Copper alloy, copper alloy plate and preparation method thereof, copper alloy wire and preparation method thereof

By adding Mn, Al, B, Co and rare earth elements to copper alloys and adopting a specific preparation process, the problems of poor corrosion resistance and dezincification corrosion of copper alloys in environments with large sand content and fast water flow are solved, and the corrosion resistance is improved. Its corrosion resistance and formability in seawater make it suitable for aquaculture environments.

CN118563163BActive Publication Date: 2024-10-11CHINALCO RES INST OF SCI & TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410907205.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

Existing copper alloys have poor corrosion resistance in environments with large sand content and fast water flow. They suffer from serious dezincification corrosion problems, and their formability and strength match poorly during the processing and forming process.

Method used

By adding Mn, Al, B, Co and rare earth elements to copper alloys, micron and nanoscale precipitated phase structures are formed, and the composition and preparation process of copper alloys are optimized, including continuous casting, hot rolling, cold rolling, recrystallization annealing and removal. Stress annealing and other steps can improve its tensile strength, elongation and corrosion resistance.

Benefits of technology

It significantly improves the corrosion resistance and formability of copper alloys, reduces the processing difficulty of breeding equipment, and enables it to maintain excellent corrosion resistance and dezincification corrosion resistance in environments with high water flow rates and high sand content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563163B_ABST
    Figure CN118563163B_ABST
Patent Text Reader

Abstract

The present invention provides a copper alloy, a copper alloy plate and a preparation method thereof, a copper alloy wire and a preparation method thereof. In terms of mass percentage, the copper alloy comprises: 55-80% of Cu element, 1-5% of Mn element, 0.1-2% of Al element, 0.001-0.05% of B element, 0.1-2% of Co element, 0.01-0.15% of rare earth element and ≤0.05% of impurity element, and the balance is Zn element; wherein the rare earth element is selected from any one or more of Y, Ce, La, Pr, and Sc; the tensile strength of the copper alloy is ≥480MPa, and the elongation is ≥30%; under the test conditions of a flow rate of 2m / s and a sand content of 300mg / L, the corrosion rate of the copper alloy is ≤0.035mm / a. The above copper alloy is not only strong and tough, easy to process and form, but also suitable for aquaculture environments with large water flow rates and high sand content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of copper alloys, and in particular to a copper alloy, a copper alloy plate and a preparation method thereof, and a copper alloy wire and a preparation method thereof. Background Art

[0002] Copper alloys have natural antibacterial and anti-attachment effects in the marine environment, and copper alloy aquaculture devices can provide a cleaner and healthier water environment for the growth and reproduction of fish. Therefore, copper alloy aquaculture devices have been widely used in the field of fishery engineering, especially in cages and fence nets for marine aquaculture, and have achieved good results. Data show that by 2026, global fishery production will reach 200 million tons, of which aquaculture will be the main booster of fishery growth in the next 10 years. The main aquaculture growth will be in China, and its growth will reach 17 million tons, accounting for about 2 / 3 of the global aquaculture increase of 26 million tons. Copper alloys used in marine aquaculture devices need to have strong structure and corrosion resistance, so that the cages have good volume retention and long service life.

[0003] Seawater is a natural electrolyte solution because it is rich in salt, oxygen and other substances. Its corrosion to metals is manifested in the following ways: 1) Chloride ions and other halogen ions hinder and destroy the passivation of metals; 2) Local destruction of passivation will also increase the probability of pitting and crevice corrosion; 3) Oxygen, as a cathode depolarizer, can accelerate cathode reactions and thus the corrosion process; 4) Seawater corrosion has a low resistivity and is prone to galvanic corrosion when dissimilar metals come into contact. In flowing seawater, the corrosion rate of metals is faster than that of static corrosion. Generally speaking, the higher the relative speed, the more, harder and heavier the suspended solid particles in the fluid, and the more severe the erosion corrosion.

[0004] The corrosion rate of brass in the atmosphere is very slow, while the corrosion rate in pure fresh water is about 0.0025~0.025mm / a, and the corrosion rate in seawater is slightly faster, about 0.0075~0.1mm / a. The main reason is that the chloride in the water has a greater corrosion effect on brass, especially in water containing gases such as O2, CO2, H2S, SO2 and NH3, the corrosion rate of brass will increase dramatically. At present, brass alloys generally have the problem of dezincification corrosion during use. The aquaculture devices made of them are damaged during use due to the selective dissolution of zinc elements, which leads to the failure of zinc elements, and then the corrosion of aquaculture devices made of brass alloys is aggravated. Summary of the invention

[0005] The main purpose of the present invention is to provide a copper alloy, a copper alloy plate and a preparation method thereof, a copper alloy wire and a preparation method thereof, so as to solve the problems in the prior art of poor corrosion resistance of copper alloys in environments with high sand content and fast water flow, severe dezincification corrosion, and poor forming performance and strength matching of copper alloys during processing and forming.

[0006] In order to achieve the above object, according to one aspect of the present invention, a copper alloy is provided. In terms of mass percentage, the copper alloy comprises: 55-80% of Cu element, 1-5% of Mn element, 0.1-2% of Al element, 0.001-0.05% of B element, 0.1-2% of Co element, 0.01-0.15% of rare earth element and ≤0.05% of impurity element, and the balance is Zn element; wherein the rare earth element is selected from any one or more of Y, Ce, La, Pr, and Sc; the tensile strength of the copper alloy is ≥480MPa, and the elongation of the copper alloy is ≥30%; under the test conditions of a flow rate of 2m / s and a sand content of 300mg / L, the corrosion rate of the copper alloy is ≤0.035mm / a.

[0007] Furthermore, the copper alloy comprises, in terms of mass percentage, 65-75% of Cu element, 2-4% of Mn element, 0.5-1% of Al element, 0.001-0.02% of B element, 0.5-1.5% of Co element, 0.01-0.15% of rare earth element and ≤0.05% of impurity element, with the remainder being Zn element; and / or the mass ratio of Mn element to Al element is 2-4:0.5-1, and / or the mass ratio of B element to Co element is 0.001-0.02:0.5-1.5.

[0008] Furthermore, the recrystallization texture content of the copper alloy is 10-30%, and / or the dislocation density of the copper alloy is 1-10×10 -9 cm -2 , and / or the average grain size of the copper alloy is 5~60μm.

[0009] According to another aspect of the present invention, there is provided a method for preparing the copper alloy, which is a copper alloy sheet, and the preparation method comprises: step S11, performing a first batching according to the raw materials corresponding to the copper alloy and then performing a first continuous casting to obtain a copper alloy slab; step S21, hot rolling, cooling and milling the copper alloy slab in sequence to obtain a copper alloy slab after milling; step S31, rough rolling and first recrystallization annealing are performed on the copper alloy slab after milling in sequence to obtain a copper plate; step S41, finish rolling the copper plate to obtain a finish rolled copper plate; step S51, first alkali washing and stress relief annealing are performed on the finish rolled copper plate in sequence to obtain a copper alloy sheet; wherein the melting temperature of the first continuous casting is 1070~1170℃; the starting rolling temperature of hot rolling is 800~900℃; the final rolling temperature of hot rolling is 550~620℃; the temperature of the first recrystallization annealing is 400~650℃; the temperature of the stress relief annealing is 300~350℃.

