A new bismuth MOFs catalytic material and its preparation method and application
Through the three-dimensional framework structure and low coordination number design of the new bismuth agent MOFs catalytic material, the problems of high energy barrier and low selectivity in the electrocatalytic carbon dioxide reduction reaction are solved, and efficient and selective catalysis for the efficient reduction of CO2 to formic acid is achieved. Effect.
Patent Information
- Application Number
- CN202411054119.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing technology has the problems of high energy barrier limitation and low product selectivity in the electrocatalytic carbon dioxide reduction reaction. In particular, the reaction in aqueous solution is excessive and the competitive reaction-hydrogen evolution reaction is serious, making it difficult to develop efficient and selective catalysts.
Using a new bismuth agent MOFs catalytic material formed by a three-dimensional framework structure, trivalent bismuth and N,N'-bis(terphenyl-4,4''-di Formic acid) naphthalene diimine ligands are connected to water molecule ligands to form a catalyst with high porosity, which lowers the energy barrier for CO2 reduction and inhibits the hydrogen evolution reaction.
The efficient reduction of CO2 to formic acid is achieved, which significantly improves the catalytic reaction rate and selectivity. The porosity of the catalyst reaches 70%-76%, ensuring the stability and efficient catalytic effect of the catalyst.
Smart Images

Figure CN118581494B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalyst technology, and in particular to a novel bismuth MOFs catalytic material and a preparation method and application thereof. Background Art
[0002] The electrocatalytic carbon dioxide reduction reaction (CO2RR) is a catalytic reaction that converts carbon dioxide into valuable chemicals or fuels. In this process, carbon dioxide molecules, under the action of catalysts, undergo multi-electron and proton transfer processes in electrolyte solutions to form various hydrocarbons and carbon oxides, such as CO, HCOOH, CH4 or C2H4. These products can be used not only as chemical raw materials, but also as energy storage media. Electrocatalytic carbon dioxide reduction technology makes it possible to achieve effective utilization of carbon dioxide and reduce greenhouse gas emissions, and is one of the current research hotspots.
[0003] However, CO2RR still faces some challenges. The linear CO2 molecule has a stable structure, in which the breaking of the C=O bond requires a high energy barrier, which limits the efficient conversion of CO2. CO2 reduction involves complex multi-electron / proton transfer steps, making the preparation of a single product a huge challenge. In addition, since the reaction process is carried out in aqueous solution and the overpotential is low, the competing reaction - hydrogen evolution reaction is extremely intense, further affecting the selectivity of the product. Therefore, the development of efficient catalysts to achieve high activity and high selectivity reduction of CO2 has important research significance and application prospects.
[0004] In the prior art, although MOFs are often used as catalyst materials, the final unit cell, bismuth coordination number, structure and catalytic effect are completely different due to the different ligands connected to MOFs. In Chinese patent CN115028848A, a Bi-based MOFs catalyst is recorded, the ligand is 2-mercapto-4-methyl-5-thiazoleacetic acid, and the final product is a bismuth with five coordination, which can be used as a catalyst for oxidizing phenylboric acid to phenol. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a novel bismuth MOFs catalytic material and a preparation method and application thereof. The bismuth MOFs catalytic material of the present invention can efficiently reduce CO2 to formic acid.
[0006] The invention provides a novel bismuth-based MOFs catalytic material. The catalyst is formed by doubly interlacing a three-dimensional framework structure. The catalyst structure is formed by sequentially connecting a plurality of minimum asymmetric repeating structural units. The minimum asymmetric repeating unit uses trivalent bismuth in a spatial coordination configuration of a seven-coordinated capped triangular pyramid as a metal node, and three N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligands and one water molecule ligand are connected around the metal node. The Bi atom of the current minimum asymmetric repeating structural unit forms a Bi-O bond with an O atom of the N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligand in an adjacent repeating structural unit to achieve three-dimensional connection to form a three-dimensional framework structure.
[0007] Furthermore, the porosity of the catalytic material is 70%-76%.
[0008] Furthermore, the unit cell parameters of the catalytic material are a=47.3857Å, b=17.3285Å, c=49.1655Å, α=β=90°, γ=118.178°, and the unit cell volume is 35586.37Å. 3 .
[0009] Furthermore, the XRD of the catalytic material has characteristic diffraction peaks at 6.2°, 7.4°, 7.6°, 8.2°, 8.5°, 10.9°, and 12.8° in an X-ray powder diffraction pattern represented by a diffraction angle 2θ.
[0010] The present invention also provides a method for preparing the bismuth MOFs catalytic material, the preparation method comprising:
[0011] Bismuth nitrate (Bi(NO3)3), N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide, formic acid and N,N'-dimethylformamide are uniformly mixed and reacted to obtain an intermediate product. The intermediate product is washed and dried with N,N'-dimethylformamide to obtain a bismuth MOFs catalytic material.
