A method for preparing an anti-oxidation SBS modified asphalt waterproofing membrane

By combining nanotitanium dioxide and tetrakis (semi-hindered phenol) pentaerythritol diphosphate in SBS modified asphalt waterproof rolls, the deterioration problem of traditional SBS modified asphalt waterproof rolls in light, oxygen and water environments is solved. It significantly improves its antioxidant, heat resistance and flame retardant properties, meeting the multifunctional needs of modern society.

CN118563576BActive Publication Date: 2024-11-01BEIXIN YUWANG WATERPROOF TECH (ANHUI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411053695.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-01
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Traditional SBS modified asphalt waterproof coils are prone to yellowing and hardening in light, oxygen and water-enriched environments, which affects their application performance and lacks antioxidant properties, which cannot meet the multifunctional needs of modern society.

Method used

Mannich reaction was carried out using aminopropyltriethoxysilane, formaldehyde and 4-vinylphenol. After obtaining the intermediate, it condensed with nanotitanium dioxide. The nanotitanium dioxide modified SBS was obtained through grafting reaction and was modified with 4 (and a half) Stuck phenol) pentaerythritol diphosphate is combined and added to the asphalt to form an antioxidant SBS modified asphalt waterproof roll.

Benefits of technology

It significantly improves the oxidation resistance, heat resistance and flame retardant properties of the waterproof coil, extends the service life, and improves the heat resistance and waterproof properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563576B_ABST
    Figure CN118563576B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of waterproofing coiled materials, and discloses a method for preparing an antioxidant SBS modified asphalt waterproofing coiled material. The invention uses aminopropyl triethoxysilane, formaldehyde, 4-vinylphenol, nano titanium dioxide, SBS and the like as raw materials, and obtains nano titanium dioxide modified SBS through a series of reactions. Pentaerythritol, triethyl phosphite, β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride and the like are used as raw materials, and tetra (semi-hindered phenol) pentaerythritol diphosphate is obtained through reaction. Finally, SBS, nano titanium dioxide modified SBS, tetra (semi-hindered phenol) pentaerythritol diphosphate and the like are added to the asphalt, mixed evenly, coated on a polyester base, and covered with a PE film to obtain an antioxidant SBS modified asphalt waterproofing coiled material. The waterproofing coiled material prepared by the invention has excellent antioxidant properties, flame retardant properties and heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coiled materials, in particular to a method for preparing an antioxidant SBS modified asphalt waterproof coiled material. Background Art

[0002] SBS modified asphalt waterproof membrane has excellent waterproof performance and is therefore widely used on roads. However, with the rapid development of the economy, traditional SBS modified asphalt waterproof membrane can no longer meet the demand. Therefore, it is necessary to give SBS modified asphalt waterproof membrane more functions to adapt to the development of modern society.

[0003] Styrene-butadiene-styrene block copolymer (SBS) is a thermoplastic elastomer with excellent impact toughness, elasticity and other properties. However, due to the large number of unsaturated carbon-carbon double bonds in the SBS molecular structure, SBS will turn yellow and harden in an environment rich in light, oxygen and water, especially under ultraviolet rays, which affects the application of SBS in waterproof membranes. Therefore, it is also necessary to improve the antioxidant properties of SBS.

[0004] Adding antioxidants to materials is the simplest and most effective way to delay material degradation and extend service life. Semi-hindered phenol antioxidants are derivatives based on 2-methyl-6-tert-butylphenol. They not only have the characteristics of traditional hindered phenol antioxidants, but also have more advantages in synergistic stabilization with auxiliary antioxidants than traditional fully hindered phenol antioxidants. They are suitable for thermal oxidative degradation and are widely used in various polymer materials. Phosphite antioxidants are a major hydroperoxide decomposition auxiliary antioxidant, which has a good synergistic effect with hindered phenol main antioxidants. They have always received high attention from the polymer materials industry and are widely used in polymer materials. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing an antioxidant SBS modified asphalt waterproofing membrane. The prepared modified asphalt waterproofing membrane has excellent antioxidant performance, heat resistance and flame retardant performance.

