Gas barrier polyamide elastomer material and preparation method thereof

By using capsule catalysts and introducing naphthalene rings in polyamide elastomers, the problems of catalyst deactivation and poor material flexibility are solved, gas barrier and mechanical properties are improved, and more efficient polymerization control is achieved.

CN118562124BActive Publication Date: 2024-10-18SHANDONG GUANGYIN NEW MATERIALS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411031169.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-18
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing polyamide elastomer materials are prone to catalyst deactivation during the esterification reaction, resulting in low molecular weight and poor performance. Short-chain nylon has high water absorption and poor flexibility, which affects gas barrier properties.

Method used

A capsule-type catalyst is used to embed the esterification reaction catalyst in nylon capsule walls with different melting points. By controlling the temperature, the catalyst is gradually released, reducing the contact between the catalyst and by-products, and a naphthalene ring is introduced to improve the gas barrier performance.

Benefits of technology

It improves the gas barrier properties, heat resistance and mechanical properties of the polyamide elastomer, reduces the deactivation of the catalyst, simplifies the process and facilitates industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyamide elastomers, and specifically relates to a gas barrier polyamide elastomer material and a preparation method thereof. The preparation method comprises the following steps: S1, preparing a dicarboxyl-terminated polyamide prepolymer, wherein the polyamide is a long carbon chain polyamide; S2, preparing a polyester oligomer containing a naphthalene ring, which is prepared from naphthalene dicarboxylic acid and a polyether diol; S3, the dicarboxyl-terminated polyamide prepolymer, the polyester oligomer containing a naphthalene ring, and the polyether diol are subjected to a polycondensation reaction under the action of a catalyst A to obtain a polyamide elastomer containing a naphthalene ring, which is the gas barrier polyamide elastomer material; the catalyst A is a capsule-type catalyst, comprising a heated and molten nylon capsule wall and an esterification reaction catalyst embedded in the nylon capsule wall. The present invention improves gas barrier performance, heat resistance and mechanical properties. The preparation method of the present invention has an easy-to-control reaction and reduces the deactivation of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyamide elastomers, and in particular relates to a gas barrier polyamide elastomer material and a preparation method thereof. Background Art

[0002] Gas barrier performance is an important performance that affects the packaging effect, and is crucial for maintaining the freshness of products and extending the shelf life. At present, the main film materials used for packaging are PA66, PA6, PAMXD6, etc., and are mostly used for composite films. However, short-chain nylon has a high water absorption rate and slightly poor elasticity, and the packaging film made of it has poor flexibility. Polyamide elastomer materials are widely used in electronics, aerospace, medical devices, etc. due to their excellent elasticity, good low temperature resistance, and good mechanical properties.

[0003] Polyamide elastomer is obtained by polycondensation of polyamide hard segment and polyester soft segment through esterification reaction. The byproduct of esterification reaction is water, and the esterification reaction catalyst is easily hydrolyzed, which easily causes the catalyst to be deactivated. The obtained polymer has a low molecular weight, poor performance and even cannot be used normally. Chinese invention patent publication number CN113968966A disperses the esterification reaction catalyst in a low-viscosity nylon with double carboxyl end-capping, and obtains a catalyst carrier after stranding and granulation to prevent the catalyst from being deactivated by water and ensure that the catalyst is evenly dispersed to ensure the reaction. However, the invention does not consider whether the catalyst and low-viscosity nylon will be partially "deteriorated" due to high temperature and shearing when blended through a twin-screw extruder, thereby affecting the catalytic effect. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a gas barrier polyamide elastomer material, which improves the gas barrier performance, heat resistance and mechanical properties. The present invention also provides a preparation method thereof, which makes the reaction easy to control and reduces the deactivation of the catalyst.

