A prestressed crack arrest and life extension design method for fatigue cracks
Through linear elastic fracture mechanics and stress strength factor superposition method, combined with deformation coordination method, the problems of high time and economic costs and insufficient calculation ability of fatigue crack stop and life extension research in the existing technology are solved, and the accuracy of metal plates is achieved Analysis and prediction guide the fatigue crack-restraining and life-extending design of prestressed CFRP bands.
Patent Information
- Application Number
- CN202411027401.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
In the research on prestressed cracking and life extension of fatigue cracks, there are problems such as time-consuming and labor-intensive experiments, insufficient finite element analysis and calculation capabilities, and insufficient theoretical model accuracy, especially in complex structures, it is difficult to accurately analyze cracking stops at different reinforcement positions. and the effects of life prolongation.
By using linear elastic fracture mechanics and stress strength factor superposition method, the total stress strength factor of the split reinforced structure is the strength factor caused by far-field load, bridge stress and prestress, and the minimum effective stress strength factor is determined by deformation coordination method. Amplitude, compare it with the stress strength factor threshold to determine the optimal reinforcement position, if cracks cannot be stopped, the fatigue crack proliferation life is calculated through the Paris relationship to determine the life prolongation effect.
Accurate analysis of the global reinforcement position of metal plates is realized, the force transmission mechanism between metal wall plates and CFRP strips is revealed, the fatigue crack growth life and rate after prestressed reinforcement is predicted, and the prestressed CFRP strips are guided to fatigue cracks The crack-resistance and life-extending design avoids the high time and economic costs of experiments and finite element analysis.
Smart Images

Figure CN118568992B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solid mechanics, and relates to but is not limited to a prestressed crack arrest and life extension design method for fatigue cracks. Background Art
[0002] At present, a large number of metal structures in the world are gradually aging, such as steel structures of building bridges, offshore work platforms and aircraft skins. With the extension of service time and the influence of harsh environment, the "aging" problem of metal structures will become more and more serious. If the aging steel structure is dismantled and replaced, it will not only cause huge economic losses, but also harm the environment. The technology of using prestressed CFRP (Carbon Fiber Reinforced Polymer) to strengthen aging metal structures has been widely used. Prestressed CFRP strips can further improve the reinforcement efficiency or prevent fatigue crack propagation. Prestressing effectively reduces the stress intensity factor (SIF) around the crack tip and improves the fatigue life of metal structures.
[0003] Most of the research on mechanical reinforcement of aging metal structures with prestressed CFRP is based on experimental and finite element research. In terms of experiments, Ghafoori et al. used mechanical connection of prestressed units to reinforce metal beams in 2015, and used constant life diagrams (CLDs) to determine the minimum prestress level to prevent fatigue cracks in metal beams. The experiment proved that this prestressing strengthening method can prevent the initiation of cracks, especially when the stress history of previous cyclic loads is unknown. In terms of finite elements, Hosseini et al. used Abaqus commercial finite element software to calculate the stress intensity factor of prestressed CFRP mechanically reinforced steel plates with central cracks, which was used to guide the study of fatigue crack arrest. In addition, some scholars have conducted theoretical research on the fatigue properties of prestressed CFRP reinforced cracked plates. Liu et al., based on the strain coordination principle at the connection between steel plate and CFRP, considered the influence of crack tension displacement in steel plate on strain, and developed a method for predicting the fatigue crack propagation life and rate of prestressed CFRP mechanically anchored steel plates with central cracks, which can be used to guide the study of fatigue crack arrest and life extension.
[0004] However, experimental research on such fatigue crack arrest and life extension takes a lot of time. If the experimental research is converted to engineering application, the time period required is even longer, and a lot of financial and material resources are also consumed, resulting in the disadvantages of high time and economic costs in engineering application. Finite element analysis has certain advantages in prestressed CFRP reinforcement with simple structure. However, in actual engineering applications, the structure to be reinforced is often relatively complex, which is also a test for the calculation ability and analysis time of finite element analysis. Compared with experimental methods and finite element analysis methods, theoretical research is more efficient and economical. While it can quickly analyze and predict the crack arrest and life extension effects, it is not restricted by the complex conditions of the reinforced structure. However, the current theoretical research still has defects. For example, Hosseini et al. converted the prestress in CFRP into stress equivalent to the far-field load action mode, derived the calculation formula of the stress intensity factor at the crack tip, and used it to guide the prestressed crack arrest research of fatigue cracks. This method does not consider the effect of crack opening angle on load transfer between CFRP and steel plate, so the model of Hosseini et al. is only accurate enough in the small crack stage. Liu et al. considered the effect of crack opening displacement and developed a new prediction model for prestressed crack arrest and life extension, but the prediction model is only effective when CFRP is used to reinforce cracked plates in the far field, and cannot analyze the effect of global reinforcement position on crack arrest and life extension. Summary of the invention
[0005] In view of this, an embodiment of the present invention provides a prestressed crack arrest and life extension design method for fatigue cracks, which not only avoids the time-consuming and labor-intensive shortcomings of experimental methods, but also can accurately analyze the effects of different reinforcement positions on crack arrest and life extension.