[0007] (II) Technical solution

[0008] A method for preparing an antioxidant SBS modified asphalt waterproofing membrane, the preparation method comprising:

[0009] Step (1), add aminopropyltriethoxysilane and formaldehyde into a flask containing chloroform solvent, stir evenly, then add 4-vinylphenol, heat to 60-70°C, reflux for 4-8h, after the reaction is completed, cool to room temperature, filter, rotary evaporate, and dry to obtain intermediate 1.

[0010] Step (2), adding nano titanium dioxide into a flask containing toluene solvent, ultrasonically dispersing, then adding intermediate 1 thereto, reacting at 40-50°C for 5-10 hours, then heating to 85-95°C, reacting for 2-3 hours, and after the reaction is completed, washing with ethanol and drying to obtain olefinated nano titanium dioxide.

[0011] Step (3), under nitrogen conditions, SBS, maleic anhydride, and olefinic nano-titanium dioxide are added to a flask containing toluene solvent, stirred and dispersed, heated to 80-90° C., benzoyl peroxide is added thereto, stirred and reacted for 2-5 hours, and after the reaction is completed, vacuum distillation is performed, ethanol precipitation is performed, suction filtration is performed, and drying is performed to obtain nano-titanium dioxide modified SBS.

[0012] Step (4), adding asphalt into a drying oven at 150-170°C, heating and melting, then adding SBS and nano-titanium dioxide modified SBS, stirring evenly, then adding cyclohexane oil, tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and talcum powder, stirring and mixing evenly, discharging at 180-190°C, coating on the impregnated and squeezed polyester base, and covering the upper and lower surfaces with PE film to obtain an antioxidant SBS modified asphalt waterproof membrane.

[0013] Preferably, in step (1), the usage ratio of aminopropyltriethoxysilane, formaldehyde and 4-vinylphenol is (180-200) g: (50-80) g: 100 g.

[0014] Preferably, in step (2), the usage ratio of nano titanium dioxide to intermediate 1 is 1 g: (0.4-0.8) g.

[0015] Preferably, in step (3), the usage ratio of SBS, maleic anhydride and olefinated nano-titanium dioxide is 100 g: (5-15) g: (10-20) g.

[0016] Preferably, in step (3), the amount of benzoyl peroxide used is 2-5% of the total mass of SBS, maleic anhydride, and olefinic nano-titanium dioxide.

[0017] Preferably, in step (4), the usage ratio of asphalt, SBS, nano-titanium dioxide modified SBS, cyclohexane oil, tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and talc is 100 g: (10-20) g: (10-20) g: (40-60) g: (0.5-5): (20-25) g.

[0018] Preferably, in step (4), the preparation method of tetrakis(semi-hindered phenol) pentaerythritol diphosphate is:

[0019] S1. Add pentaerythritol, triethyl phosphite and dibutyltin oxide into a flask, stir and disperse, heat to 130-140°C, stir and react for 2-4 hours, and after the reaction is completed, distill under reduced pressure, then add 3,5-dinitrobenzyl alcohol into the flask, stir and react for 1-3 hours at 170-180°C, and after the reaction is completed, distill under reduced pressure to obtain intermediate 2;

[0020] S2. Under nitrogen, add intermediate 2 and hydrazine monohydrate to a flask filled with ethanol solvent, stir and disperse, then add 5% Pd-C, reflux for 12-24h, and after the reaction is completed, cool to room temperature, filter, distill under reduced pressure, and dry to obtain intermediate 3;

[0021] S3. Add intermediate 3 and potassium carbonate into a flask filled with deionized water, stir and disperse, add β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride at 0-5°C, stir and disperse, heat to 20-30°C, react for 20-30h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain pentaerythritol diphosphate containing tetrakis(semi-hindered phenol).

[0022] Preferably, in S1, the usage ratio of pentaerythritol, triethyl phosphite and 3,5-dinitrobenzyl alcohol is 100 g: (240-300) g: (280-340) g.

[0023] Preferably, in S3, the usage ratio of intermediate 3, potassium carbonate and β-(3-methyl-5-tert-butyl-4-hydroxyphenyl)propionyl chloride is 100 g:(220-300) g:(420-500) g.

