a preparation method thereof and application in composite express bags.

[0005] To achieve the above object, the present invention is implemented through the following technical solutions:

[0006] A polypropylene pearlescent film, consisting of an outer layer, an intermediate layer and an inner layer, wherein the outer layer is composed of the following raw materials in parts by weight: polypropylene: 40-50 parts, organic pearlescent masterbatch: 8-15 parts, titanium dioxide: 1-2 parts, calcium carbonate: 2-4 parts, flame retardant: 3-5 parts, antistatic agent: 2-3 parts, lignin: 30-40 parts;

[0007] The middle layer is composed of the following raw materials in parts by weight: polypropylene: 30-40 parts, titanium dioxide: 1-2 parts, lignin: 10-20 parts;

[0008] The raw materials and the number of the inner surface layer are the same as those of the outer surface layer.

[0009] The flame retardant is prepared by the following method:

[0010] S1: Deionized water, urotropine, p-aminophenol and glacial acetic acid are added to the reactor in sequence, stirred and dissolved, heated to 65-70°C, reacted for 2-3h, cooled to room temperature to separate layers, removed the water layer, washed with deionized water 3 times, and obtained a condensation polymer; the reaction equation is as follows:

[0011] S2: Tetrahydrofuran, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and triethylamine are added to the reactor in sequence, stirred and mixed evenly, and then a tetrahydrofuran solution of diphenylphosphinyl chloride is added dropwise. After the addition is completed, the temperature is raised to 75-85° C. and reacted for 13-16 hours. After post-treatment, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate is obtained; the reaction equation is shown as follows:

[0012]

[0013] S3: Add DMF to the reactor, stir, raise the temperature to 95-105°C, add polycondensate, glycidyl methacrylate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, catalyst C-94, 1-butyl-3-methylimidazolium methane sulfonate ionic liquid in sequence, react for 3-4 hours under nitrogen protection, cool to room temperature, add deionized water and stir evenly, obtain a polymer filter cake after centrifugal filtration, wash with anhydrous ethanol and deionized water, and vacuum dry at 50-60°C to obtain a flame retardant; the reaction equation is as follows:

[0014]

[0015] Among them, m=o+p+q.

[0016] In step S1, the mass ratio of deionized water, hexamethylenetetramine, p-aminophenol and glacial acetic acid is 10:2.5:(1.0-1.2):(0.8-1.0).

[0017] In step S2, the mass ratio of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol, triethylamine and diphenylphosphine chloride is 10:(4.8-6):(15-20).

[0018] In step S3, the feed mass ratio of the condensation polymer, glycidyl methacrylate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, catalyst C-94, and 1-butyl-3-methylimidazolium methane sulfonate ionic liquid is 10:(4-5):(16-20):(0.2-0.4):(0.2-0.3).

[0019] The concentration of the tetrahydrofuran solution of diphenylphosphinic chloride is 20-30 wt %.

[0020] The antistatic agent is one of Armostat 400 antistatic agent and Armostat 1800 antistatic agent.

[0021] The present invention also provides a method for preparing a polypropylene pearlescent film, comprising the following steps:

[0022] S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively;

[0023] S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming;

[0024] Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

[0025] Furthermore, the polypropylene pearlescent film can be used in the field of composite express bags.

[0026] Due to the adoption of the above technical solution, the beneficial effects of the present invention include:

[0027] (1) The present invention prepares the intermediate 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate used as a flame retardant by reacting diphenylphosphine chloride with 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol under the action of an acid-binding agent, triethylamine; and then prepares a new flame retardant by graft copolymerization of a condensation product of urotropine-p-aminophenol with 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate and glycidyl methacrylate.

[0028] (2) The present invention improves the flame retardancy of the polypropylene pearlescent film by adding a flame retardant to the polypropylene. The reason for improving the flame retardancy is that: the main chain contains a large number of N-containing groups, and the grafted 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate also provides a large number of N-containing groups, which will pyrolyze when heated to produce non-flammable nitrogen-containing inert gas, which can dilute the concentration of combustible gas in the gas phase, thereby achieving the purpose of strengthening the gas phase flame retardancy mechanism; the grafted 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate contains phosphoric acid groups, which exhibit condensed phase flame retardancy when phosphorus is in a higher oxidation state (+3, +5), and exhibit gas phase flame retardancy when phosphorus is in a lower oxidation state (0, +1). DETAILED DESCRIPTION

[0029] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.