[0006] The technical solution of the embodiment of the present invention is achieved as follows:
[0007] An embodiment of the present invention provides a method for prestressed crack arrest and life extension design of fatigue cracks, the method comprising:
[0008] Determine the size and material parameters of the metal plate and carbon fiber reinforced polymer CFRP, load parameters, and initial reinforcement point coordinates; based on the linear elastic fracture mechanics and the loading conditions of the metal plate, the total stress intensity factor K of the reinforced structure is total Split into the intensity factor K caused by far-field load ff , Intensity factor K caused by bridging stress br and the strength factor K caused by prestress pre Solve them separately; where K br The bridge force F is solved according to the deformation coordination method. br Based on the total stress intensity factor K total, determine the minimum effective stress intensity factor amplitude ΔK in the global reinforcement position of the metal plate eff ; By comparing the effective stress intensity factor amplitude ΔK eff and stress intensity factor threshold ΔK th , determine whether the designed reinforcement position can successfully stop cracks under the existing prestressing conditions; when crack arrest cannot be achieved at any reinforcement point, calculate the fatigue crack growth life through the Paris relationship to determine the target reinforcement position with the best life extension effect.
[0009] In some possible embodiments, assuming that the length of the reinforcement center crack is 2a, the intensity factor K caused by the bridging stress is br It is solved by the following formula:
[0010] ;
[0011] ;
[0012] ;
[0013] ;
[0014] In the formula, is half the crack length, is the intermediate variable, is the geometric correction factor of a metal plate with a central crack under four-point concentrated force loading, is the thickness of the metal plate, is the Poisson’s ratio of the metal plate, is the coordinate of the initial reinforcement point, i is an imaginary unit, y is the ordinate of any position of the metal plate, and It is the complex function expression of the coordinates of the four-point concentrated force positions in the global coordinate system of the cracked plate; The bridging force is solved by the deformation coordination relationship between the metal crack plate and the CFRP strip at the reinforcement point; is the metal sheet width, is the stress distribution in the cross section in front of the crack tip where no crack occurs in the direction of the far-field load.
[0015] In some possible embodiments, the deformation coordination relationship is represented by the following formula:
[0016] ;
[0017] Where V ff is the displacement of the metal plate at the reinforcement point under the action of the far-field load; V br is the bridge force F of the metal plate br The displacement at the reinforcement point caused by the action of Vpre It is the displacement of the metal plate at the reinforcement point under the action of prestress; The bridging force F of CFRP br The displacement at the reinforcement point caused by the action of It is the displacement caused by the shrinkage of CFRP due to the prestressed compression deformation of the metal plate.
[0018] In some possible embodiments, the strength factor K caused by the prestress pre Solve by the following formula:
[0019] ;
[0020] ;
[0021] In the formula, For prestressing, is the CFRP strip width, is the thickness of the CFRP strip, is the metal sheet width, is the metal sheet width.
[0022] In some possible embodiments, the total stress intensity factor K total , determine the minimum effective stress intensity factor amplitude ΔK in the global reinforcement position of the metal plate eff , including: based on the total stress intensity factor K total Determine the total stress intensity factor amplitude ΔK total , and the crack closure effect coefficient U is used to correct the effective stress intensity factor amplitude ΔK eff ; First fix the horizontal coordinate of the current fixed point and reduce the vertical coordinate to obtain the minimum ΔK in the y direction eff_y ; Then fix the minimum ΔK in the y direction eff_y The corresponding ordinate changes the abscissa to obtain the minimum ΔK in the x direction. eff_x , and finally obtain the minimum ΔK in the global reinforcement position of the metal plate eff .
[0023] In some possible embodiments, by comparing the effective stress intensity factor amplitude ΔK eff and stress intensity factor threshold ΔK th , determine whether the designed reinforcement position is successful in preventing cracks under the existing prestressing conditions, including: eff Less than or equal to ΔK th In the case of ΔK, it is determined that the designed reinforcement position can achieve complete fatigue crack arrest under the existing prestressing condition; eff Greater than ΔK thIn the case of a change in the reinforcement position coordinates, and recalculate ΔK eff Then compare ΔK again eff and ΔK th .
[0024] In some possible embodiments, the determining of the target reinforcement position with the best life extension effect includes: when crack arrest cannot be achieved, first fix the horizontal coordinate of the current fixed point, reduce the vertical coordinate, analyze the life extension effect of different reinforcement positions in the y direction, and compare the fatigue life of different schemes to obtain the maximum fatigue crack growth life N ymax , determine the best reinforcement position in the y direction; then fix the ordinate of the best reinforcement position in the y direction, change the abscissa, analyze the life extension effect of different reinforcement positions in the x direction, and compare the fatigue life of different schemes to obtain the maximum fatigue crack growth life N xmax , and finally the target reinforcement position with the best life extension effect is obtained; the y direction is the loading direction and the x direction is the crack propagation direction.