[0010] Furthermore, in the above step S11, the first continuous casting is carried out under non-vacuum conditions by horizontal continuous casting, and / or the insulation temperature of the first continuous casting is 1000~1100°C, and / or the insulation time of the first continuous casting is 10~30min, and / or the casting speed of the first continuous casting is 10~200mm / min; and / or the first covering agent is added during the first continuous casting, and / or the first covering agent is charcoal and / or cryolite, and / or the thickness of the copper alloy slab is 100~150mm.

[0011] Furthermore, in the above step S21, the copper alloy slab is hot rolled to obtain a hot-rolled plate, and / or the deformation amount of hot rolling is 90-95%, and / or the thickness of the hot-rolled plate is 10-15 mm, and / or the thickness of the copper alloy slab after milling is 8-10 mm.

[0012] Further, in the above step S31, the rough rolling includes three cold rolling passes, the three cold rolling passes include a first cold rolling pass, a second cold rolling pass and a third cold rolling pass performed sequentially, and / or the total deformation of the rough rolling is 70~80%, and / or the deformation of the first cold rolling pass is 30~50%, and / or the deformation of the second cold rolling pass is 35~45%, and / or the deformation of the third cold rolling pass is 20~40%; and / or the first recrystallization annealing is performed 1~2 times during the rough rolling process, and / or the thickness of the copper plate is 1.5~3mm; and / or in the above step S41, the deformation of the finish rolling is 5~10%, and / or the thickness of the copper plate after the finish rolling is 1~2mm; and / or in the above step S51, the thickness of the copper alloy plate is 1~2mm.

[0013] According to another aspect of the present invention, there is provided a copper alloy plate material prepared by the above-mentioned preparation method.

[0014] According to another aspect of the present invention, there is provided a method for preparing the copper alloy, which is a copper alloy wire, and the preparation method comprises: step S21, performing a second batching according to the raw materials corresponding to the copper alloy and then performing a second continuous casting to obtain a copper alloy wire billet; step S22, performing a first stretching on the copper alloy wire billet to obtain a first wire billet; step S23, performing a second recrystallization annealing, pickling, a second stretching and a second alkali washing on the first wire billet in sequence to obtain a copper alloy wire; wherein the melting temperature of the second continuous casting is 1050~1150℃; and the temperature of the second recrystallization annealing is 350~550℃.

[0015] Furthermore, in the above step S21, under non-vacuum conditions, the second continuous casting is carried out by the upward continuous casting method, and / or the holding temperature of the second continuous casting is 950~1050℃, and / or the holding time of the second continuous casting is 10~30min, and / or the casting speed of the second continuous casting is 2.5~3.5m / min; and / or the second covering agent is added during the second continuous casting, and / or the second covering agent is charcoal and / or cryolite; and / or cooling water is used for cooling after the second continuous casting, the temperature of the cooling water is 20~35℃, the flow rate of the cooling water is 18~35L / min, and / or the diameter of the copper alloy wire billet is φ10~φ20mm.

[0016] Furthermore, in the above step S22, the deformation amount of the first stretching is 20%~80%, and / or the diameter of the first wire blank is φ8~φ15mm; and / or in the above step S23, the deformation amount of the second stretching is 20%~90%, and / or the diameter of the copper alloy wire is φ3~φ10mm.

[0017] According to another aspect of the present invention, there is provided a copper alloy wire, which is prepared by the above-mentioned preparation method.

[0018] By applying the technical solution of the present invention, the present application adds alloying elements such as Mn, Al, B, Co and rare earth elements to the Cu-Zn binary alloy through an alloying method, which not only enables the copper alloy to have micron and nanoscale precipitation phase structures of different sizes, and dispersedly distributes them in the Cu-Zn alloy matrix, thereby slowing down dezincification corrosion and effectively improving the strength and erosion corrosion resistance of the copper alloy, but also optimizes the forming performance of the copper alloy, thereby reducing the processing difficulty of aquaculture device products. Among them, adding Mn element to the alloy can distort the copper lattice of the copper alloy during the solid solution strengthening process, thereby improving the corrosion resistance of the copper alloy in seawater and chlorides; adding Al element can not only significantly improve the strength and corrosion resistance of the copper alloy, but also form a dense and hard Al2O3 film, thereby blocking the corrosion of the matrix. Even in flowing seawater, the copper alloy can still resist the impact and friction of seawater; adding B element can not only effectively modify and refine the structure of the copper alloy, but also occupy the vacancies in the passivation layer generated after dezincification and prevent the migration of zinc atoms, thereby improving the corrosion resistance of the copper alloy; adding Co element can not only reduce the grain size of the cast copper alloy and change the grain shape, but also simultaneously improve the strength and ductility of the copper alloy; controlling the content and type of rare earth elements within the above range can not only effectively deoxidize, dehydrogenate and remove impurity elements, but also improve the fluidity of the melt, thereby improving the corrosion resistance of the copper alloy. The present invention mixes the above elements in different types and contents to obtain a copper alloy that is not only strong and tough, easy to process and form, but also has good matching between forming performance and strength. It can also be used in aquaculture environments with high water flow rates and high sand content, and maintains excellent corrosion resistance and anti-dezincification corrosion performance in the above aquaculture environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0020] Figure 1 The microstructure diagram of the copper alloy in Example 1 of the present application is shown. DETAILED DESCRIPTION

[0021] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0022] As analyzed in the background technology of the present application, the prior art has problems such as poor corrosion resistance of copper alloys in environments with high sand content and fast water flow, severe dezincification corrosion, and poor matching of forming performance and strength of copper alloys during processing and forming. In order to solve the above problems, the present application provides a copper alloy, a copper alloy plate and a preparation method thereof, and a copper alloy wire and a preparation method thereof.

[0023] In a typical embodiment of the present application, a copper alloy is provided, which includes, by mass percentage, 55-80% of Cu element, 1-5% of Mn element, 0.1-2% of Al element, 0.001-0.05% of B element, 0.1-2% of Co element, 0.01-0.15% of rare earth element and ≤0.05% of impurity element, and the balance is Zn element; wherein the rare earth element is selected from any one or more of Y, Ce, La, Pr, and Sc; the tensile strength of the copper alloy is ≥480MPa, and the elongation of the copper alloy is ≥30%; under the test conditions of a flow rate of 2m / s and a sand content of 300mg / L, the corrosion rate of the copper alloy is ≤0.035mm / a.