[0030] Example 1 Preparation of flame retardant

[0031] S1: 1000 g of deionized water, 250 g of urotropine, 100 g of p-aminophenol, and 80 g of glacial acetic acid were added to the reactor in sequence, stirred and dissolved, heated to 65°C, reacted for 3 h, cooled to room temperature to separate the layers, removed the water layer, and washed with deionized water for 3 times (using 180 g of deionized water each time) to obtain a polycondensate;

[0032] S2: 300g of tetrahydrofuran, 100g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and 48g of triethylamine were added to the reactor in sequence, stirred and mixed evenly, and then a tetrahydrofuran solution of diphenylphosphinyl chloride (15g of diphenylphosphinyl chloride was dissolved in 60g of tetrahydrofuran) was added dropwise. After the addition was completed, the temperature was raised to 75°C and reacted for 16h; filtered to remove insoluble salts; evaporated at 55°C to obtain a crude product, which was dissolved in 250g of dichloromethane and washed 3 times with deionized water (100g of deionized water was used each time), the organic phase was separated and separated, and evaporated at 55°C to obtain 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate;

[0033] S3: Add 450g of DMF to the reactor, stir, raise the temperature to 95°C, add 100g of condensation polymer, 40g of glycidyl methacrylate, 160g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, 2g of catalyst C-94, and 2g of 1-butyl-3-methylimidazolium methane sulfonate ionic liquid in sequence, react for 4h under nitrogen protection, cool to room temperature, add 500g of deionized water and stir evenly, obtain a polymer filter cake after centrifugal filtration, wash with 100g of anhydrous ethanol and then with 100g of deionized water, and dry in vacuo at 50°C for 10h to obtain a flame retardant.

[0034] Its nuclear magnetic hydrogen spectrum data is: 1 H NMR (300 MHz, DMSO- d 6) δ 8.57 (s, 1H), 7.87 – 7.72 (m, 6H), 7.72 – 7.61 (m, 3H), 7.55 – 7.44 (m, 6H), 7.14 – 7.02 (m, 5H), 7.00– 6.90 (m, 2H), 6.87 – 6.77 (m, 4H), 6.77 – 6.68 (m, 2H), 4.81 (d, J = 12.3Hz, 1H), 4.75 (d,J = 1.1 Hz, 2H), 4.64 (d, J = 12.5 Hz, 1H), 4.32 – 4.02 (m,6H), 3.72 – 3.56 (m, 2H), 3.45 (qd, J = 8.0, 1.6 Hz, 2H), 3.35 – 3.20 (m,1H), 2.82 (h, J = 6.9 Hz, 1H), 2.68 (ddd, J = 7.6, 6.5, 1.1 Hz, 2H), 2.31 (d, J = 0.6 Hz, 3H), 2.01 (pd, J = 7.1, 0.8 Hz, 2H), 1.28 – 1.16 (m, 3H).

[0035] Example 2 Preparation of flame retardant

[0036] S1: 1000 g of deionized water, 250 g of urotropine, 110 g of p-aminophenol, and 90 g of glacial acetic acid were added to the reactor in sequence, stirred and dissolved, heated to 70°C, reacted for 2 h, cooled to room temperature to separate the layers, removed the water layer, and washed with deionized water for 3 times (using 180 g of deionized water each time) to obtain a polycondensate;

[0037] S2: 300g of tetrahydrofuran, 100g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and 54g of triethylamine were added to the reactor in sequence, stirred and mixed evenly, and then a tetrahydrofuran solution of diphenylphosphinyl chloride (18g of diphenylphosphinyl chloride was dissolved in 55g of tetrahydrofuran) was added dropwise. After the addition was completed, the temperature was raised to 80°C and reacted for 15h; filtered to remove insoluble salts; evaporated at 55°C to obtain a crude product, which was dissolved in 250g of dichloromethane and washed 3 times with deionized water (100g of deionized water was used each time), the organic phase was separated and separated, and evaporated at 55°C to obtain 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate;