[0025] The beneficial effects brought about by the technical solution provided by the embodiment of the present invention include at least:
[0026] In the embodiment of the present invention, based on the mechanical reinforcement of the metal plate with the center crack by the prestressed CFRP strip, the total stress intensity factor K of the reinforced structure is calculated based on the linear elastic fracture mechanics, the stress intensity factor superposition method and the deformation coordination method. total The solution is divided into three parts and then further solved to obtain the minimum effective stress intensity factor amplitude ΔK in the global reinforcement position of the metal plate. eff and the stress intensity factor threshold ΔK th By comparison, the best crack arrest reinforcement position can be determined. If crack arrest cannot be achieved, the best life extension reinforcement position can be determined. This method can reveal the force transmission mechanism between metal siding and CFRP strips, analyze the effects of different reinforcement positions on fatigue crack arrest and life extension of metal plates with central cracks, predict the fatigue crack growth life and rate after prestressed reinforcement, and can be used to guide the design of prestressed CFRP strips for fatigue crack arrest and life extension. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0028] Figure 1 A schematic diagram of a structure of a metal plate with a center crack mechanically reinforced with a prestressed CFRP strip provided in an embodiment of the present invention;
[0029] Figure 2 A schematic flow chart of a method for prestressed crack arrest and life extension design of fatigue cracks provided in an embodiment of the present invention;
[0030] Figure 3 A theoretical model for splitting stress intensity factors using a stress intensity factor superposition method provided in an embodiment of the present invention;
[0031] Figure 4 A schematic diagram of a central cracked metal plate subjected to symmetrical loading of four-point concentrated forces provided by an embodiment of the present invention;
[0032] Figure 5 A flowchart for implementing the prestressed crack arrest and life extension design method for fatigue cracks provided in an embodiment of the present invention;
[0033] Figure 6 A schematic diagram showing the comparison between the prediction / experimental results and the finite element results of the fatigue crack growth life provided in an embodiment of the present invention;
[0034] Figure 7 A schematic diagram showing the comparison between the prediction / experimental results of fatigue crack growth rate and the finite element results provided in an embodiment of the present invention;
[0035] Figure 8 A schematic diagram comparing the predicted results and experimental results corresponding to the evolution process of strain with crack propagation in CFRP provided by an embodiment of the present invention;
[0036] Fig. 9 A schematic diagram showing the comparison results between the stress intensity factor calculated by the method provided in the embodiment of the present invention and the stress intensity factor calculated by the finite element method;
[0037] Fig.10 ΔK provided in the embodiment of the present invention eff Schematic diagram of crack arrest range analysis results;
[0038] Fig.11 A histogram of fatigue crack growth life under different reinforcement positions provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. The following embodiments are used to illustrate the present invention, but are not used to limit the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0040] In the following description, reference is made to “some embodiments”, which describe a subset of all possible embodiments, but it will be understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.
[0041] It should be pointed out that the terms "first\second\third" involved in the embodiments of the present invention are only used to distinguish similar objects and do not represent a specific ordering of the objects. It can be understood that "first\second\third" can be interchanged in a specific order or sequence where permitted, so that the embodiments of the present invention described here can be implemented in an order other than that illustrated or described here.
[0042] Those skilled in the art will appreciate that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art in the field to which the embodiments of the present invention belong. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with those in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as here.
[0043] Mechanical reinforcement of metal plates with central cracks by prestressed CFRP strips Principle: The CFRP strips are connected to the metal plates through mechanical clamps. The remote field load can be distributed to the CFRP strips through the stiffness principle to reduce the stress in the cracked metal plates. Since the CFRP strips and the metal plates are rigidly connected, a bridging effect is generated between the two to inhibit the cracks from opening. The prestress in the CFRP strips will also be transferred to the metal plates to inhibit the cracks from opening.
[0044] Figure 1 A schematic diagram of a structure of a metal plate with a center crack mechanically reinforced with a prestressed CFRP strip provided in an embodiment of the present invention is shown in FIG. Figure 1 As shown, a CFRP strip mechanically reinforces a metal crack plate with a central crack length of 2a. The CFRP strip is pre-tensioned before being connected to the metal plate in order to activate the prestress in the CFRP strip. Subsequently, the two ends of the CFRP strip are mechanically connected to the metal plate. Two CFRP strips of the same size are connected to the upper and lower surfaces of the metal plate, and are symmetrical about the two ends of the central crack. The prestress in the CFRP strip is transferred to the metal plate through the reinforcement point, causing the metal plate to shrink. When the metal plate is subjected to a uniform tensile load in the far field, the prestress will reduce the stress level at the crack tip and inhibit the crack from opening. Among them is the far-field uniform load, For prestressing, is the length of the metal plate, is the length of the CFRP strip, is the metal sheet width, is the CFRP strip width, is the thickness of the metal plate, is the thickness of the CFRP strip.