[0024] The present application adds alloying elements such as Mn, Al, B, Co and rare earth elements to the Cu-Zn binary alloy through an alloying method, which not only enables the copper alloy to have micrometer and nanometer precipitate phase structures of different sizes and dispersedly distributes them in the Cu-Zn alloy matrix, thereby slowing down dezincification corrosion and effectively improving the strength and erosion corrosion resistance of the copper alloy, but also optimizes the forming performance of the copper alloy, thereby reducing the processing difficulty of aquaculture device products. Among them, adding Mn element to the alloy can distort the copper lattice of the copper alloy during the solid solution strengthening process, thereby improving the corrosion resistance of the copper alloy in seawater and chlorides; adding Al element can not only significantly improve the strength and corrosion resistance of the copper alloy, but also form a dense and hard Al2O3 film, thereby blocking the corrosion of the matrix. Even in flowing seawater, the copper alloy can still resist the impact and friction of seawater; adding B element can not only effectively modify and refine the structure of the copper alloy, but also occupy the vacancies in the passivation layer generated after dezincification and prevent the migration of zinc atoms, thereby improving the corrosion resistance of the copper alloy; adding Co element can not only reduce the grain size of the cast copper alloy and change the grain shape, but also simultaneously improve the strength and ductility of the copper alloy; controlling the content and type of rare earth elements within the above range can not only effectively deoxidize, dehydrogenate and remove impurity elements, but also improve the fluidity of the melt, thereby improving the corrosion resistance of the copper alloy. The present invention mixes the above elements in different types and contents to obtain a copper alloy that is not only strong and tough, easy to process and form, but also has good matching between forming performance and strength. It can also be used in aquaculture environments with high water flow rates and high sand content, and maintains excellent corrosion resistance and anti-dezincification corrosion performance in the above aquaculture environments.

[0025] In one embodiment of the present application, the copper alloy comprises, by mass percentage: 65-75% of Cu element, 2-4% of Mn element, 0.5-1% of Al element, 0.001-0.02% of B element, 0.5-1.5% of Co element, 0.01-0.15% of rare earth element and ≤0.05% of impurity element, and the balance is Zn element; and / or the mass ratio of Mn element to Al element is 2-4:0.5-1, and / or the mass ratio of B element to Co element is 0.001-0.02:0.5-1.5.

[0026] It is further preferred that the types and contents of elements in the copper alloy are within the above-mentioned range, which helps to improve the synergistic effect between the elements, thereby further improving the strength, erosion corrosion resistance and formability of the copper alloy; wherein, it is preferred to control the mass ratio of the Mn element and the Al element within the above-mentioned range, which helps to enhance the effects of solid solution strengthening and precipitation strengthening, thereby further improving the strength and erosion corrosion resistance of the copper alloy; it is preferred to control the mass ratio of the B element and the Co element within the above-mentioned range, which helps to refine the microstructure of the copper alloy, thereby making the grain size of the copper alloy reach below 60 μm.

[0027] In one embodiment of the present application, the recrystallization texture content of the copper alloy is 10-30%, and / or the dislocation density of the copper alloy is 1-10×10 -9 cm -2 , and / or the average grain size of the copper alloy is 5~60μm.

[0028] Controlling the recrystallization texture content, dislocation density and average grain size of the copper alloy within the above ranges helps to form a sufficient recrystallization structure and a lower dislocation density, thereby further improving the density of the surface product film after corrosion of the copper alloy, thereby improving the erosion corrosion resistance of the copper alloy.

[0029] In another typical embodiment of the present application, a preparation method of the above-mentioned copper alloy is provided, and the copper alloy is a copper alloy plate, and the preparation method comprises: step S11, performing a first batching according to the raw materials corresponding to the above-mentioned copper alloy and then performing a first continuous casting to obtain a copper alloy slab; step S21, hot rolling, cooling and milling the copper alloy slab in sequence to obtain a copper alloy slab after milling; step S31, rough rolling and first recrystallization annealing are performed on the copper alloy slab after milling in sequence to obtain a copper plate; step S41, finish rolling the copper plate to obtain a finish-rolled copper plate; step S51, first alkali washing and stress relief annealing are performed on the finish-rolled copper plate in sequence to obtain a copper alloy plate; wherein, the melting temperature of the first continuous casting is 1070~1170℃; the starting rolling temperature of hot rolling is 800~900℃; the final rolling temperature of hot rolling is 550~620℃; the temperature of the first recrystallization annealing is 400~650℃; the temperature of the stress relief annealing is 300~350℃.

[0030] The present invention controls the composition of the copper alloy raw material within the above range for the first batching, and can fully utilize the strengthening effect of the alloy elements. Preferably, the melting temperature of the first continuous casting is controlled within the above range, which helps the alloy elements to fully melt and diffuse evenly, thereby obtaining a continuous casting billet with uniform composition. It is preferred to control the starting rolling temperature and the final rolling temperature of hot rolling within the above range, which is conducive to the full solid solution of the alloy elements in the matrix, thereby obtaining a hot-rolled plate with a large solid solubility; the copper alloy slab after milling is subjected to multiple rough rolling, which can greatly reduce the cross-sectional size of the copper alloy slab after milling, and it is preferred to control the temperature of the first recrystallization annealing within the above range, which is conducive to alloy recrystallization and promotes the precipitation phase to be fully separated out, thereby obtaining a copper plate with good toughness; the copper plate is subjected to fine rolling, which can not only accurately control the thickness of the copper plate and improve the surface quality of the copper plate, but also improve the strength and toughness of the copper plate; the copper plate after fine rolling is subjected to the first alkali washing, which can remove surface pollutants and improve surface activity, thereby improving the corrosion resistance of the copper alloy plate; the copper plate after fine rolling is subjected to stress relief annealing, which can eliminate internal stress, thereby improving the stability of the copper alloy plate and improving the processing performance of the copper alloy plate. The copper alloy plate prepared by the above process of the present invention has sufficient recrystallization structure and low dislocation density, and has excellent strength, erosion corrosion resistance and forming performance.

[0031] In one embodiment of the present application, in the above-mentioned step S11, the first continuous casting is performed under non-vacuum conditions by horizontal continuous casting, and / or the insulation temperature of the first continuous casting is 1000~1100℃, and / or the insulation time of the first continuous casting is 10~30min, and / or the casting speed of the first continuous casting is 10~200mm / min; and / or the first covering agent is added during the first continuous casting, and / or the first covering agent is charcoal and / or cryolite, and / or the thickness of the copper alloy slab is 100~150mm.

[0032] Preferably, the first continuous casting is carried out in a horizontal continuous casting manner under non-vacuum conditions, which is helpful in producing copper alloy slabs with good surface quality and uniform internal structure; preferably, the holding temperature, holding time and casting speed of the first continuous casting are within the above ranges, which is helpful in optimizing the grain size and recrystallization texture of the copper alloy slab, thereby helping to improve the surface quality, strength and other properties of the copper alloy slab; preferably, charcoal and / or cryolite are added as the first covering agent during the first continuous casting process, which not only helps to inhibit the oxidation of the molten metal during the first continuous casting process, but also helps to improve the uniformity of the internal structure of the copper alloy slab; preferably, the thickness of the copper alloy slab is within the above range, which is helpful for subsequent hot rolling.

[0033] In one embodiment of the present application, the copper alloy slab is hot rolled to obtain a hot-rolled plate, and / or the deformation of the hot rolling is 90~95%, and / or the thickness of the hot-rolled plate is 10~15mm, and / or the thickness of the copper alloy slab after milling is 8~10mm.

