A high thermal conductivity and high purity spherical magnesium oxide precursor and preparation method thereof

By using soluble hydrated magnesium ion salts, magnesium ion surfactants and reaction aids in ethanol aqueous solution to form spherical micelle powder, the problem of controlling the morphology and particle size of the spherical magnesium oxide precursor is solved, and high purity and high thermal conductivity are achieved The high-performance spherical magnesium oxide powder reduces water consumption and improves activity.

CN118561305BActive Publication Date: 2024-10-22SHANDONG RES & DESIGN ACADEMY OF IND CERAMICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411034689.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-22
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The morphology characteristics of the existing spherical magnesium oxide precursor are difficult to control, and the particle size is difficult to control at the nanometer level, resulting in low activity and many internal defects, which affects the performance of the terminal magnesium oxide powder, and the production process requires high water consumption and low output rate.

Method used

The soluble hydrated magnesium ion salt, magnesium ion surfactant and reaction aid are reacted in an ethanol aqueous solution to form spherical micelle powder agglomeration, and a white precipitate is formed through the action of the magnesium ion surfactant and reaction aid, which is prepared after drying. Obtain high thermal conductivity and high purity spherical magnesium oxide precursor, control the particle size to 10-50nm, reduce internal defects and improve activity.

Benefits of technology

It achieves nanoscale particle size control of the spherical magnesium oxide precursor, improves activity and performance, reduces water consumption, is suitable for industrial-scale production, and ensures the high purity and thermal conductivity of the spherical magnesium oxide powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561305B_ABST
    Figure CN118561305B_ABST
Patent Text Reader

Abstract

The present invention provides a high-thermal-conductivity and high-purity spherical magnesium oxide precursor and a preparation method thereof, which belong to the field of high-thermal-conductivity fillers. The preparation method of the high-thermal-conductivity and high-purity spherical magnesium oxide precursor adopts the following raw materials for preparation: soluble hydrated magnesium ion salt, magnesium ion surfactant, reaction aid, solvent; the magnesium ion surfactant is at least one of the following: octadecyl magnesium chloride, cyclohexyl magnesium chloride, and tridecyl magnesium sulfate. The preparation method of the high-thermal-conductivity and high-purity spherical magnesium oxide precursor effectively controls the morphological characteristics of the spherical magnesium oxide precursor, and the obtained spherical magnesium oxide precursor has a nanometer-scale size, reduces the internal defects of the spherical magnesium oxide precursor, effectively improves its activity, and ensures the performance of the terminal spherical magnesium oxide powder; and effectively overcomes the problem of the existing spherical magnesium oxide precursor in subsequent applications, which is caused by factors such as magnesium oxide crystallization and grain growth, and the spherical particle size is difficult to control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high thermal conductivity fillers, and in particular to a high thermal conductivity and high purity spherical magnesium oxide precursor and a preparation method thereof. Background Art

[0002] The existing spherical magnesium oxide precursor generally adopts soluble hydrated magnesium ion salt, adds carbonate (such as sodium carbonate, potassium carbonate, etc.) as a precipitant, and uses the soda ash method to obtain the spherical magnesium oxide precursor (magnesium carbonate hydrate). The spherical magnesium oxide precursor is washed to remove impurity ions such as sodium and potassium, and then dried, calcined, etc. to obtain spherical magnesium oxide powder.

[0003] However, the existing method for preparing a spherical magnesium oxide precursor has the following technical defects: First, the morphological characteristics of the spherical magnesium oxide precursor are difficult to control, and the spherical magnesium oxide precursor prepared by the existing preparation method is a magnesium carbonate hydrate with irregular angular or rod-shaped structures. Second, due to the limitation of the preparation process, the spherical magnesium oxide powder is prepared by the existing spherical magnesium oxide precursor, and it is necessary to achieve the purpose of purification by washing. A large amount of washing water is required during the washing process, and the production water consumption is high, and the output rate of the prepared spherical magnesium oxide powder is low; Third, since the existing spherical magnesium oxide precursor is prepared by direct precipitation, its particle size is generally in the micron level, and it is difficult to achieve nano-level control; and the larger the particle size of the spherical magnesium oxide precursor, the lower the activity, and the activity of the spherical magnesium oxide powder prepared by it is also low; At the same time, the larger the particle size of the spherical magnesium oxide precursor, the more defects inside the precursor particles, which has a greater impact on the performance of the terminal magnesium oxide powder, and seriously affects the back-end application of the spherical magnesium oxide powder.