[0038] S3: Add 450g of DMF to the reactor, stir, raise the temperature to 100°C, add 100g of condensation polymer, 45g of glycidyl methacrylate, 180g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, 3g of catalyst C-94, and 2.5g of 1-butyl-3-methylimidazolium methane sulfonate ionic liquid in sequence, react for 3.5h under nitrogen protection, cool to room temperature, add 500g of deionized water and stir evenly, obtain a polymer filter cake after centrifugal filtration, wash with 100g of anhydrous ethanol and then with 100g of deionized water, and dry in vacuo at 55°C for 9h to obtain a flame retardant.

[0039] Example 3 Preparation of flame retardant

[0040] S1: 1000 g of deionized water, 250 g of urotropine, 120 g of p-aminophenol, and 100 g of glacial acetic acid were added to the reactor in sequence, stirred and dissolved, heated to 70°C, reacted for 2.5 h, cooled to room temperature to separate the layers, removed the water layer, and washed with deionized water for 3 times (180 g of deionized water was used each time) to obtain a polycondensate;

[0041] S2: 300g of tetrahydrofuran, 100g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and 60g of triethylamine were added to the reactor in sequence, stirred and mixed evenly, and then a tetrahydrofuran solution of diphenylphosphinyl chloride (20g of diphenylphosphinyl chloride was dissolved in 45g of tetrahydrofuran) was added dropwise. After the addition was completed, the temperature was raised to 85°C and reacted for 13h; filtered to remove insoluble salts; evaporated at 55°C to obtain a crude product, which was dissolved in 250g of dichloromethane and washed 3 times with deionized water (100g of deionized water was used each time), the organic phase was separated and separated, and evaporated at 55°C to obtain 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate;

[0042] S3: Add 450g of DMF to the reactor, stir, raise the temperature to 105°C, add 100g of condensation polymer, 50g of glycidyl methacrylate, 200g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, 4g of catalyst C-94, and 3g of 1-butyl-3-methylimidazolium methane sulfonate ionic liquid in sequence, react for 3h under nitrogen protection, cool to room temperature, add 500g of deionized water and stir evenly, obtain a polymer filter cake after centrifugal filtration, wash with 100g of anhydrous ethanol and then with 100g of deionized water, and dry in vacuo at 60°C for 8h to obtain a flame retardant.

[0043] Example 4

[0044] A polypropylene pearlescent film has a thickness of 0.16 mm, wherein the thicknesses of the outer layer and the inner layer are both 0.05 mm, and the thickness of the middle layer is 0.06 mm; the raw material composition of the outer layer is: polypropylene: 400 g, organic pearlescent masterbatch 80 g, titanium dioxide: 10 g, calcium carbonate: 20 g, flame retardant (prepared in Example 1) 30 g, antistatic agent (Armostat 400 antistatic agent) 20 g, lignin 300 g; the raw material composition of the middle layer is: polypropylene: 300 g, titanium dioxide: 10 g, lignin 100 g; the raw materials and proportions of the inner layer are the same as those of the outer layer.

[0045] Example 5

[0046] A polypropylene pearlescent film has a thickness of 0.16 mm, wherein the thicknesses of the outer layer and the inner layer are both 0.05 mm, and the thickness of the middle layer is 0.06 mm; the raw material composition of the outer layer is: polypropylene: 450 g, organic pearlescent masterbatch 120 g, titanium dioxide: 15 g, calcium carbonate: 30 g, flame retardant (prepared in Example 2) 40 g, antistatic agent (Armostat 1800 antistatic agent) 25 g, lignin 350 g; the raw material composition of the middle layer is: polypropylene: 350 g, titanium dioxide: 15 g, lignin 150 g; the raw materials and proportions of the inner layer are the same as those of the outer layer.

[0047] Example 6

[0048] A polypropylene pearlescent film has a thickness of 0.16 mm, wherein the thicknesses of the outer layer and the inner layer are both 0.05 mm, and the thickness of the middle layer is 0.06 mm; the raw material composition of the outer layer is: 500 g of polypropylene, 150 g of organic pearlescent masterbatch, 20 g of titanium dioxide, 40 g of calcium carbonate, 50 g of flame retardant (prepared in Example 3), 30 g of antistatic agent (Armostat 400 antistatic agent), and 400 g of lignin; the raw material composition of the middle layer is: 400 g of polypropylene, 20 g of titanium dioxide, and 200 g of lignin; the raw materials and proportions of the inner layer are the same as those of the outer layer.