[0034] Preferably, controlling the deformation amount of hot rolling within the above range helps to refine the grains and improve the texture, thereby improving the surface quality of the copper alloy slab after milling, and further obtaining a hot-rolled plate with a thickness within the above range; preferably, double-sided milling is used to obtain the copper alloy slab after milling with a thickness within the above range, which helps to improve the surface quality of the copper alloy slab after milling, thereby facilitating rough rolling.

[0035] In one embodiment of the present application, in the above-mentioned step S31, the rough rolling includes three cold rolling passes, the three cold rolling passes include a first cold rolling pass, a second cold rolling pass and a third cold rolling pass performed sequentially, and / or the total deformation of the rough rolling is 70~80%, and / or the deformation of the first cold rolling pass is 30~50%, and / or the deformation of the second cold rolling pass is 35~45%, and / or the deformation of the third cold rolling pass is 20~40%; and / or the first recrystallization annealing is performed 1~2 times during the rough rolling process, and / or the thickness of the copper plate is 1.5~3mm; and / or in the above-mentioned step S41, the deformation of the finish rolling is 5~10%, and / or the thickness of the copper plate after the finish rolling is 1~2mm; and / or in the above-mentioned step S51, the thickness of the copper alloy plate is 1~2mm.

[0036] Preferably, the rough rolling includes three cold rolling passes and the total deformation of the rough rolling, the deformation of the first cold rolling, the second cold rolling and the third cold rolling are controlled within the above range, which helps to gradually control the size and shape of the copper alloy slab after milling, and obtain a copper plate with a thickness within the above range; preferably, 1 to 2 first recrystallization annealings are performed during the rough rolling process, and it is further preferred to perform the first recrystallization annealing after the second cold rolling, so as to make full use of the deformation energy storage to promote the precipitation of the second phase particles from the matrix, thereby improving the strength of the copper plate. Preferably, the deformation of the finish rolling is controlled, which helps to obtain a copper plate after finish rolling with a thickness within the above range. Controlling the temperature of the stress relief annealing within the above range helps to eliminate internal stress, thereby improving the processing performance of the copper alloy sheet; preferably, the thickness of the copper alloy sheet is within the above range, which is more conducive to use as a copper alloy material for aquaculture devices.

[0037] In another typical embodiment of the present application, a copper alloy plate is provided, which is prepared by the above-mentioned preparation method.

[0038] The copper alloy plate prepared by the above preparation method not only has sufficient recrystallization structure and low dislocation density, but also has excellent strength, erosion corrosion resistance and formability.

[0039] In another typical embodiment of the present application, a preparation method of the above-mentioned copper alloy is provided, and the copper alloy is a copper alloy wire, and the preparation method comprises: step S21, performing a second batching according to the raw materials corresponding to the above-mentioned copper alloy and then performing a second continuous casting to obtain a copper alloy wire billet; step S22, performing a first stretching on the copper alloy wire billet to obtain a first wire billet; step S23, performing a second recrystallization annealing, pickling, a second stretching, and a second alkali washing on the first wire billet in sequence, and deforming the first wire billet to obtain a copper alloy wire; wherein the melting temperature of the second continuous casting is 1050~1150℃; and the temperature of the second recrystallization annealing is 350~550℃.

[0040] The present invention can make full use of the strengthening effect of alloy elements by controlling the composition of copper alloy raw materials within the above range for the second batching. It is preferred to control the melting temperature of the second continuous casting within the above range, which is conducive to the full melting and uniform diffusion of alloy elements, thereby obtaining a melt with uniform composition; the copper alloy wire billet is subjected to the first stretching, which can not only significantly reduce the diameter of the first wire billet, but also rearrange the internal grains of the first wire billet along the stretching direction to form a fibrous structure, thereby improving the tensile strength and elasticity of the first wire billet; it is preferred to control the temperature of the second recrystallization annealing within the above range, which is conducive to making full use of deformation energy storage to promote the precipitation of second phase particles from the matrix, thereby further improving the strength of the copper alloy wire; the first wire billet is pickled, which can not only remove the oxide layer and impurities on the surface of the first wire billet, but also help to perform the second stretching; the first wire billet is pickled and then subjected to the second stretching, which can not only further control the diameter of the copper alloy wire, but also improve the tensile strength and elasticity of the copper alloy wire. The first wire blank is subjected to a first alkali wash to remove surface pollutants of the high copper alloy wire and improve the surface activity of the copper alloy wire, thereby improving the corrosion resistance of the copper alloy sheet. The copper alloy wire prepared by the above process of the present invention has a sufficient recrystallized structure and a low dislocation density, and has excellent strength, erosion corrosion resistance and forming performance.

[0041] In one embodiment of the present application, in the above-mentioned step S21, under non-vacuum conditions, the second continuous casting is carried out by the upward continuous casting method, and / or the holding temperature of the second continuous casting is 950~1050℃, and / or the holding time of the second continuous casting is 10~30min, and / or the casting speed of the second continuous casting is 2.5~3.5m / min; and / or the second covering agent is added during the second continuous casting, and / or the second covering agent is charcoal and / or cryolite; and / or cooling water is used for cooling after the second continuous casting, the temperature of the cooling water is 20~35℃, the flow rate of the cooling water is 18~35L / min, and / or the diameter of the copper alloy wire billet is φ10~φ20mm.

[0042] It is preferred that the second continuous casting is carried out in an upward continuous casting manner under non-vacuum conditions, which is helpful in producing copper alloy wire billets with good surface quality and dense internal structure; it is preferred that the holding temperature, holding time and casting speed of the second continuous casting are within the above range, which is helpful in optimizing the grain size and recrystallization texture of the copper alloy wire billet, thereby helping to improve the surface quality, strength and other properties of the copper alloy wire billet; it is preferred that charcoal and / or cryolite be added as a second covering agent during the second continuous casting process, which not only helps to inhibit the oxidation of the molten metal during the second continuous casting process, but also helps to improve the internal structure uniformity of the copper alloy wire billet; it is preferred that cooling water is used for cooling after the second continuous casting, and the temperature and flow rate of the cooling water are controlled within the above range, which is helpful in controlling the solidification rate of the copper alloy wire billet, thereby helping the copper alloy to form a dense internal structure, and further improving the surface quality, strength and other properties of the copper alloy wire billet; it is preferred that the diameter of the copper alloy wire billet is within the above range, which is helpful for the subsequent first stretching.

[0043] In one embodiment of the present application, in the above step S22, the deformation amount of the first stretching is 20%~80%, and / or the diameter of the first wire blank is φ8~φ15mm; and / or in the above step S23, the deformation amount of the second stretching is 20%~90%, and / or the diameter of the copper alloy wire is φ3~φ10mm.

[0044] Controlling the deformation amount of the first stretching within the above-mentioned range helps to improve the tensile strength and toughness of the first wire billet, and obtain the first wire billet with a diameter within the above-mentioned range; at the same time, controlling the deformation amount of the second stretching within the above-mentioned range helps to further improve the tensile strength and toughness of the copper alloy wire, and obtain the copper alloy wire with a diameter within the above-mentioned range, making it more suitable for use as a copper alloy material for aquaculture devices.