[0024] 3. Beneficial technical effects

[0025] The present invention uses aminopropyl triethoxysilane, formaldehyde and 4-vinylphenol to obtain intermediate 1 through Mannich reaction, and then obtains olefinic nano titanium dioxide through condensation reaction. Using olefinic nano titanium dioxide and maleic anhydride as grafting monomers, SBS is grafted through solution polymerization to obtain nano titanium dioxide modified SBS. Using pentaerythritol, triethyl phosphite and 3,5-dinitrobenzyl alcohol as raw materials and dibutyltin oxide as catalyst, intermediate 2 is obtained, intermediate 2 is reduced through palladium carbon to obtain intermediate 3, and the amino group contained in intermediate 3 and β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride are used to obtain tetrakis (semi-hindered phenol) pentaerythritol diphosphate under the catalysis of potassium carbonate. Finally, SBS, nano-titanium dioxide modified SBS, tetrakis(semi-hindered phenol) pentaerythritol diphosphate, etc. are added to the asphalt, stirred and mixed evenly, the material is discharged, coated on the polyester base, and the upper and lower surfaces are covered with PE film to obtain an antioxidant SBS modified asphalt waterproof membrane.

[0026] The invention prepares tetra(semi-hindered phenol) pentaerythritol diphosphate, which has a novel structure and a simple preparation method. In addition, the semi-hindered phenol structure is used as a main antioxidant and the phosphite structure is used as an auxiliary antioxidant. The semi-hindered phenol structure is added to the waterproof membrane, and the two antioxidant structures are used in combination to effectively improve the antioxidant performance of the waterproof membrane.

[0027] The nano titanium dioxide used in the present invention is an inorganic nanoparticle, but because it has a large surface energy, the nano titanium dioxide is easy to agglomerate. The present invention makes it organic, reduces the degree of agglomeration, increases its compatibility with organic substances, and then evenly distributes it in the waterproof coiled material. And because it has good heat resistance, it is added to the waterproof coiled material to improve the heat resistance. In addition, the nano titanium dioxide modified SBS prepared by the present invention contains a benzoxazine structure, which absorbs heat when heated, can open the ring to form a cross-linked network structure, and further improves the heat resistance of the material. And it also contains a silicon oxygen bond, which has a large bond energy and can absorb more heat, further improving the heat resistance of the material.

[0028] The waterproof roll prepared by the present invention contains phosphorus, nitrogen and silicon, which are flame retardant elements. Adding them to the waterproof roll can improve the flame retardant performance of the waterproof roll. The waterproof roll prepared by the present invention has excellent antioxidant performance, flame retardant performance and heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is the reaction formula of olefination nano-titanium dioxide;

[0030] Figure 2 It is a reaction formula containing tetrakis(semi-hindered phenol) pentaerythritol diphosphate. DETAILED DESCRIPTION

[0031] In order to make the technical problems, technical solutions and comparative effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention, rather than to limit the present invention.

[0032] The preparation method of β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride is prepared according to the literature "Study on the Synthesis of β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride"; the asphalt is 90 # asphalt. Embodiment 1

[0033] (1) Add 18 g of aminopropyltriethoxysilane and 8 g of formaldehyde into a flask containing 100 mL of chloroform solvent and stir evenly. Then add 10 g of 4-vinylphenol and heat to 70°C. Reflux for 5 h. After the reaction is completed, cool to room temperature, filter, rotary evaporate, and dry to obtain intermediate 1.

[0034] (2) 5 g of nano titanium dioxide was added to a flask containing 100 mL of toluene solvent and dispersed by ultrasonication. Then 3 g of intermediate 1 was added thereto and reacted at 45 °C for 6 h. The temperature was then raised to 95 °C and the reaction was continued for 2 h. After the reaction was completed, the mixture was washed with ethanol and dried to obtain olefinated nano titanium dioxide.

[0035] (3) Under nitrogen conditions, 10 g of SBS, 1.5 g of maleic anhydride, and 1 g of olefinated nano-titanium dioxide were added to a flask containing 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 80°C. 0.025 g of benzoyl peroxide was added thereto, and the reaction was stirred for 2 h. After the reaction was completed, vacuum distillation was performed, ethanol precipitation was performed, suction filtration was performed, and drying was performed to obtain nano-titanium dioxide modified SBS.

[0036] (4) 8 g of pentaerythritol, 19.2 g of triethyl phosphite and 0.8 g of dibutyltin oxide were added to a flask, stirred and dispersed, heated to 135°C, stirred and reacted for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure. Then 27.2 g of 3,5-dinitrobenzyl alcohol was added to the flask, stirred and reacted at 180°C for 2 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.