[0004] Furthermore, in subsequent applications, the existing spherical magnesium oxide precursors still have problems such as broken spheres or difficulty in controlling the particle size of the spheres due to factors such as magnesium oxide crystallization and grain growth. Summary of the invention

[0005] In order to solve the technical problems existing in the prior art, the present invention provides a high-thermal conductivity and high-purity spherical magnesium oxide precursor and a preparation method thereof, which effectively controls the morphological characteristics of the spherical magnesium oxide precursor, and the prepared spherical magnesium oxide precursor has a nanometer size, reduces the internal defects of the spherical magnesium oxide precursor, avoids the adverse effect on the performance of the terminal magnesium oxide powder, effectively improves its activity, and ensures the performance of the terminal spherical magnesium oxide powder; and effectively overcomes the problem of broken balls or difficult to control the spherical particle size caused by magnesium oxide crystallization, grain growth and other factors in the subsequent application of the existing spherical magnesium oxide precursor.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a high-thermal-conductivity and high-purity spherical magnesium oxide precursor is prepared by using the following raw materials: a soluble hydrated magnesium ion salt, a magnesium ion surfactant, a reaction aid, and a solvent.

[0008] The soluble hydrated magnesium ion salt is at least one of the following: hydrated magnesium chloride salt, hydrated magnesium sulfate salt, and hydrated magnesium acetate salt.

[0009] The magnesium ion surfactant is at least one of the following: octadecyl magnesium chloride, cyclohexyl magnesium chloride, and tridecyl magnesium sulfate.

[0010] The reaction aid is at least one of the following: ammonium oxalate, ammonium acetate, ammonium formate, ammonium citrate, and ammonium phosphate.

[0011] The solvent is an ethanol aqueous solution; the water is not particularly limited and can be tap water or deionized water.

[0012] The method for preparing a high-thermal-conductivity high-purity spherical magnesium oxide precursor comprises the following steps: a soluble hydrated magnesium ion salt is dissolved in a solvent ethanol aqueous solution to form an ionic solution in the solvent; under the action of a magnesium ion surfactant, a spherical micelle powder agglomeration state is formed; the soluble hydrated magnesium ion salt is enriched on the surface of the polar bond of the magnesium-containing surfactant; under the action of a reaction aid, a white precipitate is formed; the white precipitate is dried to obtain a white spherical Mg(OH) x (CO) y (NH2) z Powder, that is, high thermal conductivity and high purity spherical magnesium oxide precursor.

[0013] The white spherical Mg(OH) x (CO) y (NH2) z In the powder, x is any number between 1 and 2, y is any number between 1 and 2, and z is any number between 1 and 2.

[0014] Preferably, the hydrated magnesium chloride salt is magnesium chloride hexahydrate; the hydrated magnesium sulfate salt is at least one of the following: magnesium sulfate heptahydrate, magnesium sulfate trihydrate, magnesium sulfate sulfate; and the hydrated magnesium acetate salt is magnesium oxalate dihydrate.

[0015] The hydrated magnesium chloride salt effectively achieves high concentration enrichment during the reaction and spheroidization agglomeration process. The magnesium ion surfactant can form spherical micelles in the solvent, which is further conducive to the enrichment of metal magnesium ions, and forms a combination of Mg-OH bonds, further improving the sphericity and ball densification of the magnesium ion product. After the reaction aid is dissolved in the solvent, under the action of ionic reaction, the ammonium ions react with the magnesium ions and the anion roots to form Mg-OH-NH bonding, and at the same time, the product is stripped from ethanol to form a precipitate, effectively realizing the collection of the spherical magnesium oxide precursor in the preparation process.

[0016] Preferably, the mass ratio of the soluble hydrated magnesium ion salt to the solvent is 15-35:65-85; the volume ratio of ethanol to water in the solvent is 15-25:75-85.

[0017] The dosage of magnesium ion surfactant is 0.1-0.5% of the mass of soluble hydrated magnesium ion salt;

[0018] The dosage of the reaction aid is 1-5% of the mass of the soluble hydrated magnesium ion salt.

[0019] The method for preparing the high thermal conductivity and high purity spherical magnesium oxide precursor comprises the following steps:

[0020] Step S001, water and anhydrous ethanol are mixed as a solvent, a magnesium ion surfactant is added, and the temperature is raised to 50-80°C under high-speed stirring conditions of more than 1000 r / min in a negative pressure environment of -0.1 MPa, and the reaction is kept warm for 2 hours or more, the pressure is released, and the mixture is allowed to stand to obtain a transparent solution, and then the mixing and stirring is continued for 0.5 hours in a normal pressure environment to obtain a white low-viscosity slurry with a viscosity of 350-600 mPa·s.