[0045] In another typical embodiment of the present application, a copper alloy wire is provided, which is prepared by the above-mentioned preparation method.

[0046] The copper alloy wire prepared by the above preparation method not only has sufficient recrystallization structure and low dislocation density, but also has excellent strength, erosion corrosion resistance and formability.

[0047] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.

[0048] Example 1

[0049] In terms of mass percentage, the copper alloy raw material is made into a second batching and a second continuous casting according to Cu: 65%, Mn: 4%, B: 0.02%, rare earth element La: 0.15%, Co: 1.5%, Al: 0.5% and impurity elements ≤ 0.05%, and the balance is Zn, and a φ14.4mm copper alloy wire billet is obtained; wherein, the second continuous casting is carried out under non-vacuum conditions by an upward continuous casting method, the melting temperature of the second continuous casting is 1150°C, the holding temperature of the second continuous casting is 1050°C, the holding time of the second continuous casting is 10min, the casting speed of the second continuous casting is 2.5m / min, and the second covering agent charcoal is added during the second continuous casting, and cooling water is used for cooling, the temperature of the cooling water is 25°C, and the flow rate of the cooling water is 35L / min. The copper alloy wire billet is first stretched to obtain a φ10mm first wire billet, wherein the deformation of the first stretching is 52%. The first wire billet is subjected to second recrystallization annealing, pickling, second stretching and second alkali washing in sequence to obtain a φ8 mm copper alloy wire, wherein the temperature of the second recrystallization annealing is 350° C. and the deformation amount of the second stretching is 36%.

[0050] Example 2

[0051] In terms of mass percentage, the copper alloy raw material is made into a second batching and a second continuous casting according to Cu: 70%, Mn: 3%, B: 0.001%, rare earth element La: 0.08%, Co: 1%, Al: 0.7% and impurity elements ≤ 0.05%, and the balance is Zn, and a φ14.4mm copper alloy wire billet is obtained; wherein, the second continuous casting is carried out under non-vacuum conditions by an upward continuous casting method, the melting temperature of the second continuous casting is 1050°C, the holding temperature of the second continuous casting is 950°C, the holding time of the second continuous casting is 30min, the casting speed of the second continuous casting is 3.5m / min, and the second covering agent cryolite is added during the second continuous casting, and cooling water is used for cooling, the temperature of the cooling water is 35°C, and the flow rate of the cooling water is 20L / min. The copper alloy wire billet is first stretched to obtain a φ10mm first wire billet, wherein the deformation of the first stretching is 52%. The first wire billet is subjected to second recrystallization annealing, pickling, second stretching and second alkali washing in sequence to obtain a φ8 mm copper alloy wire, wherein the temperature of the second recrystallization annealing is 500° C. and the deformation amount of the second stretching is 36%.

[0052] Example 3

[0053] In terms of mass percentage, the copper alloy raw material is made into a second batching and a second continuous casting according to Cu: 75%, Mn: 2%, B: 0.01%, rare earth element La: 0.01%, Co: 0.5%, Al: 1% and impurity elements ≤ 0.05%, and the balance is Zn, and a φ14.4mm copper alloy wire billet is obtained; wherein, the second continuous casting is carried out under non-vacuum conditions by an upward continuous casting method, the melting temperature of the second continuous casting is 1100°C, the holding temperature of the second continuous casting is 1000°C, the holding time of the second continuous casting is 20min, the casting speed of the second continuous casting is 3m / min, and the second covering agent cryolite is added during the second continuous casting, and cooling water is used for cooling, the temperature of the cooling water is 30°C, and the flow rate of the cooling water is 25L / min. The copper alloy wire billet is first stretched to obtain a φ10mm first wire billet, wherein the deformation of the first stretching is 52%. The first wire billet is subjected to second recrystallization annealing, pickling, second stretching and second alkali washing in sequence to obtain a φ8 mm copper alloy wire, wherein the temperature of the second recrystallization annealing is 550° C. and the deformation amount of the second stretching is 36%.

[0054] Example 4

[0055] The copper alloy raw materials are prepared according to the mass percentage of Cu: 65%, Mn: 4%, B: 0.02%, rare earth elements La: 0.15%, Co: 1.5%, Al: 0.5% and impurity elements ≤0.05%, and the balance is Zn, and the first batching and the first continuous casting are carried out to obtain a copper alloy slab with a thickness of 100 mm; wherein, the first continuous casting is carried out under non-vacuum conditions by horizontal continuous casting, the melting temperature of the first continuous casting is 1170°C, the holding temperature of the first continuous casting is 1100°C, the holding time of the first continuous casting is 10 min, the casting speed of the first continuous casting is 200 mm / min, and the first covering agent cryolite is added during the first continuous casting.

[0056] The copper alloy slab was hot rolled to obtain a hot rolled plate with a thickness of 10 mm, and then cooled and milled to obtain a milled copper alloy slab with a thickness of 8 mm, wherein the hot rolling start temperature was 900°C, the hot rolling final rolling temperature was 620°C, and the hot rolling deformation was 90%. The milled copper alloy slab was rough rolled and subjected to the first recrystallization annealing to obtain a copper plate with a thickness of 1.6 mm, wherein the rough rolling process was subjected to three cold rolling deformations, the total deformation of the rough rolling was 80%, the deformation of the first cold rolling was 50%, the deformation of the second cold rolling was 37.5%, and the deformation of the third cold rolling was 36%; after the second cold rolling, a first recrystallization annealing was performed under the protection of 75% nitrogen and 25% hydrogen, and the temperature of the first recrystallization annealing was 650°C.

[0057] The copper plate is finish-rolled to obtain a finish-rolled copper plate with a thickness of 1.5 mm, wherein the deformation amount of the finish rolling is 6.25%.

[0058] The copper plate after fine rolling was subjected to a first alkali washing to remove oil stains on the surface of the sample, and then stress relief annealing was performed under nitrogen protection to obtain a copper alloy plate with a thickness of 1.5 mm, wherein the temperature of the stress relief annealing was 350°C.

[0059] Example 5

[0060] The copper alloy raw materials are prepared according to the mass percentage of Cu: 70%, Mn: 3%, B: 0.001%, rare earth elements La: 0.08%, Co: 1%, Al: 0.7% and impurity elements ≤0.05%, and the balance is Zn, and the first batching and the first continuous casting are carried out to obtain a copper alloy slab with a thickness of 100 mm; wherein, the first continuous casting is carried out under non-vacuum conditions by horizontal continuous casting, the melting temperature of the first continuous casting is 1070°C, the holding temperature of the first continuous casting is 1000°C, the holding time of the first continuous casting is 30min, the casting speed of the first continuous casting is 10mm / min, and the first covering agent charcoal is added during the first continuous casting.