[0049] Comparative Example 1

[0050] A polypropylene pearlescent film is substantially the same as Example 5, except that no flame retardant is added to the outer surface layer and the inner surface layer.

[0051] Comparative Example 2

[0052] A polypropylene pearlescent film is basically the same as Example 5, except that the flame retardant added to the outer layer and the inner layer is replaced by an equal weight of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate prepared in step S2 of Example 2.

[0053] Comparative Example 3

[0054] A polypropylene pearlescent film is substantially the same as Example 5, except that the flame retardant added to the outer layer and the inner layer is replaced by an equal weight of 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide (CAS No.: 99208-50-1).

[0055] Comparative Example 4

[0056] A polypropylene pearlescent film is substantially the same as Example 5, except that the flame retardant added to the outer layer and the inner layer is replaced by a flame retardant prepared by the following method:

[0057] S1: 1000 g of deionized water, 250 g of urotropine, 110 g of p-aminophenol, and 90 g of glacial acetic acid were added to the reactor in sequence, stirred and dissolved, heated to 70°C, reacted for 2 h, cooled to room temperature to separate the layers, removed the water layer, and washed with deionized water for 3 times (using 180 g of deionized water each time) to obtain a polycondensate;

[0058] S2: 300g of tetrahydrofuran, 100g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and 54g of triethylamine were added to the reactor in sequence, stirred and mixed evenly, and then a tetrahydrofuran solution of diphenylphosphinyl chloride (18g of diphenylphosphinyl chloride was dissolved in 55g of tetrahydrofuran) was added dropwise. After the addition was completed, the temperature was raised to 80°C and reacted for 15h; filtered to remove insoluble salts; evaporated at 55°C to obtain a crude product, which was dissolved in 250g of dichloromethane and washed 3 times with deionized water (100g of deionized water was used each time), the organic phase was separated and separated, and evaporated at 55°C to obtain 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate;

[0059] S3: Add 450g of DMF to the reactor, stir, raise the temperature to 100°C, add 100g of condensation polymer, 180g of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, 3g of catalyst C-94, and 2.5g of 1-butyl-3-methylimidazolium methane sulfonate ionic liquid in sequence, react for 3.5h under nitrogen protection, cool to room temperature, add 500g of deionized water and stir evenly, obtain a polymer filter cake after centrifugal filtration, wash with 100g of anhydrous ethanol and then with 100g of deionized water, and dry in vacuo at 55°C for 9h to obtain a flame retardant.

[0060] Comparative Example 5

[0061] A polypropylene pearlescent film is prepared by using the raw materials and method of Example 3 of Chinese patent CN116574329A.

[0062] The brand of titanium dioxide used in the examples and comparative examples of the present application is DuPont R-706, the brand of calcium carbonate is KJ-106, the polypropylene is homopolymer polypropylene CJS-700 produced by Sinopec, the organic pearlescent masterbatch is ZG905 produced by Foshan Suxing Masterbatch Co., Ltd., and the lignin is guaiac-based lignin.

[0063] The polypropylene pearlescent films of Examples 4-6 and Comparative Examples 1-4 of the present application were prepared by the following process:

[0064] S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively;

[0065] S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming;

[0066] Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

[0067] The polypropylene pearlescent films prepared in Examples 4-6 and Comparative Examples 1-5 were subjected to a vertical combustion (UL-94) test. According to the ASTM D3801 standard, the vertical combustion rating of the samples was evaluated using a CZF-3 instrument. The sample size was 130×13×3.2 mm. 3 (Its thickness is achieved by stacking the number of pearlescent film layers). The test results are shown in Table 1.

[0068] The polypropylene pearlescent films prepared in Examples 4-6 of the present application and Comparative Examples 1-5 were subjected to tensile strength tests according to the method of GB13002-91. The test results are shown in Table 1.