[0045] The generation and expansion of fatigue cracks bring immeasurable harm to metal structures. One of the reasons for the generation of fatigue cracks is that metal structures are subjected to long-term cyclic loads during service. When the crack grows to a certain stage, it will enter a stable expansion stage. Subsequently, the crack will continue to expand under cyclic loads until the structure breaks.
[0046] The embodiment of the present invention provides a method for prestressed crack arrest and life extension design of fatigue cracks. Figure 2 A schematic flow chart of a method for prestressed crack arrest and life extension design of fatigue cracks provided by an embodiment of the present invention, such as Figure 2 As shown, the method comprises at least the following steps:
[0047] Step S110, determining the size and material parameters, load parameters, and initial reinforcement point position coordinates of the metal plate with a central crack and the CFRP strip.
[0048] Here, dimensional parameters include width (w), thickness (t), length (L); material parameters include elastic modulus, Poisson's ratio and elastic strength; and load parameters of the structure include far-field tensile load and prestress.
[0049] Step S120: Based on the linear elastic fracture mechanics and the loading condition of the metal plate, the total stress intensity factor K of the reinforced structure is total Split into the intensity factor K caused by far-field load ff , Intensity factor K caused by bridging stress br and the strength factor K caused by prestress pre Solve them separately.
[0050] Here, K br The bridge force F is solved according to the deformation coordination method br Obtained later.
[0051] The stress intensity factor is a key parameter to measure the stress intensity at the crack tip, which can control the growth rate of fatigue cracks. In the design method of the present invention, the stress intensity factor is divided into three parts using the superposition method, such as Figure 3 And formula (1) shows:
[0052] Formula (1);
[0053] In the formula, K total is the total stress intensity factor of the reinforced structure, which is divided into the intensity factor K caused by the far-field load according to the loading condition of the structure. ff, Intensity factor K caused by bridging stress br and the strength factor K caused by prestress pre , the principle is as follows:
[0054] Before any reinforcement of the metal cracked plate, the remote field load All of it is borne by the metal crack plate, and the stress intensity factor at this time is K ff ; When the metal crack plate is connected to the CFRP, due to the different stiffness of the CFRP and the metal crack plate, a bridging force F is generated at the reinforcement position br The bridging force can inhibit the opening of fatigue cracks. The gravitational intensity factor generated by the bridging force is K br , solved by the displacement compatibility principle of the metal plate and the CFRP strip at the connection position; the CFRP is connected to the metal crack plate after pre-tensioning, and the prestress in the CFRP It will also be transferred to the metal crack plate through the reinforcement position. Simplified to concentrated force F pre , F pre With F br The direction and effect of action are the same, inhibiting the crack from opening. pre The stress intensity factor generated by the action of pre .
[0055] Step S130, based on the total stress intensity factor K total , determine the minimum effective stress intensity factor amplitude ΔK in the global reinforcement position of the metal plate eff .
[0056] Here, the stress intensity factor K total It is an important parameter to characterize the stress and strain field at the crack tip and can control the fatigue crack growth rate.
[0057] By adjusting the position of the initial reinforcement point , calculate the stress intensity factor amplitude ΔK at different positions total , and the crack closure effect coefficient U is used to correct ΔK eff Finally, we find the value that makes ΔK eff The location of the smallest reinforcement point, which usually means the greatest chance of crack arrest.
[0058] Step S140, by comparing the effective stress intensity factor amplitude ΔK eff and stress intensity factor threshold ΔK th , determine whether the designed reinforcement position can successfully stop cracks under the existing prestressing conditions.
[0059] Here, the stress intensity factor threshold ΔK of the material thIt is a material parameter and is used to determine whether fatigue cracks extend. eff Less than ΔK th , it is considered that the fatigue crack can be arrested.
[0060] Step S150, when crack arrest cannot be achieved at any reinforcement point, fatigue crack growth life is calculated by using the Paris relationship to determine the target reinforcement position with the best life extension effect.
[0061] Here, if fatigue crack arrest cannot be achieved through reinforcement, that is, it is impossible to find a solution that satisfies ΔK eff Less than ΔK th The reinforcement position under this condition needs to be designed for life extension analysis. In other words, find the reinforcement point position that can maximize the fatigue crack growth life N. Optimize N by adjusting the position of the reinforcement point. Finally, determine the best reinforcement solution by comparing the fatigue crack growth life and growth rate under different reinforcement positions.