[0021] In step S001, in a mixed solvent of ethanol and water, at a negative pressure of -0.1MPa and an environment of 50-80°C, a magnesium ion surfactant is introduced, the magnesium ion surfactant is dissolved in the mixed solution, and a structure with polar bonds facing outward and non-polar bonds facing inward is formed, generating a spherical micelle system; due to the polar bond effect, the magnesium ion salt can be more effectively adsorbed in subsequent steps. Furthermore, since the magnesium ion surfactant used itself has a magnesium element component, the uniformity of the magnesium element in the spherical micelle can be effectively maintained.

[0022] Step S002: add soluble hydrated magnesium ion salt to the white low-viscosity slurry, raise the temperature to 200-300° C. under stirring conditions of 300-500 r / min, in a negative pressure environment of -0.1 MPa, and keep the mixture warm and stirred for 1 hour or more to obtain a milky white uniform solution with a viscosity of 500-700 mPa·s.

[0023] Step S003, adding a reaction aid to the milky white uniform solution, stirring at 150-200 r / min, in a negative pressure environment of -0.1 MPa, heat-insulating mixing and stirring for 0.5 h or more, standing for 2 h or more, and separating to obtain a white precipitate.

[0024] The white low-viscosity slurry in step S001 has a spherical micelle system, and the spherical micelles form chemical bonds. In steps S002 and S003, a soluble hydrated magnesium ion salt is added to the white low-viscosity slurry, and the magnesium ions are freely adsorbed on the polar bonds on the surface of the spherical micelles and are enriched in high concentration to form Mg-OH bonds; then, under the action of the reaction aid, the ammonium ions react with the Mg 2+ Ion, OH - The ions react to form Mg-OH-NH bonds, which in turn form a white precipitate.

[0025] Step S004: wash the white precipitate with 1-2 times the weight of water, and then dry it to obtain a white spherical powder, i.e., a high thermal conductivity and high purity spherical magnesium oxide precursor.

[0026] A high thermal conductivity and high purity spherical magnesium oxide precursor is prepared by the above-mentioned preparation method; the particle size of the high thermal conductivity and high purity spherical magnesium oxide precursor is 10-50nm, the spheroidization rate is greater than 90% and the density is less than 3.1g / cm 3 .

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The preparation method of the high thermal conductivity and high purity spherical magnesium oxide precursor of the present invention comprises the following steps: a soluble hydrated magnesium ion salt is dissolved in an ethanol aqueous solvent to form an ionic solution in the solvent; under the action of a magnesium ion surfactant, a spherical micelle powder is formed in an agglomerated state; the soluble hydrated magnesium ion salt is enriched on the polar bond surface of the magnesium-containing surfactant; under the action of a reaction aid, a white precipitate is formed; the white precipitate is dried to obtain a white spherical Mg(OH) x (CO) y (NH2) z The powder, i.e. a high-thermal-conductivity and high-purity spherical magnesium oxide precursor, effectively controls the morphology characteristics of the spherical magnesium oxide precursor, and the prepared spherical magnesium oxide precursor has a nanometer-scale size, reduces the internal defects of the spherical magnesium oxide precursor, avoids the adverse effect on the performance of the terminal magnesium oxide powder, effectively improves its activity, and ensures the performance of the terminal spherical magnesium oxide powder; and effectively overcomes the problem of broken balls or difficult to control spherical particle size caused by magnesium oxide crystallization, grain growth and other factors in the subsequent application of the existing spherical magnesium oxide precursor.

[0029] (2) The high thermal conductivity and high purity spherical magnesium oxide precursor of the present invention has a particle size of 10-50nm, a spheroidization rate of more than 90% and a density of less than 3.1g / cm 3, the particle size of the spherical magnesium oxide precursor can be controlled at the nanometer level, and the spheroidization rate is high; and by using the high thermal conductivity and high purity spherical magnesium oxide precursor, high crystallization of the spherical magnesium oxide powder can be achieved through low temperature calcination, and the preparation of micrometer-level and nanometer-level spherical magnesium oxide powder is effectively realized, while ensuring the performance, the manufacturing cost of small-size spherical magnesium oxide powder is reduced; the spherical magnesium oxide powder prepared by using the high thermal conductivity and high purity spherical magnesium oxide precursor can control the particle size d50 within the range of 0.05-5μm, and the spheroidization rate is greater than 90% detected by SEM, the purity is greater than 98.5wt%, and the density is less than 3.6g / cm 3 The thermal conductivity is in the range of 40-60W / (m·K). The particle size of the spherical magnesium oxide powder can be regulated by the precursor and is easy to control. The spherical magnesium oxide powder has good sphericity, high purity and good thermal conductivity, which effectively guarantees the subsequent application performance of the spherical magnesium oxide powder.