[0005] The method for preparing the gas barrier polyamide elastomer material of the present invention comprises the following steps:

[0006] S1, preparing a dicarboxyl-terminated polyamide prepolymer, wherein the polyamide is a long carbon chain polyamide;

[0007] S2, preparing a polyester oligomer containing a naphthalene ring, which is prepared from naphthalene dicarboxylic acid and a polyether diol, and an esterification catalyst can be added in step S2;

[0008] S3, a dicarboxyl-terminated polyamide prepolymer, a polyester oligomer containing a naphthalene ring, and a polyether diol are subjected to a polycondensation reaction under the action of a catalyst A to obtain a polyamide elastomer containing a naphthalene ring, which is the gas barrier polyamide elastomer material;

[0009] Catalyst A is a capsule-type catalyst, comprising a heated and melted nylon capsule wall and an esterification reaction catalyst embedded in the nylon capsule wall.

[0010] Preferably, in step S1, the dicarboxyl-terminated polyamide prepolymer is prepared by polycondensation of a dibasic acid and a diamine, the dibasic acid is selected from one of sebacic acid, dodecanedioic acid, and tetradecanedioic acid, and the diamine is selected from one of hexanediamine, nonanediamine, decanediamine, dodecanediamine, and tetradecanediamine.

[0011] Preferably, in step S2, the naphthalene dicarboxylic acid is selected from one of 2,6-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, and 2,3-naphthalene dicarboxylic acid; the polyether diol is a low molecular weight polyether diol selected from one of polyethylene glycol, polypropylene glycol, and polytetrahydrofuran diol, and has a number average molecular weight of 200 to 600.

[0012] Preferably, in step S3, the polyether diol is selected from one of polyethylene glycol, polypropylene glycol, and polytetrahydrofuran diol, and has a number average molecular weight of 800 to 2000.

[0013] Preferably, in step S3, the reaction temperature is 200-280°C, and the reaction is divided into two consecutive stages, the reaction temperature of the first stage is 200-230°C, and the reaction temperature of the second stage is 230-280°C; the reaction vacuum degree is 50-500 Pa, and the reaction time is 4-8h.

[0014] Preferably, the esterification reaction catalyst is one or more of zinc acetate, magnesium acetate, antimony acetate, triisobutyl lithium, dibutyl tin oxide, titanium dioxide, antimony trioxide, butyl titanate, tetrabutyl zirconate, and isopropyl titanate; in step S2 or S3, the amount of the esterification reaction catalyst used is 0.1% to 3% of the mass of the polyether diol.

[0015] Preferably, the nylon capsule wall is made of nylon and has a thickness of 200-500 μm.

[0016] Preferably, the nylon capsule wall includes an inner layer and an outer layer, which are made of nylon materials with different melting points, respectively, and are selected from one of PA66, PA610, PA612, PA1010, PA1012, and PA1212. The melting point of the outer nylon capsule wall is 185~218°C, and the melting point of the inner nylon capsule wall is 218~253°C; the esterification reaction catalyst is embedded in the inner layer and between the inner layer and the outer layer.

[0017] Preferably, the mass ratio of the esterification reaction catalyst embedded in the inner layer and between the inner layer and the outer layer is 1:2.

[0018] Preferably, in step S1, the molar number of the diamine is a, and the molar number of the dibasic acid is b; in step S2, the molar number of naphthalene dicarboxylic acid is c, and the molar number of the polyether diol is d; in step S3, the molar number of the polyether diol is e; then b / a=1.02-1.4, c / d=1, a+d+e=b+c;

[0019] The amount of naphthalene dicarboxylic acid added is 10% to 20% of the total mass of the diamine and dibasic acid in step S1, the naphthalene dicarboxylic acid and polyether diol in step S2, and the polyether diol in step S3.

[0020] Preferably, a polymerization additive may be added in step S3, and the polymerization additive is an antioxidant and a heat stabilizer. The antioxidant is one of antioxidant 1010, antioxidant 1098, and antioxidant 626; the heat stabilizer is one or more of organic copper salt heat stabilizer Finnre-336, organic tin heat stabilizer TBPT, and organic phosphite. The addition amount of the polymerization additive is 0.1% to 0.5% of the total mass of the diamine and dibasic acid in step S1, the naphthalene dicarboxylic acid and polyether diol in step S2, and the polyether diol in step S3.