[0037] (5) Under nitrogen, 30 g of intermediate 2 and 100 mL of hydrazine monohydrate were added to a flask containing 150 mL of ethanol solvent, stirred and dispersed, and then 4 g of 5% Pd-C was added thereto. The reaction was refluxed for 20 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, evaporated under reduced pressure, and dried to obtain intermediate 3.

[0038] (6) Add 5 g of intermediate 3 and 12 g of potassium carbonate into a flask containing 100 mL of deionized water, stir and disperse, add 24 g of β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride at 0°C, stir and disperse, raise the temperature to 25°C, react for 24 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain pentaerythritol diphosphate containing tetrakis(semi-hindered phenol).

[0039] (7) Add 40 g of asphalt into a drying oven at 160°C, heat to melt, then add 8 g of SBS and 4 g of nano-titanium dioxide modified SBS, stir evenly, then add 24 g of cyclohexane oil, 0.2 g of tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and 10 g of talcum powder, stir and mix evenly, discharge at 185°C, coat on the impregnated and squeezed polyester base, cover the upper and lower surfaces with PE film, and obtain an antioxidant SBS modified asphalt waterproof membrane. Embodiment 2

[0040] (1) Add 20 g of aminopropyltriethoxysilane and 6 g of formaldehyde into a flask containing 100 mL of chloroform solvent and stir evenly. Then add 10 g of 4-vinylphenol and heat to 65 °C. Reflux for 8 h. After the reaction is completed, cool to room temperature, filter, rotary evaporate, and dry to obtain intermediate 1.

[0041] (2) 5 g of nano titanium dioxide was added to a flask containing 100 mL of toluene solvent and dispersed by ultrasonication. Then 3 g of intermediate 1 was added thereto and reacted at 40 °C for 5 h. The temperature was then raised to 90 °C and the reaction was continued for 2 h. After the reaction was completed, the mixture was washed with ethanol and dried to obtain olefinated nano titanium dioxide.

[0042] (3) Under nitrogen conditions, 10 g of SBS, 0.5 g of maleic anhydride, and 2 g of olefinated nano-titanium dioxide were added to a flask containing 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 90°C. 0.062 g of benzoyl peroxide was added thereto, and the reaction was stirred for 5 h. After the reaction was completed, vacuum distillation was performed, ethanol precipitation was performed, suction filtration was performed, and drying was performed to obtain nano-titanium dioxide modified SBS.

[0043] (4) 8 g of pentaerythritol, 24 g of triethyl phosphite and 1 g of dibutyltin oxide were added to a flask, stirred and dispersed, heated to 130°C, stirred and reacted for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure. Then 22.4 g of 3,5-dinitrobenzyl alcohol was added to the flask, stirred and reacted at 180°C for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.

[0044] (5) Under nitrogen, 30 g of intermediate 2 and 140 mL of hydrazine monohydrate were added to a flask containing 150 mL of ethanol solvent, stirred and dispersed, and then 3 g of 5% Pd—C was added thereto. The reaction was refluxed for 24 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, evaporated under reduced pressure, and dried to obtain intermediate 3.

[0045] (6) Add 5 g of intermediate 3 and 11 g of potassium carbonate into a flask containing 100 mL of deionized water, stir and disperse, add 25 g of β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride at 5°C, stir and disperse, raise the temperature to 25°C, react for 30 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain pentaerythritol diphosphate containing tetra(semi-hindered phenol).

[0046] (7) Add 40 g of asphalt into a drying oven at 150°C, heat to melt, then add 6 g of SBS and 5 g of nano-titanium dioxide modified SBS, stir evenly, then add 16 g of cyclohexane oil, 1 g of tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and 10 g of talcum powder, stir and mix evenly, discharge at 180°C, coat on the impregnated and squeezed polyester base, cover the upper and lower surfaces with PE film, and obtain an antioxidant SBS modified asphalt waterproof membrane. Embodiment 3

[0047] (1) Add 20 g of aminopropyltriethoxysilane and 5 g of formaldehyde into a flask containing 100 mL of chloroform solvent and stir evenly. Then add 10 g of 4-vinylphenol and heat to 60 °C. Reflux for 4 h. After the reaction is completed, cool to room temperature, filter, rotary evaporate, and dry to obtain intermediate 1.