[0030] (3) The high thermal conductivity and high purity spherical magnesium oxide precursor of the present invention has a simple process flow and low requirements for production raw materials. Compared with the existing preparation process, it does not require a large amount of water for washing and purification, which can reduce water consumption and increase the output of the terminal spherical magnesium oxide powder, and is suitable for industrial-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is an electron microscope photograph of the high thermal conductivity and high purity spherical magnesium oxide precursor prepared in Example 1. DETAILED DESCRIPTION

[0032] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0033] Example 1

[0034] like Figure 1 As shown, this embodiment provides a high thermal conductivity and high purity spherical magnesium oxide precursor, and the specific specifications are shown in Table 1:

[0035] Table 1 Specific specifications of the high thermal conductivity and high purity spherical magnesium oxide precursor of Example 1

[0036]

[0037] The high-thermal-conductivity and high-purity spherical magnesium oxide precursor is prepared from the following raw materials: soluble hydrated magnesium ion salt, magnesium ion surfactant, reaction aid, and solvent.

[0038] The soluble hydrated magnesium ion salt is specifically a combination of magnesium chloride hexahydrate, magnesium sulfate heptahydrate, and magnesium oxalate dihydrate; the mass ratio of the magnesium chloride hexahydrate, magnesium sulfate heptahydrate, and magnesium oxalate dihydrate is 1:1:1.

[0039] The magnesium ion surfactant is octadecyl magnesium chloride.

[0040] The reaction aid is ammonium oxalate.

[0041] The solvent is an ethanol-water solution; the volume ratio of ethanol to water is 25:75.

[0042] The mass ratio of the soluble hydrated magnesium ion salt to the solvent is 15:85.

[0043] The dosage of magnesium ion surfactant is 0.1% of the mass of soluble hydrated magnesium ion salt;

[0044] The dosage of the reaction aid is 5% of the mass of the soluble hydrated magnesium ion salt.

[0045] Specifically, the specific weight portions of the above raw materials are as follows:

[0046] 5 parts of magnesium chloride hexahydrate;

[0047] 5 parts of magnesium sulfate heptahydrate;

[0048] 5 parts of magnesium oxalate dihydrate;

[0049] Water 63.75 parts;

[0050] Ethanol 21.25 parts;

[0051] 0.015 parts of octadecyl magnesium chloride;

[0052] 0.75 parts of ammonium oxalate.

[0053] This embodiment also provides a method for preparing the aforementioned high thermal conductivity and high purity spherical magnesium oxide precursor, wherein a soluble hydrated magnesium ion salt is dissolved in a solvent ethanol aqueous solution to form an ionic solution in the solvent, and under the action of a magnesium ion surfactant, a spherical micelle powder agglomeration state is formed, and the soluble hydrated magnesium ion salt is enriched on the surface of the polar bond of the magnesium element-containing surfactant, and under the action of a reaction aid, a white precipitate is formed; the white precipitate is dried to obtain a white spherical Mg(OH) x (CO) y (NH2) z Powder, that is, high thermal conductivity and high purity spherical magnesium oxide precursor.

[0054] Wherein, the white spherical Mg(OH) x (CO) y (NH2) z In powder, x=1, y=1, z=2.

[0055] The method for preparing the high thermal conductivity and high purity spherical magnesium oxide precursor comprises the following steps:

[0056] Step S001, water and anhydrous ethanol are mixed as a solvent, a magnesium ion surfactant is added, and the temperature is raised to 60° C. under a high-speed stirring condition of 1200 r / min in a negative pressure environment of -0.1 MPa, and the reaction is kept warm for 2 hours or more, the pressure is released, and the mixture is allowed to stand to obtain a transparent solution, and then the mixing and stirring is continued for 0.5 hours in a normal pressure environment to obtain a white low-viscosity slurry with a viscosity of 550 mPa·s.

[0057] Step S002: add soluble hydrated magnesium ion salt to the white low-viscosity slurry, raise the temperature to 300° C. under a stirring condition of 300 r / min and a negative pressure environment of -0.1 MPa, and keep the mixture warm and stirred for 1 hour to obtain a milky white uniform solution with a viscosity of 700 mPa·s.