[0021] The gas barrier polyamide elastomer material of the present invention is prepared by the above-mentioned preparation method.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. In order to increase the gas barrier performance of the polyamide elastomer, the present invention introduces naphthalene rings into the molecular chain of the polyamide elastomer. Since the naphthalene rings are more likely to be planar, the gas barrier performance of the material can be greatly improved;

[0024] 2. In order to ensure the activity of the catalyst and the simplicity of the process, the present invention adopts a "capsule" stacking method to seal the esterification reaction catalyst in the capsule of the nylon capsule wall with different melting points. As the reaction proceeds, the temperature increases from low to high. After reaching the melting point of the outer nylon, the outer nylon first melts to release a part of the esterification reaction catalyst, and then the temperature rises to reach the melting point of the inner nylon, and the inner nylon melts again to release the remaining part of the esterification reaction catalyst, thereby realizing the gradual release of the esterification reaction catalyst, reducing the contact probability between the catalyst and the reaction by-products, and ensuring that the catalyst can maintain good catalytic activity during the entire reaction process; the inner nylon capsule wall and the outer nylon capsule wall can be matched and stacked in multiple layers, and a plurality of capsule-type catalysts with different melting rates can be set at the same time, and the release time and amount of the esterification reaction catalyst can be controlled by controlling the reaction temperature, so as to better control the progress of the reaction;

[0025] 3. The capsule catalyst can be added into the reactor together with the reaction monomers. The release of the esterification reaction catalyst can be controlled by controlling the reaction temperature. It does not need to be added during the reaction. It is simple and easy to operate. The process is scientific and reasonable, and it is easy to realize industrial production. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.

[0027] Unless otherwise specified, all raw materials used in the examples are commercially available.

[0028] Example 1

[0029] S1. Preparation of dicarboxyl-terminated polyamide prepolymer

[0030] 1568.7g (13.5mol) hexamethylenediamine, 3171.2g (13.77mol) dodecanedioic acid and deionized water were stirred evenly and heated until clear, then added into a polymerization kettle, and the reaction was started after nitrogen replacement for 5 times; the temperature was raised to 220°C, the pressure to 1.3MPa, and the pressure was maintained constant, and the temperature was continued to be raised to 240°C, and the pressure was reduced to normal pressure after 2h; after the normal pressure, the vacuum reaction was carried out, the vacuum degree was -0.05MPa, and the reaction time was 30min, and the product was obtained;

[0031] S2. Preparation of polyester oligomers containing naphthalene rings

[0032] 1620g (7.5mol) of 1,4-naphthalenedicarboxylic acid and 1500g (7.5mol) of polyethylene glycol with a molecular weight of 200 were added to a polymerization kettle, and 45g of butyl titanate was added. The mixture was heated to 100°C, and the negative pressure was maintained at 200Pa. The reaction was continued for 3h to obtain the product.

[0033] S3. Preparation of polyamide elastomer

[0034] The products of step S1 and S2, the dicarboxyl-terminated polyamide prepolymer, the polyester oligomer containing naphthalene rings, and 270g (0.27mol) of polyethylene glycol with a molecular weight of 1000 are added to a polymerization kettle, and 13.5g of antioxidant 1098, 27.1g of heat stabilizer Finnre-336, and 6g of esterification catalyst tetrabutyl zirconate are added. Of the 6g of tetrabutyl zirconate, 2g is embedded in the inner layer (thickness 200μm) made of PA66 (melting point 253°C), and 4g is embedded between the inner layer and the outer layer (thickness 200μm) made of PA612 (melting point 218°C). The reaction is heated to vacuumize, the first stage reaction temperature is 230°C, and the reaction is continued to heat to the second stage reaction temperature of 270°C after 3h, and the reaction is carried out for 5h. Nitrogen is pressed, and the vacuum degree is 50Pa during the negative pressure reaction process to obtain the gas barrier polyamide elastomer material.