[0048] (2) 5 g of nano titanium dioxide was added to a flask containing 100 mL of toluene solvent and dispersed by ultrasonication. Then 4 g of intermediate 1 was added thereto and reacted at 50 °C for 6 h. The temperature was then raised to 95 °C and the reaction was carried out for 3 h. After the reaction was completed, the mixture was washed with ethanol and dried to obtain olefinated nano titanium dioxide.

[0049] (3) Under nitrogen conditions, 10 g of SBS, 1 g of maleic anhydride, and 1.5 g of olefinated nano-titanium dioxide were added to a flask containing 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 85°C. 0.05 g of benzoyl peroxide was added thereto, and the reaction was stirred for 4 h. After the reaction was completed, vacuum distillation was performed, ethanol precipitation was performed, suction filtration was performed, and drying was performed to obtain nano-titanium dioxide modified SBS.

[0050] (4) 8 g of pentaerythritol, 22 g of triethyl phosphite and 1.5 g of dibutyltin oxide were added to a flask, stirred and dispersed, and the temperature was raised to 140°C. The mixture was stirred and reacted for 2 h. After the reaction was completed, the mixture was distilled under reduced pressure. Then 25 g of 3,5-dinitrobenzyl alcohol was added to the flask, and the mixture was stirred and reacted at 170°C for 1 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.

[0051] (5) Under nitrogen, 30 g of intermediate 2 and 80 mL of hydrazine monohydrate were added to a flask containing 150 mL of ethanol solvent, stirred and dispersed, and then 4 g of 5% Pd—C was added thereto. The reaction was refluxed for 12 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, evaporated under reduced pressure, and dried to obtain intermediate 3.

[0052] (6) Add 5 g of intermediate 3 and 12 g of potassium carbonate into a flask containing 100 mL of deionized water, stir and disperse, add 21 g of β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride at 0°C, stir and disperse, raise the temperature to 30°C, react for 20 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain pentaerythritol diphosphate containing tetrakis(semi-hindered phenol).

[0053] (7) Add 40 g of asphalt into a drying oven at 170°C, heat to melt, then add 5 g of SBS and 6 g of nano-titanium dioxide modified SBS, stir evenly, then add 20 g of cyclohexane oil, 1.5 g of tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and 8 g of talcum powder, stir and mix evenly, discharge at 190°C, coat on the impregnated and squeezed polyester base, and cover the upper and lower surfaces with PE film to obtain an antioxidant SBS modified asphalt waterproof membrane. Embodiment 4

[0054] (1) Add 20 g of aminopropyltriethoxysilane and 6 g of formaldehyde into a flask containing 100 mL of chloroform solvent and stir evenly. Then add 10 g of 4-vinylphenol and heat to 65 °C. Reflux for 5 h. After the reaction is completed, cool to room temperature, filter, rotary evaporate, and dry to obtain intermediate 1.

[0055] (2) 5 g of nano titanium dioxide was added to a flask containing 100 mL of toluene solvent and dispersed by ultrasonication. Then 2 g of intermediate 1 was added thereto and reacted at 45 °C for 10 h. The temperature was then raised to 85 °C and the reaction was continued for 2 h. After the reaction was completed, the mixture was washed with ethanol and dried to obtain olefinated nano titanium dioxide.

[0056] (3) Under nitrogen conditions, 10 g of SBS, 1.5 g of maleic anhydride, and 1.5 g of olefinated nano-titanium dioxide were added to a flask containing 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 85°C. 0.06 g of benzoyl peroxide was added thereto, and the reaction was stirred for 4 h. After the reaction was completed, vacuum distillation was performed, ethanol precipitation was performed, suction filtration was performed, and drying was performed to obtain nano-titanium dioxide modified SBS.

[0057] (4) 8 g of pentaerythritol, 20 g of triethyl phosphite and 1.2 g of dibutyltin oxide were added to a flask, stirred and dispersed, heated to 135°C, stirred and reacted for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure. Then 26 g of 3,5-dinitrobenzyl alcohol was added to the flask, stirred and reacted at 175°C for 2 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.