[0062] In the embodiment of the present invention, based on the mechanical reinforcement of the metal plate with the center crack by the prestressed CFRP strip, the total stress intensity factor K of the reinforced structure is calculated based on the linear elastic fracture mechanics, the stress intensity factor superposition method and the deformation coordination method. total The solution is divided into three parts and then further solved to obtain the minimum effective stress intensity factor amplitude ΔK in the global reinforcement position of the metal plate. eff and the stress intensity factor threshold ΔK th By comparison, the best crack arrest reinforcement position can be determined. If crack arrest cannot be achieved, the best life extension reinforcement position can be determined. This method can reveal the force transmission mechanism between metal siding and CFRP strips, analyze the effects of different reinforcement positions on fatigue crack arrest and life extension of metal plates with central cracks, predict the fatigue crack growth life and rate after prestressed reinforcement, and can be used to guide the design of prestressed CFRP strips for fatigue crack arrest and life extension.
[0063] In some possible embodiments, the intensity factor K caused by the far-field load is ff It can be calculated according to the stress intensity factor manual, as shown in formulas (2) and (3):
[0064] Formula (2);
[0065] Formula (3);
[0066] Among them, β ff is the geometric correction factor, is the far-field uniform load, a is half of the total crack length, is the metal sheet width.
[0067] K br It is due to the bridging force The four-point symmetrical loading of the metal plate at the center crack is generated, and the four-point concentrated force is in the form of Figure 4 shown. It is solved by the complex function solution developed by Tada et al. based on the Westergaard stress function. This solution has two key points: one is to establish a global rectangular coordinate system with the crack center as the origin; the other is the finite plate width correction factor. In the embodiment of the present invention, a new geometric finite plate width correction factor is introduced to make The solution is more accurate, which is also the key point that makes the method proposed in the embodiment of the present invention have global applicability.
[0068] In some possible embodiments, assuming that the reinforcement center crack length is 2a, the intensity factor K caused by the bridging stress is br It is solved by the following formula:
[0069] Formula (4);
[0070] Formula (5);
[0071] Formula (6);
[0072] Formula (7);
[0073] In the formula, is the geometric correction factor of a metal plate with a central crack under four-point concentrated force loading, is the thickness of the metal plate, is the Poisson’s ratio of the metal plate, is the coordinate of the initial reinforcement point, y is the ordinate of any position of the cracked plate metal plate, and is the complex function expression of the four-point concentrated force position coordinates in the crack plate global coordinate system; F br The bridging force is solved by the deformation coordination relationship between the metal crack plate and the CFRP strip at the reinforcement point; is the stress distribution in the cross section in front of the crack tip where no crack occurs in the direction of the far-field load.
[0074] The embodiment of the present invention innovatively derives the geometric correction factor of a central crack under four-point concentrated force loading , which makes the stress intensity factor calculation of the reinforced structure globally accurate, and its accuracy is no longer limited by the reinforcement position, which also lays the foundation for determining the optimal crack arrest position and life extension position later.
[0075] In some possible embodiments, the deformation coordination relationship is represented by the following formula:
[0076] Formula (8);
[0077] Where V ff is the displacement of the metal plate at the reinforcement point under the action of the far-field load; V br is the bridge force F of the metal plate br The displacement at the reinforcement point caused by the action of V pre It is the displacement of the metal plate at the reinforcement point under the action of prestress; is the bridging force F of the CFRP strip br The displacement at the reinforcement point caused by the action of It is the displacement caused by the contraction of the CFRP strips due to the prestressed compression deformation of the metal plate.
[0078] By solving formula (8), we can get the bridging force F br , we can use formulas (4) to (7) to solve for K br .
[0079] For the structure of a metal wall plate with a central crack mechanically reinforced with a prestressed CFRP strip, the deformation coordination relationship used in the prestressed crack arrest and life extension design method provided in the embodiment of the present invention can more accurately calculate and analyze the force transfer model between the metal crack plate and the CFRP strip. Thus, the crack growth life and fatigue crack growth rate of the fatigue crack can be predicted and the bridging stress changes in the CFRP strip can be accurately captured.
[0080] In some possible embodiments, the strength factor F caused by prestressing pre is the stress intensity factor generated by the prestress, which simplifies the prestress in the CFRP strip into a concentrated force F pre , as shown in formula (9). pre The effect of F br The same, so K pre The solution is shown in formula (10).
[0081] Formula (9);
[0082] Formula (10);
[0083] In the formula, For prestressing, is the CFRP strip width, is the thickness of the CFRP strip, is the metal sheet width, is the thickness of the metal plate.
[0084] Applying the above formula (1) to obtain K total Afterwards, it can be substituted into the Paris formula to calculate the fatigue crack growth rate, as shown in formula (11):
[0085] Formula (11);
[0086] Where da / dN is the crack growth rate, ΔK eff is the effective stress intensity factor amplitude, C and m are material constants. Further, the fatigue crack growth life N can be solved by combining the crack length 2a.