[0035] Example 2

[0036] S1. Preparation of dicarboxyl-terminated polyamide prepolymer

[0037] 3962.9g (23mol) of decanediamine, 5561.7g (24.15mol) of dodecanedioic acid and deionized water were stirred evenly and heated until clear, then added into a polymerization kettle, and the reaction was started after nitrogen replacement for 5 times; the temperature was raised to 210°C and the pressure was raised to 1.3MPa, and the pressure was maintained constant, and the temperature was continued to be raised to 230°C, and the pressure was reduced to normal pressure after 2h; after the normal pressure, the vacuum reaction was carried out, the vacuum degree was -0.05MPa, and the reaction time was 20min, and the product was obtained;

[0038] S2. Preparation of polyester oligomers containing naphthalene rings

[0039] 1728g (8mol) of 2,6-naphthalene dicarboxylic acid and 3200g (8mol) of polypropylene glycol with a molecular weight of 400 were added to a polymerization kettle, and 3.2g of isopropyl titanate was added. The mixture was heated to 100°C, and the negative pressure was maintained at 200Pa. The reaction was continued for 3h to obtain the product.

[0040] S3. Preparation of polyamide elastomer

[0041] The products of step S1 and S2, the dicarboxyl-terminated polyamide prepolymer, the polyester oligomer containing naphthalene rings, and 2300g (1.15mol) of polypropylene glycol with a molecular weight of 2000 are added to a polymerization kettle, and 8g of antioxidant 1010, 8.7g of heat stabilizer TBPT, and 18g of esterification reaction catalyst zinc acetate are added. Of the 18g of zinc acetate, 6g is embedded in the inner layer (thickness 300μm) made of PA610 (melting point 225°C), and 12g is embedded between the inner layer and the outer layer (thickness 300μm) made of PA1012 (melting point 193°C). The reaction is heated to vacuumize, the first stage reaction temperature is 210°C, and the reaction is continued after 3h to the second stage reaction temperature of 260°C. After 2h of reaction, nitrogen is injected to press the material, and the vacuum degree is 400Pa during the negative pressure reaction process to obtain the gas barrier polyamide elastomer material.

[0042] Example 3

[0043] S1. Preparation of dicarboxyl-terminated polyamide prepolymer

[0044] 3400g (17mol) of dodecanediamine, 5089.6g (22.1mol) of dodecanediacid and deionized water were stirred evenly and heated until clear, then added into a polymerization kettle, and the reaction was started after nitrogen replacement for 5 times; the temperature was raised to 210°C and the pressure was raised to 1.5MPa, and the pressure was maintained constant, and the temperature was continued to be raised to 230°C, and the pressure was reduced to normal pressure in 1h; after the normal pressure, the vacuum reaction was carried out, the vacuum degree was -0.05MPa, and the reaction time was 30min, and the product was obtained;

[0045] S2. Preparation of polyester oligomers containing naphthalene rings

[0046] Add 2376g (11mol) of 2,3-naphthalene dicarboxylic acid and 6600g (11mol) of polytetrahydrofuran diol with a molecular weight of 600 into a polymerization kettle, add 66g of magnesium acetate, heat to 100°C, maintain a negative pressure of 200Pa, and react for 3h to obtain;