[0058] (5) Under nitrogen, 30 g of intermediate 2 and 100 mL of hydrazine monohydrate were added to a flask containing 150 mL of ethanol solvent, stirred and dispersed, and then 2 g of 5% Pd-C was added thereto. The reaction was refluxed for 20 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, evaporated under reduced pressure, and dried to obtain intermediate 3.

[0059] (6) Add 5 g of intermediate 3 and 15 g of potassium carbonate into a flask containing 100 mL of deionized water, stir and disperse, add 22 g of β-(3-methyl-5-tert-butyl-4-hydroxyphenyl) propionyl chloride at 0°C, stir and disperse, raise the temperature to 20°C, react for 24 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain pentaerythritol diphosphate containing tetra(semi-hindered phenol).

[0060] (7) Add 40 g of asphalt into a drying oven at 160°C, heat to melt, then add 4 g of SBS and 8 g of nano-titanium dioxide modified SBS, stir evenly, then add 24 g of cyclohexane oil, 2 g of tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and 10 g of talcum powder, stir and mix evenly, discharge at 185°C, coat on the impregnated and squeezed polyester base, cover the upper and lower surfaces with PE film, and obtain an antioxidant SBS modified asphalt waterproof membrane.

[0061] Comparative Example 1

[0062] The difference between this comparative example and Example 1 is that in step (7), nano-titanium dioxide-modified SBS is not contained.

[0063] Comparative Example 2

[0064] The difference between this comparative example and Example 1 is that in step (7), pentaerythritol diphosphate containing tetrakis(semi-hindered phenol) is not contained.

[0065] The waterproof membrane was added into the hot oxygen aging test oven and subjected to hot oxygen aging at 70°C for 3 days. Referring to GB / T4507-2014, an automatic asphalt softening point tester was used to test the softening point of the waterproof membrane. The softening point increment (°C) = softening point after aging (°C) - softening point before aging (°C).

[0066] Table 1: Antioxidant performance test of various embodiments and comparative examples

[0067] Softening point increment (℃) Example 1 4.2 Example 2 3.8 Example 3 3.1 Example 4 2.8 Comparative Example 1 4.6 Comparative Example 2 5.0

[0068] It can be seen from the table that the softening point increments of Examples 1-4 and Comparative Example 1 are smaller than that of Comparative Example 2, and it can be seen from Examples 1-4 that as the amount of tetrakis(semi-hindered phenol) pentaerythritol diphosphate increases, the softening point increment gradually decreases, and the thermal oxidation resistance of the waterproof membrane is better. This is because the tetrakis(semi-hindered phenol) pentaerythritol diphosphate prepared by the present invention contains a semi-hindered phenol structure and a phosphite structure, wherein the semi-hindered phenol structure has the ability to capture free radicals, thereby playing a chain termination role, and the phosphite structure can promote the decomposition of hydroperoxides, decomposing the peroxides formed in the oxidation process into non-free radicals, thereby preventing the auto-catalytic free radical process in the oxidation process and controlling the oxidation reaction. The two are compatible with each other and jointly increase the antioxidant properties of the waterproof membrane.

[0069] Refer to GB / T328.11-2007 to test the heat resistance of waterproof membrane. Take 100mm×50mm and hang it vertically in an oven at 120℃. After 1h, test the displacement of the coating layers on both sides relative to the carcass. If the average displacement exceeds 2mm, it is unqualified.

[0070] Refer to GB8624-2012 to test the flame retardant properties of waterproof membranes. B1 is a flame retardant material, and B2 is a flammable material.

[0071] Table 2: Heat resistance and flame retardancy tests of various embodiments and comparative examples

[0072] Eligibility Flame retardant grade Example 1 yes B1 Example 2 yes B1 Example 3 yes B1 Example 4 yes B1 Comparative Example 1 no B1 Comparative Example 2 yes B2

[0073] It can be seen from the table that the waterproof coiled material prepared by the present invention has good heat resistance and flame retardancy.