[0012] Furthermore, the purpose of the uniform mixing is to promote sufficient reaction between the raw materials, and those skilled in the art can achieve this by using ultrasound and stirring methods.
[0013] Furthermore, after uniform mixing, the molar concentration of the bismuth nitrate is 0.003 mol / L-0.013 mol / L.
[0014] Furthermore, after uniform mixing, the molar concentration of the bismuth nitrate is 0.008 mol / L.
[0015] Furthermore, the molar ratio of the bismuth nitrate to N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide is 0.01-0.04:0.005-0.02.
[0016] Furthermore, the molar ratio of the bismuth nitrate to N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide is 0.025:0.0095.
[0017] Furthermore, the volume ratio of formic acid to N,N'-dimethylformamide is 0.01-0.1:3.
[0018] Furthermore, the volume ratio of formic acid to N,N'-dimethylformamide is 0.045:3.
[0019] Furthermore, the specific steps of the reaction are: heating to 60°C-120°C at a heating rate of 5°C / h-10°C / h, conducting a constant temperature reaction for 70h-80h, and then cooling to 25°C-35°C at a cooling rate of 25°C / 36h-95°C / 36h.
[0020] Furthermore, the specific steps of the reaction are: heating to 120°C at a heating rate of 10°C / h, conducting a constant temperature reaction for 72h, and then cooling to 30°C at a cooling rate of 90°C / 36h.
[0021] Furthermore, the drying temperature is 55° C.-65° C., and the drying time is 11 h-13 h.
[0022] The present invention also provides the use of the bismuth MOFs catalytic material in catalytic reduction of CO2 to formic acid.
[0023] The embodiments of the present invention have the following technical effects:
[0024] 1. The metal organic framework material in the present invention is a type of crystalline material with a highly ordered porous structure formed by self-assembly of metal ions or metal clusters and organic ligands through coordination bonds. The bismuth-based metal organic framework material (Bi-MOFs) formed by coordination bonds between bismuth ions and organic ligands shows high selectivity in reducing CO2 to formic acid. This is because when CO2 is converted to formic acid, the CO2 molecule needs to be adsorbed on the active site first, and then reduced to , and then obtain protons to reduce to HCOO-. Bi can significantly reduce The formation energy barrier of formic acid can be reduced and the generation of -H, an important intermediate in the hydrogen evolution reaction, can be inhibited, thereby efficiently reducing CO2 to formic acid.
[0025] 2. In the present invention, a seven-coordinated bismuth is obtained by coordinating bismuth with three N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalene diimide ligands and one water molecule ligand. In the electrocatalytic CO2 reduction process, the coordination number of the active site has an important influence on the performance. On the one hand, a lower coordination number is beneficial to the interaction between the reaction substrate and the metal active site, promoting the activation of CO2 molecules, thereby increasing the catalytic reaction rate; on the other hand, a low coordination number is beneficial to reducing the The generation energy of the intermediate can change the CO2 reduction path and improve the selectivity of the reaction; in addition, the present invention has N, N'-bis (terphenyl-4,4''-dicarboxylic acid) naphthalene diimide ligand, which has redox properties and is beneficial to improving the charge transfer in the catalytic process. Secondly, the porosity of the catalytic material is crucial to the material transport in the reaction process. The porosity of the catalyst of the present invention is as high as 70%-76%, which is beneficial to the enrichment and transmission of CO2 molecules in the catalytic process. Finally, the catalyst in the present invention has a three-dimensional framework structure that is double-interpenetrated, which ensures that the catalyst can make the overall structure of the catalyst more stable under the condition of high porosity, and further improve the catalytic effect of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 It is a schematic diagram of the minimum asymmetric repeating structural unit provided by an embodiment of the present invention.
[0028] Figure 2 This is the spatial coordination configuration of the seven-coordinate capped triangular pyramid provided by the embodiment of the present invention.
[0029] Figure 3 The three-dimensional frame structure provided by the embodiment of the present invention is double interlaced.
[0030] Figure 4 It is a Fourier infrared spectrum diagram provided by an embodiment of the present invention.
[0031] Figure 5 It is the XRD diagram provided by the embodiment of the present invention.
[0032] Figure 6 is a test result diagram of an embodiment of the present invention, wherein: Figure 6 Figure a is the Faraday efficiency diagram of the catalyst selecting formic acid at a voltage of -0.9~-1.6V. Figure 6 Figure b is the actual current density diagram of the catalyst selecting formic acid at a voltage of -0.9~-1.6V. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0034] In the first aspect, some embodiments of the present invention provide a novel bismuth-containing MOFs catalytic material, wherein the catalyst is formed by doubly interlacing a three-dimensional framework structure, and the catalyst structure is formed by sequentially connecting a number of minimum asymmetric repeating structural units; the minimum asymmetric repeating unit uses trivalent bismuth in a spatial coordination configuration of a seven-coordinated capped triangular pyramid as a metal node, and connects three N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligands and one water molecule ligand around the metal node; the Bi atom of the current minimum asymmetric repeating structural unit forms a Bi-O bond with the O atom of the N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligand in the adjacent repeating structural unit to achieve three-dimensional connection to form a three-dimensional framework structure.