[0047] S3. Preparation of polyamide elastomer

[0048] The products of step S1 and S2, the dicarboxyl-terminated polyamide prepolymer, the polyester oligomer containing naphthalene rings, and 4080g (5.1mol) of polytetrahydrofuran diol with a molecular weight of 800 are added to a polymerization kettle, and 20.6g of antioxidant 626, 25g of heat stabilizer organic phosphite, and 21g of esterification catalyst triisobutyl lithium are added. Of the 21g of triisobutyl lithium, 7g is embedded in the inner layer (thickness 400μm) made of PA610 (melting point 225°C), and 14g is embedded between the inner layer and the outer layer (thickness 400μm) made of PA1212 (melting point 185°C). The reaction is heated to vacuumize, the first stage reaction temperature is 210°C, and the reaction is continued after 3h to the second stage reaction temperature of 260°C. After 2h of reaction, nitrogen is injected to press the material, and the vacuum degree is 500Pa during the negative pressure reaction process to obtain the gas barrier polyamide elastomer material.

[0049] Example 4

[0050] S1. Preparation of dicarboxyl-terminated polyamide prepolymer

[0051] 3420g (15mol) of tetradecanediamine, 5424.3g (21mol) of tetradecanediacid and deionized water were stirred evenly and heated until clear, and then added into a polymerization kettle. After nitrogen replacement for 5 times, the reaction began; the temperature was raised to 200°C and the pressure was raised to 1.7MPa. The pressure was maintained constant, and the temperature was further raised to 220°C. The pressure was reduced and reduced to normal pressure in 1h; after the pressure was normal, the vacuum reaction was carried out, the vacuum degree was -0.05MPa, and the reaction time was 30min, and the product was obtained;

[0052] S2. Preparation of polyester oligomers containing naphthalene rings

[0053] Add 2592g (12mol) of 2,6-naphthalenedicarboxylic acid and 2400g (12mol) of polyethylene glycol with a molecular weight of 200 into a polymerization kettle, add 24g of antimony trioxide, heat to 100°C, maintain a negative pressure of 200Pa, and react for 3h to obtain;

[0054] S3. Preparation of polyamide elastomer

[0055] The products of step S1 and S2, the dicarboxyl-terminated polyamide prepolymer, the polyester oligomer containing naphthalene rings, and 6000g (6mol) of polytetrahydrofuran diol with a molecular weight of 1000 are added to a polymerization kettle, and 20g of antioxidant 1010, 24g of heat stabilizer Finnre-336, and 21g of esterification reaction catalyst dibutyltin oxide are added. Of the 21g of dibutyltin oxide, 7g is embedded in the inner layer (thickness 500μm) made of PA612 (melting point 218°C), and 14g is embedded between the inner layer and the outer capsule wall (thickness 500μm) made of PA1212 (melting point 185°C). The reaction is heated to vacuumize, the first stage reaction temperature is 200°C, and the reaction is continued to heat to the second stage reaction temperature of 250°C after 3h, and the reaction is carried out for 1h. Nitrogen is pressed, and the vacuum degree is 500Pa during the negative pressure reaction process to obtain the gas barrier polyamide elastomer material.

[0056] Example 5

[0057] S1. Preparation of dicarboxyl-terminated polyamide prepolymer

[0058] 1583g (10mol) nonanediamine, 2427g (12mol) sebacic acid and deionized water were stirred evenly and heated until clear, then added into a polymerization kettle, and the reaction was started after nitrogen replacement for 5 times; the temperature was raised to 230°C, the pressure to 1.6MPa, the pressure was maintained constant, the temperature was continued to be raised to 250°C, the pressure was started to be reduced, and it was reduced to normal pressure in 1h; after normal pressure, the vacuum reaction was carried out, the vacuum degree was -0.05MPa, and the reaction time was 30min, and the product was obtained;

[0059] S2. Preparation of polyester oligomers containing naphthalene rings

[0060] 1123.2g (5.2mol) of 2,6-naphthalene dicarboxylic acid and 2080g (5.2mol) of polypropylene glycol with a molecular weight of 400 were added to a polymerization kettle, and 20.8g of titanium dioxide was added. The mixture was heated to 100°C, and the negative pressure was maintained at 200Pa. The reaction was continued for 3h to obtain the product.