[0087] In some possible embodiments, the total stress intensity factor K total , determine the minimum effective stress intensity factor amplitude ΔK in the global reinforcement position of the metal plate eff , including: based on the total stress intensity factor K total Determine the total stress intensity factor amplitude ΔK total , and the crack closure effect coefficient U is used to correct the effective stress intensity factor amplitude ΔK eff ; First fix the horizontal coordinate of the current fixed point and reduce the vertical coordinate to obtain the minimum ΔK in the y direction eff_y ; Then fix the minimum ΔK in the y direction eff_y The corresponding ordinate changes the abscissa to obtain the minimum ΔK in the x direction. eff_x , and finally obtain the minimum ΔK in the global reinforcement position of the metal plate eff .
[0088] Here, usually during the unloading process of the tensile load, the crack tip undergoes plastic deformation during the load cycle, resulting in the crack closing before the tensile load is unloaded to zero. This is the so-called crack closure effect. Therefore, the total stress intensity factor amplitude ΔK calculated by formula (12) is total The crack closure effect coefficient U needs to be used for correction, as shown in formula (13), so as to obtain ΔK eff , U is related to the stress ratio R.
[0089] Formula (12);
[0090] Formula (13);
[0091] In the formula, and They represent the maximum and minimum stress intensity factors at the crack tip under each cyclic loading.
[0092] In some possible embodiments, by comparing the effective stress intensity factor amplitude ΔK eff and stress intensity factor threshold ΔK th , determine whether the designed reinforcement position is successful in preventing cracks under the existing prestressing conditions, including: eff Less than or equal to ΔK th In the case of ΔK, it is determined that the designed reinforcement position can achieve complete fatigue crack arrest under the existing prestressing condition; eff Greater than ΔK th In the case of a change in the reinforcement position coordinates, and recalculate ΔK eff Then compare ΔK again eff and ΔK th .
[0093] Here, the reinforcement point position is continuously moved, if ΔK eff Less than or equal to ΔK th , it means that the designed reinforcement position can achieve complete fatigue crack arrest under the existing prestressing condition. eff Greater than ΔK th, This indicates that the stress state may lead to crack growth and that measures need to be taken, such as using a new reinforcement design, recalculating the stress intensity factor and ΔK eff , again compare ΔK eff With ΔK th , to ensure that the new reinforcement design can meet the requirements of complete fatigue crack arrest. When crack arrest cannot be achieved regardless of the location of the reinforcement point, the next best option is to conduct life extension analysis and design.
[0094] In some possible embodiments, the determining of the target reinforcement position with the best life extension effect includes: when crack arrest cannot be achieved, first fix the horizontal coordinate of the current fixed point, reduce the vertical coordinate, analyze the life extension effect of different reinforcement positions in the y direction, and compare the fatigue life of different schemes to obtain the maximum fatigue crack growth life N ymax , determine the best reinforcement position in the y direction; then fix the ordinate of the best reinforcement position in the y direction, change the abscissa, analyze the life extension effect of different reinforcement positions in the x direction, and compare the fatigue life of different schemes to obtain the maximum fatigue crack growth life N xmax , and finally the target reinforcement position with the best life extension effect is obtained; the y direction is the loading direction and the x direction is the crack propagation direction.
[0095] Here, on the one hand, by adjusting the position of the reinforcement point, the stress intensity factor change ΔK at different positions is calculated. eff The goal is to find a value that makes ΔK effThe smallest reinforcement point position, which usually means the least possibility of crack extension. On the other hand, the fatigue crack extension life N is optimized by adjusting the position of the reinforcement point, and the reinforcement point position that can maximize N is found. Finally, the fatigue crack extension life and fatigue crack extension rate after reinforcement at different extension positions are analyzed and compared with each other, and the reinforcement position with the longest life and the slowest extension rate is determined as the best reinforcement solution.
[0096] In this way, through the analysis of this design method, the influence of different reinforcement positions on crack arrest and life extension can be accurately analyzed.
[0097] The above-mentioned prestressed crack arrest and life extension design method for fatigue cracks is described below in conjunction with a specific embodiment. However, it should be noted that this specific embodiment is only for better illustrating the present invention and does not constitute an improper limitation to the present invention.
[0098] At present, the research on fatigue crack prestressing crack arrest and life extension is mainly based on experimental research. Some scholars have conducted theoretical analysis, but the theoretical analysis is not accurate and is subject to many limitations. For example, when the reinforcement position is close to the crack surface, the analysis result has a large error.