[0058] Step S003, adding a reaction aid to the milky white uniform solution, stirring at 150 r / min, in a negative pressure environment of -0.1 MPa, heat-insulating mixing and stirring for 0.5 h, letting it stand for 2 h, and separating to obtain a white precipitate.

[0059] Step S004: wash the white precipitate twice with an equal weight of water, and then dry it to obtain a white spherical powder, i.e., a high thermal conductivity and high purity spherical magnesium oxide precursor.

[0060] The high thermal conductivity and high purity spherical magnesium oxide precursor of this embodiment is used. The particle size d50 of the spherical magnesium oxide powder obtained after sintering can be controlled within the range of 0.05-5 μm. The spheroidization rate is greater than 90% and the purity is greater than 98.5wt% and the density is less than 3.6g / cm 3 The thermal conductivity is in the range of 40-60W / (m·K). The particle size of the spherical magnesium oxide powder can be regulated by the precursor and is easy to control. The spherical magnesium oxide powder has good sphericity, high purity and good thermal conductivity, which effectively guarantees the subsequent application performance of the spherical magnesium oxide powder.

[0061] Example 2

[0062] This embodiment provides a high thermal conductivity and high purity spherical magnesium oxide precursor, and the specific specifications are shown in Table 2:

[0063] Table 2 Specific specifications of the high thermal conductivity and high purity spherical magnesium oxide precursor of Example 2

[0064]

[0065] The high-thermal-conductivity and high-purity spherical magnesium oxide precursor is prepared from the following raw materials: soluble hydrated magnesium ion salt, magnesium ion surfactant, reaction aid, and solvent.

[0066] The soluble hydrated magnesium ion salt is specifically a combination of magnesium chloride hexahydrate, magnesium sulfate heptahydrate, magnesium sulfate trihydrate, and magnesium oxalate dihydrate; the mass ratio of the magnesium chloride hexahydrate, magnesium sulfate heptahydrate, magnesium sulfate trihydrate, and magnesium oxalate dihydrate is 1:0.5:0.5:1.

[0067] The magnesium ion surfactant is magnesium tridecyl sulfate.

[0068] The reaction aid is ammonium acetate.

[0069] The solvent is an ethanol-water solution; the volume ratio of ethanol to water is 15:85.

[0070] The mass ratio of the soluble hydrated magnesium ion salt to the solvent is 30:70.

[0071] The dosage of magnesium ion surfactant is 0.15% of the mass of soluble hydrated magnesium ion salt;

[0072] The dosage of the reaction aid is 3% of the mass of the soluble hydrated magnesium ion salt.

[0073] Specifically, the specific weight portions of the above raw materials are as follows:

[0074] 10 parts of magnesium chloride hexahydrate;

[0075] 5 parts of magnesium sulfate heptahydrate;

[0076] 5 parts of magnesium sulfate trihydrate;

[0077] 10 parts of magnesium oxalate dihydrate;

[0078] Water 59.5 parts;

[0079] 10.5 parts of ethanol;

[0080] 0.045 parts of tridecyl magnesium sulfate;

[0081] 0.9 parts of ammonium acetate.

[0082] This embodiment also provides a method for preparing the aforementioned high thermal conductivity and high purity spherical magnesium oxide precursor, wherein a soluble hydrated magnesium ion salt is dissolved in a solvent ethanol aqueous solution to form an ionic solution in the solvent, and under the action of a magnesium ion surfactant, a spherical micelle powder agglomeration state is formed, and the soluble hydrated magnesium ion salt is enriched on the surface of the polar bond of the magnesium element-containing surfactant, and under the action of a reaction aid, a white precipitate is formed; the white precipitate is dried to obtain a white spherical Mg(OH) x (CO) y (NH2) z Powder, that is, high thermal conductivity and high purity spherical magnesium oxide precursor.

[0083] Wherein, the white spherical Mg(OH)x (CO) y (NH2) z In powder, x=1, y=1, z=2.

[0084] The method for preparing the high thermal conductivity and high purity spherical magnesium oxide precursor comprises the following steps:

[0085] Step S001, water and anhydrous ethanol are mixed as a solvent, a magnesium ion surfactant is added, and the temperature is raised to 80° C. under a high-speed stirring condition of 1100 r / min in a negative pressure environment of -0.1 MPa, and the reaction is kept warm for 2 hours. The pressure is released and the mixture is allowed to stand to obtain a transparent solution, and then the mixture is continued to be mixed and stirred for 0.5 hours in a normal pressure environment to obtain a white low-viscosity slurry with a viscosity of 600 mPa·s.