[0061] The copper alloy slab was hot rolled to obtain a hot rolled plate with a thickness of 10 mm, and then cooled and milled to obtain a milled copper alloy slab with a thickness of 8 mm, wherein the hot rolling start temperature was 800°C, the hot rolling final rolling temperature was 550°C, and the hot rolling deformation was 90%. The milled copper alloy slab was rough rolled and subjected to the first recrystallization annealing to obtain a copper plate with a thickness of 1.6 mm, wherein the rough rolling process was subjected to three cold rolling deformations, the total deformation of the rough rolling was 80%, the deformation of the first cold rolling was 50%, the deformation of the second cold rolling was 37.5%, and the deformation of the third cold rolling was 36%; after the second cold rolling, a first recrystallization annealing was performed under the protection of 75% nitrogen and 25% hydrogen, and the temperature of the first recrystallization annealing was 400°C.

[0062] The copper plate is finish-rolled to obtain a finish-rolled copper plate with a thickness of 1.5 mm, wherein the deformation amount of the finish rolling is 6.25%.

[0063] The copper plate after fine rolling was subjected to a first alkali washing to remove oil stains on the surface of the sample, and then stress relief annealing was performed under nitrogen protection to obtain a copper alloy plate with a thickness of 1.5 mm, wherein the temperature of the stress relief annealing was 300°C.

[0064] Example 6

[0065] The copper alloy raw materials are prepared according to the mass percentage of Cu: 75%, Mn: 2%, B: 0.01%, rare earth element La: 0.01%, Co: 0.5%, Al: 1% and impurity elements ≤0.05%, and the balance is Zn, and the first batching and the first continuous casting are carried out to obtain a copper alloy slab with a thickness of 100 mm; wherein, the first continuous casting is carried out under non-vacuum conditions by horizontal continuous casting, the melting temperature of the first continuous casting is 1120°C, the holding temperature of the first continuous casting is 1050°C, the holding time of the first continuous casting is 20min, the casting speed of the first continuous casting is 100mm / min, and the first covering agent charcoal is added during the first continuous casting.

[0066] The copper alloy slab was hot rolled to obtain a hot rolled plate with a thickness of 10 mm, and then cooled and milled to obtain a milled copper alloy slab with a thickness of 8 mm, wherein the hot rolling start temperature was 850°C, the hot rolling final rolling temperature was 600°C, and the hot rolling deformation was 90%. The milled copper alloy slab was rough rolled and subjected to the first recrystallization annealing to obtain a copper plate with a thickness of 1.6 mm, wherein the rough rolling process was subjected to three cold rolling deformations, the total deformation of the rough rolling was 80%, the deformation of the first cold rolling was 50%, the deformation of the second cold rolling was 37.5%, and the deformation of the third cold rolling was 36%; after the second cold rolling, a first recrystallization annealing was performed under the protection of 75% nitrogen and 25% hydrogen, and the temperature of the first recrystallization annealing was 500°C.

[0067] The copper plate is finish-rolled to obtain a finish-rolled copper plate with a thickness of 1.5 mm, wherein the deformation amount of the finish rolling is 6.25%.

[0068] The copper plate after fine rolling was subjected to a first alkali washing to remove oil stains on the surface of the sample, and then stress relief annealing was performed under nitrogen protection to obtain a copper alloy plate with a thickness of 1.5 mm, wherein the temperature of the stress relief annealing was 325°C.

[0069] Example 7

[0070] The difference from Example 5 is that, in terms of mass percentage, the copper alloy raw material is made into Cu: 55%, Mn: 1%, B: 0.05%, rare earth element La: 0.05%, Co: 2%, Al: 0.1% and impurity elements ≤ 0.05%, and the balance is Zn, and finally a copper alloy sheet is obtained.

[0071] Example 8

[0072] The difference from Example 5 is that, in terms of mass percentage, the copper alloy raw material is made into Cu: 80%, Mn: 5%, B: 0.001%, rare earth element La: 0.1%, Co: 0.1%, Al: 2% and impurity elements ≤ 0.05%, and the balance is Zn, and finally a copper alloy sheet is obtained.

[0073] Example 9

[0074] The difference from Example 5 is that the mass content of Mn is 1%, the mass content of Al is 0.5%, the mass ratio of Mn to Al is 2:1, and finally a copper alloy sheet is obtained.

[0075] Example 10

[0076] The difference from Example 5 is that the mass content of Mn is 4%, the mass content of Al is 0.5%, the mass ratio of Mn to Al is 4:0.5, and finally a copper alloy sheet is obtained.

[0077] Embodiment 11

[0078] The difference from Example 5 is that the mass content of Mn is 1.85%, the mass content of Al is 1.85%, the mass ratio of Mn to Al is 1:1, and finally a copper alloy sheet is obtained.

[0079] Example 12

[0080] The difference from Example 2 is that the mass content of B is 0.02%, the mass content of Co is 0.5%, the mass ratio of B to Co is 0.02:0.5, and finally a copper alloy wire is obtained.

[0081] Embodiment 13

[0082] The difference from Example 2 is that the mass content of B is 0.001%, the mass content of Co is 1.5%, the mass ratio of B to Co is 0.001:1.5, and finally a copper alloy wire is obtained.

[0083] Embodiment 14

[0084] The difference from Example 2 is that the mass content of B is 0.05%, the mass content of Co is 0.951%, the mass ratio of B to Co is 0.05:0.951, and finally a copper alloy wire is obtained.

[0085] Embodiment 15

[0086] The difference from Example 5 is that the casting speed of the first continuous casting is 200 mm / min, and a copper alloy plate is finally obtained.

[0087] Example 16

[0088] The difference from Example 5 is that the casting speed of the first continuous casting is 250 mm / min, and a copper alloy plate is finally obtained.

[0089] Embodiment 17

[0090] The difference from Example 5 is that the deformation amount of hot rolling is 95%, and a copper alloy sheet is finally obtained.

[0091] Embodiment 18

[0092] The difference from Example 5 is that the deformation amount of hot rolling is 85%, and a copper alloy sheet is finally obtained.

[0093] Embodiment 19

[0094] The difference from Example 5 is that the total deformation of the rough rolling is 90%, and / or the deformation of the first cold rolling is 50%, and / or the deformation of the second cold rolling is 37.50%, and / or the deformation of the third cold rolling is 36%, and finally a copper alloy sheet is obtained.

[0095] Embodiment 20

[0096] The difference from Example 5 is that the total deformation of the rough rolling is 80%, and / or the deformation of the first cold rolling is 36%, and / or the deformation of the second cold rolling is 37.50%, and / or the deformation of the third cold rolling is 50%, and finally a copper alloy sheet is obtained.

[0097] Embodiment 21

[0098] The difference from Example 2 is that the casting speed of the second continuous casting is 2.5 m / min, and the copper alloy wire is finally obtained.

[0099] Embodiment 22

[0100] The difference from Example 2 is that the casting speed of the second continuous casting is 4.5 m / min, and the copper alloy wire is finally obtained.

[0101] Comparative Example 1

[0102] The difference from Example 2 is that the melting temperature of the second continuous casting is 1000°C, the holding temperature of the second continuous casting is 900°C, the holding time of the second continuous casting is 30 min, the casting speed of the second continuous casting is 3.5 m / min, the temperature of the second recrystallization annealing is 300°C, and finally a copper alloy wire is obtained.