[0099] The embodiment of the present invention provides a novel design method for prestressed crack arrest and life extension of fatigue cracks based on linear elastic fracture mechanics, stress intensity factor superposition method and deformation coordination method, and experimentally verifies the method. The design method can reveal the force transmission mechanism between metal siding and CFRP strips, analyze the influence of different reinforcement positions on prestressed crack arrest and life extension, predict the fatigue crack growth life and rate after prestressed reinforcement, and can be used to guide the design of prestressed CFRP strips for fatigue crack arrest and life extension.
[0100] The embodiment of this aspect provides a prestressed crack arrest and life extension design method for fatigue cracks based on mechanical reinforcement of a metal plate containing a central crack with a prestressed CFRP strip. The implementation process is as follows: Figure 5 As shown, it is divided into the following steps:
[0101] In the first step, it is necessary to determine the parameter information of the reinforced structure, which are the dimensions of the metal plate and CFRP strip (width w, thickness t, length L) and material parameters (elastic modulus, Poisson's ratio and elastic strength), the initial crack length (a0), the known load parameters of the structure (far-field uniform tensile load, prestress) and the initial reinforcement point position coordinates.
[0102] The second step is to divide the stress intensity factor of the structure into K, based on the foundation of linear elastic fracture mechanics and the stress intensity factor superposition method. ff , K br and K pre , respectively, using the formulas derived in the above embodiments to solve, where K brThe bridge force F needs to be solved according to the deformation coordination method br Only then can you obtain it.
[0103] The third step is to fix the horizontal coordinate of the current fixed point and reduce the vertical coordinate to obtain the minimum ΔK in the y direction. eff_y ; Then fix the minimum ΔK in the y direction eff_y The corresponding ordinate changes the abscissa to obtain the minimum ΔK in the x direction. eff_x , and finally obtain the minimum ΔK in the global reinforcement position of the metal plate eff . The required ΔK eff and stress intensity factor threshold ΔK th Compare, if ΔK eff < ΔK th , it means that the designed reinforcement position can achieve complete fatigue crack arrest under the existing prestressing condition. When crack arrest cannot be achieved no matter where the reinforcement point is located, the life extension analysis and design can be carried out as a fallback.
[0104] The fourth step, life extension analysis and design, is carried out when crack arrest cannot be achieved. First, fix the horizontal coordinate of the current fixed point, reduce the vertical coordinate, and obtain the maximum fatigue crack growth life N in the y direction. ymax ; Then fix the maximum N in the y direction ymax Corresponding to the ordinate, change the abscissa and obtain the maximum fatigue crack growth life N in the x direction xmax , so as to obtain the maximum N in the global reinforcement position of the metal plate and the target reinforcement position with the best life extension effect.
[0105] Through this design method, the fatigue crack growth life and fatigue crack growth rate after reinforcement at different positions are analyzed and compared with each other to determine the reinforcement position with the longest life and the slowest growth rate.
[0106] In order to prove the accuracy and feasibility of the implementation of the present invention, the prediction results of the present invention are compared with the experimental results. Figure 6 and Figure 7 As shown in the results, the predicted results of fatigue crack growth life and rate are in good agreement with the experimental results and finite element results. Figure 8 It can be seen that the embodiment of the present invention can also accurately capture the changes in stress or strain during the entire fatigue crack propagation process of CFRP. The comparison results show that the prediction results of the method of the present invention have good accuracy and feasibility.
[0107] The obvious effects brought by the embodiments of the present invention are as follows:
[0108] 1) By changing the vertical coordinate of the reinforcement point, a lower stress intensity factor can be obtained, making it lower than ΔKth , to achieve fatigue crack arrest. Fig. 9 and Fig.10 As shown in the figure, when the far-field load is 120MPa and the prestress is 750MPa, ΔK th =200MPa, keep the horizontal coordinate of the reinforcement position unchanged, reduce the vertical coordinate of the reinforcement position, and obtain the minimum ΔK at y0=30mm (millimeter) total , and is less than ΔK th , achieving the arrest of fatigue cracks. When the far-field load was increased at y0=30mm, it was found that the metal crack plate could withstand 10% more far-field load than the previous 120MPa.
[0109] 2) In the case where the existing prestressing conditions cannot stop cracking, the embodiment of the present invention can determine the best life extension position, such as Fig.11 As shown. When the initial crack length is 8.5 mm, the reinforcement point position is changed, and the fatigue crack growth life and rate under different reinforcement positions are calculated. This design method can accurately calculate the fatigue crack growth life and rate under any reinforcement position, and the best life extension scheme can be determined without experiments and finite element methods.
[0110] It should be understood that "one embodiment" or "an embodiment" mentioned throughout the specification means that specific features, structures or characteristics related to the embodiment are included in at least one embodiment of the present invention. Therefore, "in one embodiment" or "in an embodiment" appearing throughout the specification does not necessarily refer to the same embodiment. In addition, these specific features, structures or characteristics can be combined in one or more embodiments in any suitable manner. It should be understood that in various embodiments of the present invention, the size of the serial number of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiment of the present invention. The serial numbers of the above-mentioned embodiments of the present invention are only for description and do not represent the advantages and disadvantages of the embodiments.