[0086] Step S002: add soluble hydrated magnesium ion salt to the white low-viscosity slurry, raise the temperature to 300° C. under a stirring condition of 350 r / min and a negative pressure environment of -0.1 MPa, and keep the mixture stirred for 1 hour to obtain a milky white uniform solution with a viscosity of 700 mPa·s.

[0087] Step S003, adding a reaction aid to the milky white uniform solution, stirring at 150 r / min, in a negative pressure environment of -0.1 MPa, heat-insulating mixing and stirring for 1 hour, standing for 2 hours, and separating to obtain a white precipitate.

[0088] Step S004: washing the white precipitate twice with an equal weight of water, and then drying to obtain a white spherical powder, i.e., a high thermal conductivity and high purity spherical magnesium oxide precursor.

[0089] The high thermal conductivity and high purity spherical magnesium oxide precursor of this embodiment is used. The particle size d50 of the spherical magnesium oxide powder obtained after sintering can be controlled within the range of 0.05-5 μm. The spheroidization rate is greater than 90% and the purity is greater than 98.5wt% and the density is less than 3.6g / cm 3 The thermal conductivity is in the range of 40-60W / (m·K). The particle size of the spherical magnesium oxide powder can be regulated by the precursor and is easy to control. The spherical magnesium oxide powder has good sphericity, high purity and good thermal conductivity, which effectively guarantees the subsequent application performance of the spherical magnesium oxide powder.

[0090] Example 3

[0091] This embodiment provides a high thermal conductivity and high purity spherical magnesium oxide precursor, and the specific specifications are shown in Table 3:

[0092] Table 3 Specific specifications of the high thermal conductivity and high purity spherical magnesium oxide precursor of Example 3

[0093]

[0094] The high-thermal-conductivity and high-purity spherical magnesium oxide precursor is prepared from the following raw materials: soluble hydrated magnesium ion salt, magnesium ion surfactant, reaction aid, and solvent.

[0095] The soluble hydrated magnesium ion salt is a soluble hydrated magnesium ion salt, specifically a combination of magnesium chloride hexahydrate, magnesium sulfate hexahydrate, and magnesium oxalate dihydrate; the mass ratio of the magnesium chloride hexahydrate, magnesium sulfate hexahydrate, and magnesium oxalate dihydrate is 1:1:1.

[0096] The magnesium ion surfactant is cyclohexylmagnesium chloride.

[0097] The reaction aid is ammonium citrate.

[0098] The solvent is an ethanol-water solution; the volume ratio of ethanol to water is 20:80.

[0099] Wherein, the mass ratio of soluble hydrated magnesium ion salt to solvent is 18:82.

[0100] The dosage of magnesium ion surfactant is 0.3% of the mass of soluble hydrated magnesium ion salt;

[0101] The dosage of the reaction aid is 2% of the mass of the soluble hydrated magnesium ion salt.

[0102] Specifically, the specific weight portions of the above raw materials are as follows:

[0103] 6 parts of magnesium chloride hexahydrate;

[0104] 6 parts of magnesium sulfate hexahydrate;

[0105] 6 parts of magnesium oxalate dihydrate;

[0106] Water 65.6 parts;

[0107] 14.4 parts of ethanol;

[0108] 0.054 parts of cyclohexylmagnesium chloride;

[0109] 0.36 parts of ammonium citrate.

[0110] This embodiment also provides a method for preparing the aforementioned high thermal conductivity and high purity spherical magnesium oxide precursor, wherein a soluble hydrated magnesium ion salt is dissolved in a solvent ethanol aqueous solution to form an ionic solution in the solvent, and under the action of a magnesium ion surfactant, a spherical micelle powder agglomeration state is formed, and the soluble hydrated magnesium ion salt is enriched on the surface of the polar bond of the magnesium element-containing surfactant, and under the action of a reaction aid, a white precipitate is formed; the white precipitate is dried to obtain a white spherical Mg(OH) x (CO) y (NH2) z Powder, that is, high thermal conductivity and high purity spherical magnesium oxide precursor.

[0111] Wherein, the white spherical Mg(OH) x (CO) y (NH2) z In powder, x=1, y=2, z=2.