[0074] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing an antioxidant SBS modified asphalt waterproofing membrane, characterized in that: The preparation method is: Step (1), adding aminopropyltriethoxysilane and formaldehyde into a flask containing chloroform solvent, stirring evenly, adding 4-vinylphenol thereto, heating to 60-70° C., reflux reaction for 4-8 hours, cooling to room temperature after the reaction, filtering, rotary evaporation, and drying to obtain intermediate 1; Step (2), adding nano titanium dioxide into a flask filled with toluene solvent, ultrasonically dispersing, then adding intermediate 1 thereto, reacting at 40-50° C. for 5-10 hours, then heating to 85-95° C. for 2-3 hours, washing with ethanol after the reaction, and drying to obtain olefinated nano titanium dioxide; Step (3), under nitrogen conditions, SBS, maleic anhydride, and olefinic nano-titanium dioxide are added to a flask containing toluene solvent, stirred and dispersed, heated to 80-90° C., benzoyl peroxide is added thereto, stirred and reacted for 2-5 hours, and after the reaction is completed, vacuum distillation, ethanol precipitation, suction filtration, and drying are performed to obtain nano-titanium dioxide modified SBS; Step (4), adding asphalt to a drying oven at 150-170° C., heating and melting, then adding SBS and nano-titanium dioxide modified SBS thereto, stirring evenly, then adding cyclohexane oil, tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and talcum powder thereto, stirring and mixing evenly, discharging at 180-190° C., coating on the impregnated and squeezed polyester base, and covering the upper and lower surfaces with PE film to obtain an antioxidant SBS modified asphalt waterproof membrane. The preparation method of the tetrakis(semi-hindered phenol) pentaerythritol diphosphate is as follows: S1. Add pentaerythritol, triethyl phosphite and dibutyltin oxide into a flask, stir and disperse, heat to 130-140° C., stir and react for 2-4 hours, and after the reaction, distill under reduced pressure. Then add 3,5-dinitrobenzyl alcohol into the flask, stir and react for 1-3 hours at 170-180° C., and after the reaction, distill under reduced pressure to obtain intermediate 2, wherein the amount ratio of pentaerythritol, triethyl phosphite and 3,5-dinitrobenzyl alcohol is 100 g:(240-300) g:(280-340) g; S2. Under nitrogen, add intermediate 2 and hydrazine monohydrate to a flask filled with ethanol solvent, stir and disperse, then add 5% Pd-C, reflux for 12-24 hours, and after the reaction is completed, cool to room temperature, filter, distill under reduced pressure, and dry to obtain intermediate 3; S3. Add intermediate 3 and potassium carbonate into a flask filled with deionized water, stir and disperse, add β-(3-methyl-5-tert-butyl-4-hydroxyphenyl)propionyl chloride at 0-5°C, stir and disperse, heat to 20-30°C, react for 20-30h, and after the reaction, filter, wash with deionized water, and dry to obtain tetrakis(semi-hindered phenol) pentaerythritol diphosphate, wherein the usage ratio of intermediate 3, potassium carbonate, and β-(3-methyl-5-tert-butyl-4-hydroxyphenyl)propionyl chloride is 100g:(220-300)g:(420-500)g.

2. The method for preparing the antioxidant SBS modified asphalt waterproofing membrane according to claim 1, characterized in that: In the step (1), the usage ratio of aminopropyltriethoxysilane, formaldehyde and 4-vinylphenol is (180-200) g:(50-80) g:100 g.

3. The method for preparing the antioxidant SBS modified asphalt waterproofing membrane according to claim 1, characterized in that: In the step (2), the usage ratio of nano titanium dioxide and intermediate 1 is 1g:(0.4-0.8)g.

4. The method for preparing the antioxidant SBS modified asphalt waterproofing membrane according to claim 1, characterized in that: In the step (3), the usage ratio of SBS, maleic anhydride and olefinic nano-titanium dioxide is 100 g:(5-15) g:(10-20) g.

5. The method for preparing the antioxidant SBS modified asphalt waterproofing membrane according to claim 1, characterized in that: In the step (3), the amount of benzoyl peroxide used is 2-5% of the total mass of SBS, maleic anhydride and olefinic nano-titanium dioxide.

6. The method for preparing the antioxidant SBS modified asphalt waterproofing membrane according to claim 1, characterized in that: In the step (4), the usage ratio of asphalt, SBS, nano-titanium dioxide modified SBS, cyclohexane oil, tetrakis(semi-hindered phenol) pentaerythritol diphosphate, and talc is 100g:(10-20)g:(10-20)g:(40-60)g:(0.5-5):(20-25)g.