[0061] S3. Preparation of polyamide elastomer

[0062] The products of step S1 and S2, the dicarboxyl-terminated polyamide prepolymer, the polyester oligomer containing naphthalene rings, and 4000g (2mol) of polytetrahydrofuran diol with a molecular weight of 2000, are added to a polymerization kettle, and 20g of antioxidant 1010, 24g of heat stabilizer Finnre-336, and 24g of esterification reaction catalyst antimony acetate are added. Of the 24g of antimony acetate, 8g is embedded in an inner layer (thickness 300μm) made of PA66 (melting point 253°C), and 16g is embedded between the inner layer and the outer layer (thickness 300μm) made of PA1010 (melting point 203°C). The reaction is heated to vacuumize, the first stage reaction temperature is 230°C, and the reaction is continued after 3h to the second stage reaction temperature of 280°C. After 1h of reaction, nitrogen is injected to press the material, and the vacuum degree is 500Pa during the negative pressure reaction process to obtain the gas barrier polyamide elastomer material.

[0063] Comparative Example 1

[0064] The difference between Comparative Example 1 and Example 1 is that the 1,4-naphthalenedicarboxylic acid in step S2 is replaced with an equal molar number of dodecanedioic acid.

[0065] Comparative Example 2

[0066] The difference between Comparative Example 2 and Example 2 is that the 2,6-naphthalenedicarboxylic acid in step S2 is replaced with an equal molar number of dodecanedioic acid.

[0067] Comparative Example 3

[0068] The difference between Comparative Example 3 and Example 3 is only the method of adding the catalyst. In step S3, the catalyst is directly added without using nylon capsule wall for embedding.

[0069] Steps S1 and S2 are the same as those in Example 3, and step S3 is specifically as follows:

[0070] The products of step S1 and S2, the dicarboxyl-terminated polyamide prepolymer, the polyester oligomer containing naphthalene rings, and 4080g (5.1mol) of polytetrahydrofuran diol with a molecular weight of 800 are added to a polymerization kettle, and 20.6g of antioxidant 626, 25g of heat stabilizer organic phosphite, and 21g of esterification catalyst triisobutyl lithium are added. The reaction is heated to vacuumize, the reaction temperature is 210°C, and the temperature is continuously increased to 260°C after the reaction for 3h. After the reaction for 2h, the material is pressed with nitrogen, and the vacuum degree is 500Pa during the negative pressure reaction to obtain the amide elastomer material.

[0071] Performance Testing

[0072] The polyamide elastomer materials obtained in Examples 1 to 5 and Comparative Examples 1 to 2 were uniaxially stretched by extrusion to form a film with a thickness of 50 μm. The oxygen permeation rate and the carbon dioxide permeation rate were tested by the pressure difference method. The results are shown in Table 1.

[0073] Table 1 Test results of Examples 1 to 5 and Comparative Examples 1 to 2

[0074]

[0075] From the comparison of oxygen permeation and carbon dioxide permeation in Examples 1 to 5 and Comparative Examples 1 to 2, the oxygen permeation and carbon dioxide permeation data in Examples 1 to 5 are much smaller than those in Comparative Examples 1 to 2, and as the content of naphthalene dicarboxylic acid increases, the gas permeability gradually decreases, indicating that the addition of naphthalene dicarboxylic acid of the present invention improves the gas barrier properties of the material and can be used in the packaging industry.

[0076] The polyamide elastomer materials obtained in Example 3 and Comparative Example 3 were subjected to a melt index test (test standard: ISO1133). The results are shown in Table 2.

[0077] Table 2 Melt index test data of Example 3 and Comparative Example 3

[0078]

[0079] It can be seen from the data in the table that the melt index difference between Example 3 and Comparative Example 3 is large, which shows that under the same polymerization process, the release mode of the catalyst is different, resulting in different polymerization degrees. In addition, there are many light yellow particles in the polyamide elastomer prepared in Comparative Example 3, which are the residues after the hydrolysis of the catalyst. The deactivation of the catalyst affects the polymerization rate, resulting in a low polymerization degree.