[0112] The method for preparing the high thermal conductivity and high purity spherical magnesium oxide precursor comprises the following steps:

[0113] Step S001, water and anhydrous ethanol are mixed as a solvent, a magnesium ion surfactant is added, and the temperature is raised to 65° C. under a high-speed stirring condition of 1600 r / min in a negative pressure environment of -0.1 MPa, and the reaction is kept warm for 3 hours, the pressure is released, and the mixture is allowed to stand to obtain a transparent solution, and then the mixing and stirring is continued for 0.5 hours in a normal pressure environment to obtain a white low-viscosity slurry with a viscosity of 350 mPa·s.

[0114] Step S002: Add soluble hydrated magnesium ion salt to the white low-viscosity slurry, raise the temperature to 300° C. under a stirring condition of 450 r / min and a negative pressure environment of -0.1 MPa, and keep the mixture stirred for 1 hour to obtain a milky white uniform solution with a viscosity of 700 mPa·s.

[0115] Step S003, adding a reaction aid to the milky white uniform solution, stirring at 150 r / min, in a negative pressure environment of -0.1 MPa, keeping warm and mixing for 1 hour, letting it stand for 2 hours, and separating to obtain a white precipitate.

[0116] Step S004: wash the white precipitate twice with an equal weight of water, and then dry it to obtain a white spherical powder, i.e., a high thermal conductivity and high purity spherical magnesium oxide precursor.

[0117] The high thermal conductivity and high purity spherical magnesium oxide precursor of this embodiment is used. The particle size d50 of the spherical magnesium oxide powder obtained after sintering can be controlled within the range of 0.05-5 μm. The spheroidization rate is greater than 90% and the purity is greater than 98.5wt% and the density is less than 3.6g / cm 3 The thermal conductivity is in the range of 40-60W / (m·K). The particle size of the spherical magnesium oxide powder can be regulated by the precursor and is easy to control. The spherical magnesium oxide powder has good sphericity, high purity and good thermal conductivity, which effectively guarantees the subsequent application performance of the spherical magnesium oxide powder.

[0118] Comparative Example 1

[0119] Comparative Example 1 adopts the technical scheme of Example 1, except that: 1) an equal weight portion of octadecyltrimethylammonium chloride is used to replace the magnesium ion surfactant (octadecylmagnesium chloride); 2) an equal weight portion of sodium carbonate is used to replace the reaction aid (ammonium oxalate); and the weight portions of other raw materials remain unchanged.

[0120] Specifically, in the preparation method of the spherical magnesium oxide precursor of Comparative Example 1, in order to reduce the sodium ion content in step S004, it is necessary to continuously perform 10 washing and purification processes, which consumes a large amount of washing water and has a high water consumption; the white spherical Mg(OH) x (CO) y (NH2) z Powder, x=1, y=3, z=2.

[0121] The specific specifications of the spherical magnesium oxide precursor of Comparative Example 1 are shown in Table 4:

[0122] Table 4 Specific specifications of the high thermal conductivity and high purity spherical magnesium oxide precursor of Comparative Example 1

[0123]

[0124] Since the particle size d50 of the spherical magnesium oxide precursor in the comparative example is 12 μm and the spheroidization rate is low, the particle size of the spherical magnesium oxide powder obtained after sintering it is difficult to control at the nanoscale level, the spheroidization rate is poor, and there are relatively many internal defects, which affect the activity of the spherical magnesium oxide powder; and the thermal conductivity of the spherical magnesium oxide powder is reduced, which is not conducive to the subsequent application of the spherical magnesium oxide powder.

[0125] It can be seen that the preparation method of the high thermal conductivity and high purity spherical magnesium oxide precursor of the present invention is that the soluble hydrated magnesium ion salt is dissolved in the solvent ethanol aqueous solution to form an ionic solution in the solvent, and under the action of the magnesium ion surfactant, a spherical micelle powder agglomeration state is formed, and the soluble hydrated magnesium ion salt is enriched on the polar bond surface of the magnesium element-containing surfactant, and under the action of the reaction aid, a white precipitate is formed; the white precipitate is dried to obtain white spherical Mg(OH) x (CO) y (NH2) z The powder, i.e. a high-thermal-conductivity and high-purity spherical magnesium oxide precursor, effectively controls the morphology characteristics of the spherical magnesium oxide precursor, and the prepared spherical magnesium oxide precursor has a nanometer-scale size, reduces the internal defects of the spherical magnesium oxide precursor, avoids the adverse effect on the performance of the terminal magnesium oxide powder, effectively improves its activity, and ensures the performance of the terminal spherical magnesium oxide powder; and effectively overcomes the problem of broken balls or difficult to control spherical particle size caused by magnesium oxide crystallization, grain growth and other factors in the subsequent application of the existing spherical magnesium oxide precursor.