[0103] Comparative Example 2

[0104] The difference from Example 2 is that the melting temperature of the second continuous casting is 1200°C, the holding temperature of the second continuous casting is 1100°C, the holding time of the second continuous casting is 30min, the casting speed of the second continuous casting is 3.5m / min, the temperature of the second recrystallization annealing is 600°C, and finally a copper alloy wire is obtained.

[0105] Comparative Example 3

[0106] The difference from Example 2 is that, in terms of mass percentage, the copper alloy raw material is made into Cu: 55%, Mn: 5%, B: 0.1%, La: 0.2%, Co: 0.05%, Al: 0.05% and impurity elements ≤ 0.05%, and the balance is Zn, and finally a copper alloy wire is obtained.

[0107] Comparative Example 4

[0108] The difference from Comparative Example 1 is that the copper alloy raw material is subjected to a first batching and a first continuous casting to obtain a copper alloy slab with a thickness of 100 mm; wherein, the first continuous casting is carried out under non-vacuum conditions by horizontal continuous casting, the melting temperature of the first continuous casting is 1170°C, the holding temperature of the first continuous casting is 1150°C, the holding time of the first continuous casting is 30 min, the casting speed of the first continuous casting is 200 mm / min, and the first covering agent charcoal is added during the first continuous casting.

[0109] The copper alloy slab was hot rolled to obtain a hot rolled plate with a thickness of 10 mm, and then cooled and milled to obtain a milled copper alloy slab with a thickness of 8 mm, wherein the hot rolling start temperature was 700°C, the hot rolling final rolling temperature was 500°C, and the hot rolling deformation was 90%. The milled copper alloy slab was rough rolled and subjected to the first recrystallization annealing to obtain a copper plate with a thickness of 1.6 mm, wherein the rough rolling process was subjected to three cold rolling deformations, the total deformation of the rough rolling was 80%, the deformation of the first cold rolling was 50%, the deformation of the second cold rolling was 37.5%, and the deformation of the third cold rolling was 36%; after the second cold rolling, the first recrystallization annealing was carried out under the protection of 75% nitrogen and 25% hydrogen, and the temperature of the first recrystallization annealing was 350°C.

[0110] The copper plate is finish-rolled to obtain a finish-rolled copper plate with a thickness of 1.5 mm, wherein the deformation amount of the finish rolling is 6.25%.

[0111] The copper plate after fine rolling was subjected to a first alkali washing to remove oil stains on the surface of the sample, and then stress relief annealing was performed under nitrogen protection to obtain a copper alloy plate with a thickness of 1.5 mm, wherein the temperature of the stress relief annealing was 250°C.

[0112] Comparative Example 5

[0113] The difference from Example 5 is that, in terms of mass percentage, the copper alloy raw material is made into Cu: 85%, Mn: 0.5%, B: 0.0005%, rare earth element La: 0.005%, Co: 3%, Al: 3% and impurity elements ≤0.05%, and the balance is Zn, and finally a copper alloy sheet is obtained.

[0114] Comparative Example 6

[0115] The difference from Comparative Example 3 is that the copper alloy raw material is subjected to a first batching and a first continuous casting to obtain a copper alloy slab with a thickness of 100 mm; wherein, the first continuous casting is carried out under non-vacuum conditions by horizontal continuous casting, the melting temperature of the first continuous casting is 1050°C, the holding temperature of the first continuous casting is 980°C, the holding time of the first continuous casting is 30 min, the casting speed of the first continuous casting is 200 mm / min, and the first covering agent charcoal is added during the first continuous casting.

[0116] The copper alloy slab was hot rolled to obtain a hot rolled plate with a thickness of 10 mm, and then cooled and milled to obtain a milled copper alloy slab with a thickness of 8 mm, wherein the hot rolling start temperature was 925°C, the hot rolling final rolling temperature was 700°C, and the hot rolling deformation was 90%. The milled copper alloy slab was rough rolled and subjected to the first recrystallization annealing to obtain a copper plate with a thickness of 1.6 mm, wherein the rough rolling process was subjected to three cold rolling deformations, the total deformation of the rough rolling was 80%, the deformation of the first cold rolling was 50%, the deformation of the second cold rolling was 37.5%, and the deformation of the third cold rolling was 36%; after the second cold rolling, the first recrystallization annealing was carried out under the protection of 75% nitrogen and 25% hydrogen, and the temperature of the first recrystallization annealing was 680°C.

[0117] The copper plate is finish-rolled to obtain a finish-rolled copper plate with a thickness of 1.5 mm, wherein the deformation amount of the finish rolling is 6.25%.

[0118] The copper plate after fine rolling was subjected to a first alkali washing to remove oil stains on the surface of the sample, and then stress relief annealing was performed under nitrogen protection to obtain a copper alloy plate with a thickness of 1.5 mm, wherein the temperature of the stress relief annealing was 375°C.

[0119] Comparative Example 7

[0120] The difference from Example 5 is that the melting temperature of the first continuous casting is 1020°C, the holding temperature of the first continuous casting is 1000°C, the holding time of the first continuous casting is 30 min, the casting speed of the first continuous casting is 100 m / min, the starting temperature of hot rolling is 750°C, the final rolling temperature of hot rolling is 500°C, the temperature of the first recrystallization annealing is 380°C, and the temperature of stress relief annealing is 300°C, so as to finally obtain a copper alloy sheet.

[0121] Test Method

[0122] The copper alloy sheets and copper alloy wires of the embodiments and comparative examples of the present invention were subjected to organizational characterization and performance tests, and the test results are shown in Table 1.

[0123] Among them, the test method for tensile strength and elongation: the test is carried out in accordance with GB / T 228.1-2010 "Metallic materials. Tensile test. Part 1: Room temperature test method".

[0124] Corrosion rate test method: Under the test conditions of flow rate of 2m / s and sand content of 300mg / L, the thickness loss of the sample after immersion for 1 month is calculated, and the annual thickness loss is calculated.

[0125] The test method of dislocation density is as follows: Through the X-ray diffraction spectrum, the intensity of the diffraction peak is measured and the dislocation density is obtained after calculation using the Scherrer formula.

[0126] Table 1

[0127]

[0128]

[0129] in, Figure 1 is the microstructure diagram of the copper alloy in Example 1, from Figure 1 It can be seen that the precipitated phase of the copper alloy is dispersed in the matrix, and the grain size of the matrix structure is about 50μm. According to X-ray diffraction analysis, the recrystallization texture content of the copper alloy is 13.8%, and the dislocation density is 8.7×10 -9 cm -2 .