Claims

1. A method for preparing a gas barrier polyamide elastomer material, It is characterized in that The following steps are involved: S1, preparing a dicarboxyl-terminated polyamide prepolymer, wherein the polyamide is a long carbon chain polyamide; S2, preparing a polyester oligomer containing naphthalene rings, which is prepared from naphthalene dicarboxylic acid and polyether diol; S3, a dicarboxyl-terminated polyamide prepolymer, a polyester oligomer containing a naphthalene ring, and a polyether diol are subjected to a polycondensation reaction under the action of a catalyst A to obtain a polyamide elastomer containing a naphthalene ring, which is the gas barrier polyamide elastomer material; Catalyst A is a capsule-type catalyst, comprising a heated and melted nylon capsule wall and an esterification reaction catalyst embedded in the nylon capsule wall; The nylon capsule wall includes an inner layer and an outer layer, which are made of nylon materials with different melting points. The melting point of the outer nylon capsule wall is 185-218°C, and the melting point of the inner nylon capsule wall is 218-253°C. The inner layer and between the inner layer and the outer layer are both embedded with an esterification reaction catalyst. The dicarboxyl-terminated polyamide prepolymer is prepared by polycondensation of dibasic acid and diamine; The amount of naphthalene dicarboxylic acid added is 10% to 20% of the total mass of the diamine and dibasic acid in step S1, the naphthalene dicarboxylic acid and polyether diol in step S2, and the polyether diol in step S3.

2. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that In step S1, the dibasic acid is selected from one of sebacic acid, dodecanedioic acid and tetradecanedioic acid, and the diamine is selected from one of hexanediamine, nonanediamine, decanediamine, dodecanediamine and tetradecanediamine.

3. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that In step S2, the naphthalene dicarboxylic acid is selected from one of 2,6-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, and 2,3-naphthalene dicarboxylic acid; the polyether diol is selected from one of polyethylene glycol, polypropylene glycol, and polytetrahydrofuran diol, and the number average molecular weight is 200-600.

4. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that In step S3, the polyether diol is selected from one of polyethylene glycol, polypropylene glycol, and polytetrahydrofuran diol, and has a number average molecular weight of 800-2000.

5. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that In step S3, the reaction temperature is 200-280°C, and the reaction is divided into two consecutive stages, the reaction temperature of the first stage is 200-230°C, and the reaction temperature of the second stage is 230-280°C; the reaction vacuum degree is 50-500 Pa, and the reaction time is 4-8h.

6. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that The esterification reaction catalyst is one or more of zinc acetate, magnesium acetate, antimony acetate, triisobutyl lithium, dibutyl tin oxide, titanium dioxide, antimony trioxide, butyl titanate, tetrabutyl zirconate, and isopropyl titanate.

7. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that The nylon capsule wall is made of nylon and has a thickness of 200~500μm.

8. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that The nylon material of the nylon capsule wall is selected from one of PA66, PA610, PA612, PA1010, PA1012, and PA1212.

9. The method for preparing the gas barrier polyamide elastomer material according to claim 1, It is characterized in that In step S1, the molar number of diamine is a, and the molar number of dibasic acid is b; in step S2, the molar number of naphthalene dicarboxylic acid is c, and the molar number of polyether diol is d; in step S3, the molar number of polyether diol is e; then b / a=1.02~1.4, c / d=1, a+d+e=b+c.

10. A gas barrier polyamide elastomer material, It is characterized in that Prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of nylon elastomer

    CN113968966A

  • High-temperature resistant nylon / PEN copolymer and preparation method as well as application thereof

    CN102618025A

  • High temperature-resistant nylon / polyethylenenaphthalate (PEN) / polyethylene glycol terephthalate (PBT) copolymer, and preparation method and application thereof

    CN102660018A