[0126] Unless otherwise specified, all percentages used in the present invention are by mass.

[0127] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-thermal-conductivity, high-purity spherical magnesium oxide precursor, characterized in that: The preparation is carried out using the following raw materials: soluble hydrated magnesium ion salt, magnesium ion surfactant, reaction auxiliary agent and solvent; The soluble hydrated magnesium ion salt is at least one of the following: hydrated magnesium chloride salt, hydrated magnesium sulfate salt, hydrated magnesium acetate salt; The magnesium ion surfactant is at least one of the following: octadecyl magnesium chloride, cyclohexyl magnesium chloride, tridecyl magnesium sulfate; The reaction aid is at least one of the following: ammonium oxalate, ammonium acetate, ammonium formate, ammonium citrate, and ammonium phosphate; The solvent is an ethanol aqueous solution; The method for preparing a high-thermal-conductivity and high-purity spherical magnesium oxide precursor comprises the following steps: a soluble hydrated magnesium ion salt is dissolved in a solvent to form an ionic solution in the solvent; under the action of a magnesium ion surfactant, a spherical micelle powder is formed in an agglomerated state; the soluble hydrated magnesium ion salt is enriched on the surface of the polar bond of the magnesium-containing surfactant; under the action of a reaction aid, a white precipitate is formed; the white precipitate is dried to obtain a white spherical Mg(OH) x (CO) y (NH2) z Powder; The white spherical Mg(OH) x (CO) y (NH2) z In the powder, x is any number between 1 and 2, y is any number between 1 and 2, and z is any number between 1 and 2; The method for preparing the high thermal conductivity and high purity spherical magnesium oxide precursor comprises the following steps: Step S001, adding a magnesium ion surfactant to a solvent, raising the temperature to 50-80° C. in a negative pressure environment under a high-speed stirring condition of 1000 r / min or more, keeping the temperature for reaction for 2 hours or more, releasing the pressure, standing, and after obtaining a transparent solution, continuing to mix and stir in a normal pressure environment to obtain a white low-viscosity slurry; Step S002, adding a soluble hydrated magnesium ion salt to the white low-viscosity slurry, heating to 200-300° C. under a stirring condition of 300-500 r / min in a negative pressure environment, and mixing and stirring for 1 hour or more to obtain a milky white uniform solution; Step S003, adding a reaction aid to the milky white uniform solution, stirring at 150-200 r / min in a negative pressure environment, keeping the mixture warm and stirring for 0.5 h or more, letting it stand for 2 h or more, and separating to obtain a white precipitate; Step S004: The white precipitate is washed and dried to obtain a high-thermal-conductivity and high-purity spherical magnesium oxide precursor.

2. The method for preparing a high thermal conductivity and high purity spherical magnesium oxide precursor according to claim 1, characterized in that: The hydrated magnesium chloride salt is magnesium chloride hexahydrate; The hydrated magnesium sulfate salt is at least one of the following: magnesium sulfate heptahydrate, magnesium sulfate trihydrate; The hydrated magnesium acetate salt is magnesium oxalate dihydrate.

3. The method for preparing a high thermal conductivity and high purity spherical magnesium oxide precursor according to claim 1, characterized in that: The mass ratio of the soluble hydrated magnesium ion salt to the solvent is 15-35:65-85; The volume ratio of ethanol to water in the solvent is 15-25:75-85.

4. The method for preparing a high thermal conductivity and high purity spherical magnesium oxide precursor according to claim 1, characterized in that: The dosage of magnesium ion surfactant is 0.1-0.5% of the mass of soluble hydrated magnesium ion salt; The dosage of the reaction aid is 1-5% of the mass of the soluble hydrated magnesium ion salt.

5. The method for preparing a high thermal conductivity and high purity spherical magnesium oxide precursor according to claim 1, characterized in that: In the step S001, the viscosity of the white low-viscosity slurry is 350-600 mPa·s; In the step S002, the viscosity of the milky white uniform solution is 500-700 mPa·s.

6. A high thermal conductivity and high purity spherical magnesium oxide precursor, characterized in that: The high thermal conductivity and high purity spherical magnesium oxide precursor is prepared by the preparation method according to any one of claims 1 to 5; the particle size of the high thermal conductivity and high purity spherical magnesium oxide precursor is 10-50nm, the spheroidization rate is greater than 90% and the density is less than 3.1g / cm 3 .