[0069] Table 1

[0070]

[0071] It can be seen from the data of Examples 4, 5 and 6 in Table 1 that the polypropylene pearlescent film prepared by the present invention has excellent transverse and longitudinal mechanical properties, with a transverse tensile strength higher than 95 MPa and a longitudinal tensile strength higher than 85 MPa; and the flammability rating (UL-94) is V-0.

[0072] Comparative Example 1 is a comparison without adding flame retardant, and its flame retardant grade is V-2. Comparative Examples 2-3 are comparative examples in which the flame retardants are replaced with 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate and 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, respectively, and their flame retardant grades are V-1; the flame retardant added in Comparative Example 4 does not contain methacrylate glycidyl ester groups, and its flame retardant grade is V-1. It can be seen from Table 1 that the tensile strength of Comparative Examples 2-4 is lower than that of Examples 4-6. The reason is that the flame retardant does not contain methacrylate glycidyl ester groups, and the mixed compatibility of the flame retardant in polypropylene is relatively low, resulting in a decrease in the tensile strength of polypropylene synthetic paper.

[0073] Comparative Example 5 is a synthetic paper prepared using the raw materials and proportions of Example 3 of the Chinese invention patent with publication number CN116574329A, and its flammability rating (UL-94) is V-2.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A polypropylene pearlescent film, consisting of an outer layer, an intermediate layer and an inner layer, It is characterized in that The outer layer is composed of the following raw materials in parts by weight: polypropylene: 40-50 parts, organic pearlescent masterbatch: 8-15 parts, titanium dioxide: 1-2 parts, calcium carbonate: 2-4 parts, flame retardant: 3-5 parts, antistatic agent: 2-3 parts, lignin: 30-40 parts; The middle layer is composed of the following raw materials in parts by weight: polypropylene: 30-40 parts, titanium dioxide: 1-2 parts, lignin: 10-20 parts; The raw materials and the number of portions of the inner surface layer are the same as those of the outer surface layer; The flame retardant is prepared by the following method: S1: Deionized water, hexamethylenetetramine, p-aminophenol and glacial acetic acid are added to the reactor in sequence, stirred and dissolved, heated to 65-70°C, reacted for 2-3h, cooled to room temperature to separate layers, removed the water layer, and washed with deionized water for 3 times to obtain a polycondensate; S2: Tetrahydrofuran, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol and triethylamine are added to the reactor in sequence, stirred and mixed, and then a tetrahydrofuran solution of diphenylphosphinyl chloride is added dropwise. After the addition is completed, the temperature is raised to 75-85° C. for reaction for 13-16 hours, and post-treated to obtain 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate; S3: Add DMF to the reactor, stir, raise the temperature to 95-105°C, add polycondensate, glycidyl methacrylate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, catalyst C-94, 1-butyl-3-methylimidazolium methane sulfonate ionic liquid in sequence, react for 3-4 hours under nitrogen protection, cool to room temperature, add deionized water and stir evenly, obtain a polymer filter cake after centrifugal filtration, wash with anhydrous ethanol and deionized water, and vacuum dry at 50-60°C to obtain a flame retardant; In step S1, the mass ratio of deionized water, hexamethylenetetramine, p-aminophenol and glacial acetic acid is 10:2.5:(1.0-1.2):(0.8-1.0); In step S2, the mass ratio of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol, triethylamine and diphenylphosphine chloride is 10:(4.8-6):(15-20); In step S3, the feed mass ratio of the condensation polymer, glycidyl methacrylate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenyl diphenylphosphonate, catalyst C-94, and 1-butyl-3-methylimidazolium methane sulfonate ionic liquid is 10:(4-5):(16-20):(0.2-0.4):(0.2-0.3).

2. A polypropylene pearlescent film according to claim 1, It is characterized in that The concentration of the tetrahydrofuran solution of diphenylphosphine chloride is 20-30 wt %.

3. A polypropylene pearlescent film according to claim 1, It is characterized in that The antistatic agent is one of Armostat 400 antistatic agent and Armostat 1800 antistatic agent.

4. A method for preparing the polypropylene pearlescent film according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively; S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming; Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

5. Use of the polypropylene pearlescent film according to any one of claims 1 to 3 in composite express bags.