[0130] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0131] The present application adds alloying elements such as Mn, Al, B, Co and rare earth elements to the Cu-Zn binary alloy through an alloying method, which not only enables the copper alloy to have micrometer and nanometer precipitate phase structures of different sizes and dispersedly distributes them in the Cu-Zn alloy matrix, thereby slowing down dezincification corrosion and effectively improving the strength and erosion corrosion resistance of the copper alloy, but also optimizes the forming performance of the copper alloy, thereby reducing the processing difficulty of aquaculture device products. Among them, adding Mn element to the alloy can distort the copper lattice of the copper alloy during the solid solution strengthening process, thereby improving the corrosion resistance of the copper alloy in seawater and chlorides; adding Al element can not only significantly improve the strength and corrosion resistance of the copper alloy, but also form a dense and hard Al2O3 film, thereby blocking the corrosion of the matrix. Even in flowing seawater, the copper alloy can still resist the impact and friction of seawater; adding B element can not only effectively modify and refine the structure of the copper alloy, but also occupy the vacancies in the passivation layer generated after dezincification and prevent the migration of zinc atoms, thereby improving the corrosion resistance of the copper alloy; adding Co element can not only reduce the grain size of the cast copper alloy and change the grain shape, but also simultaneously improve the strength and ductility of the copper alloy; controlling the content and type of rare earth elements within the above range can not only effectively deoxidize, dehydrogenate and remove impurity elements, but also improve the fluidity of the melt, thereby improving the corrosion resistance of the copper alloy. The present invention mixes the above elements in different types and contents to obtain a copper alloy that is not only strong and tough, easy to process and form, but also has good matching between forming performance and strength. It can also be used in aquaculture environments with high water flow rates and high sand content, and maintains excellent corrosion resistance and anti-dezincification corrosion performance in the above aquaculture environments.

[0132] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A copper alloy, characterized in that: In terms of mass percentage, the copper alloy comprises: 55-80% of Cu element, 1-5% of Mn element, 0.1-2% of Al element, 0.001-0.05% of B element, 0.1-2% of Co element, 0.01-0.15% of rare earth element, ≤0.05% of impurity element, and the balance is Zn element; Wherein, the rare earth element is selected from any one or more of Y, Ce, La, Pr, and Sc; The tensile strength of the copper alloy is ≥480MPa, and the elongation of the copper alloy is ≥30%; Under the test conditions of a flow rate of 2 m / s and a sand content of 300 mg / L, the corrosion rate of the copper alloy is ≤0.035 mm / a; The mass ratio of the Mn element to the Al element is 2-4:0.5-1, and the mass ratio of the B element to the Co element is 0.001-0.02:0.5-1.

5.

2. The copper alloy according to claim 1, characterized in that In terms of mass percentage, the copper alloy includes: 65-75% of Cu element, 2-4% of Mn element, 0.5-1% of Al element, 0.001-0.02% of B element, 0.5-1.5% of Co element, 0.01-0.15% of rare earth element, ≤0.05% of impurity element, and the balance is Zn element.

3. The copper alloy according to claim 1 or 2, characterized in that: The recrystallized texture content of the copper alloy is 10-30%, and / or the dislocation density of the copper alloy is 1-10×10 -9 cm -2 , and / or the average grain size of the copper alloy is 5~60μm.

4. A method for preparing the copper alloy according to any one of claims 1 to 3, wherein the copper alloy is a copper alloy sheet, characterized in that: The preparation method comprises: Step S11, performing a first continuous casting after first batching the raw materials corresponding to the copper alloy according to any one of claims 1 to 3 to obtain a copper alloy slab; Step S21, hot rolling, cooling and milling the copper alloy slab in sequence to obtain a milled copper alloy slab; Step S31, performing rough rolling and first recrystallization annealing on the milled copper alloy slab in sequence to obtain a copper plate; Step S41, performing finish rolling on the copper plate to obtain a finish rolled copper plate; Step S51, sequentially performing a first alkali washing and a stress relief annealing on the finish-rolled copper plate to obtain the copper alloy plate; Wherein, the melting temperature of the first continuous casting is 1070-1170°C; The hot rolling start temperature is 800-900°C; the hot rolling finish temperature is 550-620°C; The temperature of the first recrystallization annealing is 400-650°C; The stress relief annealing temperature is 300-350°C.

5. The preparation method according to claim 4, characterized in that: In the step S11, the first continuous casting is performed under non-vacuum conditions by horizontal continuous casting, and / or the holding temperature of the first continuous casting is 1000-1100° C., and / or the holding time of the first continuous casting is 10-30 min, and / or the casting speed of the first continuous casting is 10-200 mm / min; And / or a first covering agent is added during the first continuous casting process, the first covering agent is charcoal and / or cryolite, and / or the thickness of the copper alloy slab is 100-150 mm.

6. The preparation method according to claim 4, characterized in that: In the step S21, the copper alloy slab is hot rolled to obtain a hot-rolled plate, the thickness of the hot-rolled plate is 10-15 mm, and / or the deformation amount of the hot rolling is 90-95%, and / or the thickness of the copper alloy slab after milling is 8-10 mm.

7. The preparation method according to claim 4, characterized in that: In the step S31, the rough rolling includes three cold rolling passes, the three cold rolling passes include a first cold rolling pass, a second cold rolling pass and a third cold rolling pass performed sequentially, the deformation amount of the first cold rolling pass is 30-50%, the deformation amount of the second cold rolling pass is 35-45%, and the deformation amount of the third cold rolling pass is 20-40%; and / or the total deformation amount of the rough rolling is 70-80%, and / or the first recrystallization annealing is performed 1-2 times during the rough rolling process, and / or the thickness of the copper plate is 1.5-3 mm; And / or in the step S41, the deformation amount of the finish rolling is 5-10%, and / or the thickness of the copper plate after the finish rolling is 1-2 mm; And / or in step S51, the thickness of the copper alloy plate is 1-2 mm.

8. A copper alloy sheet, characterized in that: The method is prepared according to any one of claims 4 to 7.

9. A method for preparing the copper alloy according to any one of claims 1 to 3, wherein the copper alloy is a copper alloy wire, characterized in that: The preparation method comprises: Step S21, performing a second batching and a second continuous casting on the raw materials corresponding to the copper alloy according to any one of claims 1 to 3 to obtain a copper alloy wire billet; Step S22, performing a first stretching on the copper alloy wire billet to obtain a first wire billet; Step S23, sequentially subjecting the first wire blank to second recrystallization annealing, pickling, second stretching, and second alkali washing to obtain the copper alloy wire; Wherein, the melting temperature of the second continuous casting is 1050-1150°C; The temperature of the second recrystallization annealing is 350-550°C.

10. The preparation method according to claim 9, characterized in that: In the step S21, the second continuous casting is performed in a non-vacuum condition by adopting an upward continuous casting method, and / or the holding temperature of the second continuous casting is 950-1050° C., and / or the holding time of the second continuous casting is 10-30 min, and / or the casting speed of the second continuous casting is 2.5-3.5 m / min; and / or adding a second covering agent during the second continuous casting process, wherein the second covering agent is charcoal and / or cryolite; And / or cooling water is used for cooling after the second continuous casting, the temperature of the cooling water is 20-35° C., the flow rate of the cooling water is 18-35 L / min, and / or the diameter of the copper alloy wire billet is φ10-φ20 mm.

11. The preparation method according to claim 9, characterized in that: In the step S22, the deformation amount of the first stretching is 20%~80%, and / or the diameter of the first wire blank is φ8~φ15mm; and / or in the step S23, the deformation amount of the second stretching is 20%~90%, and / or the diameter of the copper alloy wire is φ3~φ10mm.

12. A copper alloy wire, characterized in that: The method is prepared according to any one of claims 9 to 11.