[0111] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0112] The methods disclosed in several method embodiments provided by the present invention can be arbitrarily combined without conflict to obtain new method embodiments. The features disclosed in several method embodiments provided by the present invention can be arbitrarily combined without conflict to obtain new method embodiments.
[0113] The above is only an embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A prestressed crack arrest and life extension design method for fatigue cracks, characterized in that: include: Determine the size and material parameters, load parameters, and initial reinforcement point coordinates of the metal plate with a central crack and the carbon fiber reinforced polymer CFRP strip; Based on the linear elastic fracture mechanics and the loading conditions of the metal plate, the total stress intensity factor of the reinforced structure is K total Split into stress intensity factors due to far-field loads K ff , Intensity factor due to bridging stress K br and the stress intensity factor caused by prestress K pre Solve separately; in, K br The bridge force is solved according to the deformation coordination method F br Afterwards, Based on the total stress intensity factor K total , determine the minimum effective stress intensity factor amplitude in the global reinforcement position of the metal plate ΔK eff ; By comparing the effective stress intensity factor amplitude ΔK eff and stress intensity factor threshold ΔK th , determine whether the designed reinforcement position is successful in arresting cracks under the existing prestressing conditions; When crack arrest cannot be achieved at any reinforcement point, the fatigue crack growth life is calculated using the Paris relationship to determine the target reinforcement position with the best life extension effect; Assuming the length of the reinforcement center crack is 2 a , the bridging stress-induced intensity factor K br It is solved by the following formula: ; ; ; ; In the formula, is half the crack length, is the intermediate variable, is the geometric correction factor of a metal plate with a central crack under four-point concentrated force loading, is the thickness of the metal plate, is the Poisson’s ratio of the metal plate, is the initial reinforcement point position coordinate, is an imaginary unit, y is the ordinate of any position on the metal plate, and It is the complex function expression of the coordinates of the four-point concentrated force positions in the global coordinate system of the cracked plate; F br The bridging force is solved by the deformation coordination relationship between the metal crack plate and the CFRP strip at the reinforcement point; is the metal sheet width, is the stress distribution of the cross section in front of the crack tip where no crack occurs in the far-field load direction; The deformation coordination relationship is characterized by the following formula: ; In the formula, is the displacement of the metal plate at the reinforcement point under the action of the far-field load; The metal plate is in the bridge force Displacement caused at the reinforcement point under action; It is the displacement of the metal plate at the reinforcement point under the action of prestress; Is CFRP in bridging force The displacement at the reinforcement point caused by the action of It is the displacement caused by the contraction of the CFRP strips due to the prestressed compression deformation of the metal plate.
2. The method according to claim 1, characterized in that: The strength factor caused by the prestress K pre Solve by the following formula: ; ; In the formula, For prestressing, To simplify the concentrated force of prestressing, is the CFRP strip width, is the thickness of the CFRP strip, is the metal sheet width, is the thickness of the metal plate.
3. The method according to claim 1, characterized in that The total stress intensity factor based on , determine the minimum effective stress intensity factor amplitude in the global reinforcement position of the metal plate ,include: Based on the total stress intensity factor Determine the total stress intensity factor magnitude , and using the crack closure effect coefficient U The effective stress intensity factor amplitude is obtained by correction ; First fix the horizontal coordinate of the current fixed point and reduce the vertical coordinate to obtain y The smallest direction ; Then fix the y The smallest direction The corresponding ordinate, change the abscissa to obtain x The smallest direction , and finally obtain the smallest .
4. The method according to claim 3, characterized in that By comparing the effective stress intensity factor amplitude and stress intensity factor threshold , determine whether the designed reinforcement position is successful in arresting cracks under the existing prestressing conditions, including: exist Less than or equal to In the case of , it is determined that the designed reinforcement position can achieve complete fatigue crack arrest under the existing prestressing conditions; exist Greater than In the case of a change in the reinforcement position coordinates, and recalculate Then compare again and .
5. The method according to any one of claims 1 to 4, characterized in that: Determining the target reinforcement position with the best life extension effect includes: When crack arrest cannot be achieved, first fix the horizontal coordinate of the current fixed point, reduce the vertical coordinate, and analyze the y The life extension effect of different reinforcement positions in different directions, and the fatigue life of different schemes are compared to obtain the maximum fatigue crack growth life , confirm in y The best reinforcement position in the direction; re-fix y The ordinate of the best reinforcement position in the direction, changing the abscissa, analyzes x The life extension effect of different reinforcement positions in different directions, and the fatigue life of different schemes are compared to obtain the maximum fatigue crack growth life , Ultimately, the best life extension effect y Direction is the target reinforcement position; where the loading direction is x The direction is the crack propagation direction.