[0035] In the present invention, a seven-coordinated bismuth is obtained. On the one hand, a lower coordination number is beneficial to the interaction between the reaction substrate and the metal active site, promoting the activation of CO2 molecules, thereby increasing the catalytic reaction rate; on the other hand, a low coordination number is beneficial to certain special reaction intermediates such as The generation of CO2 can change the CO2 reduction path and improve the selectivity of the reaction. The catalyst has a three-dimensional framework structure that is double-interlaced, which can make the overall structure more stable and further enhance the catalytic effect of the catalyst.
[0036] In some embodiments, the porosity of the catalytic material is 70%-76%.
[0037] The catalyst of the present invention has a high porosity, which is beneficial to the enrichment and transmission of CO2 molecules during the catalytic process.
[0038] In some embodiments, the unit cell parameters of the catalytic material are a=47.3857Å, b=17.3285Å, c=49.1655Å, α=β=90°, γ=118.178°, and the unit cell volume is 35586.37Å. 3 .
[0039] In some embodiments, the catalytic material has characteristic diffraction peaks at 6.2°, 7.4°, 7.6°, 8.2°, 8.5°, 10.9°, and 12.8° in an X-ray powder diffraction pattern represented by a diffraction angle 2θ.
[0040] In a second aspect, some embodiments of the present invention also provide a method for preparing the bismuth MOFs catalytic material, the preparation method comprising:
[0041] Bismuth nitrate, N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide, formic acid and N,N'-dimethylformamide are uniformly mixed and reacted to obtain an intermediate product. The intermediate product is washed and dried with N,N'-dimethylformamide to obtain a bismuth MOFs catalytic material.
[0042] In the method of the present invention, the catalyst of the present invention is obtained by selecting the ligands and the number of ligands that coordinate with bismuth. It should be understood by those skilled in the art that the formation of the catalyst is not only related to the selection of raw materials, but also to the reaction conditions, and the selection of reaction conditions is often determined by the properties of the raw materials. If the parameter conditions and the properties of the raw materials do not match, the structure of the catalyst of the present invention cannot be formed. Therefore, only by the parameters in the method of the present invention can the interaction between the raw materials be achieved, and finally the catalyst of the present invention can be obtained.
[0043] In some embodiments, after uniform mixing, the molar concentration of the bismuth nitrate is 0.003 mol / L-0.013 mol / L.
[0044] In some embodiments, after uniform mixing, the molar concentration of the bismuth nitrate is 0.008 mol / L.
[0045] In some embodiments, the molar ratio of bismuth nitrate to N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide is 0.01-0.04:0.005-0.02.
[0046] In some embodiments, the molar ratio of bismuth nitrate to N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide is 0.025:0.0095.
[0047] In some embodiments, the volume ratio of formic acid to N,N'-dimethylformamide is 0.01-0.1:3.
[0048] In some embodiments, the volume ratio of formic acid to N,N'-dimethylformamide is 0.045:3.
[0049] In some embodiments, the specific steps of the reaction are: heating to 60°C-120°C at a heating rate of 5°C / h-10°C / h, conducting a constant temperature reaction for 70h-80h, and then cooling to 25°C-35°C at a cooling rate of 25°C / 36h-95°C / 36h.
[0050] In some embodiments, the specific steps of the reaction are: heating to 120°C at a heating rate of 10°C / h, conducting a constant temperature reaction for 72h, and then cooling to 30°C at a cooling rate of 90°C / 36h.
[0051] In some embodiments, the drying temperature is 55° C.-65° C., and the drying time is 11 h-13 h.
[0052] In a third aspect, some embodiments of the present invention also provide the use of the bismuth-containing MOFs catalytic material in the catalytic reduction of CO2 to formic acid.
[0053] The following is described in conjunction with some specific embodiments:
[0054] Embodiment 1:
[0055] Bismuth nitrate (0.025mmol), N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalene diimide (0.0095mmol), formic acid (45μL), and N,N'-dimethylformamide (3mL) were added into a high temperature resistant glass vial and mixed evenly to obtain a mixture; the mixture was sealed and heated to 120°C for 12h, then kept at 120°C for 72h, and then cooled to 30°C for 36h to obtain an intermediate product; the intermediate product was washed with N,N'-dimethylformamide and dried (drying temperature 60°C, drying time 12h) to obtain a bismuth MOFs catalytic material, recorded as Bi-BTD.
[0056] The catalyst obtained in the example was tested: the catalyst was placed in a liquid flow cell, under the reaction conditions of 1M KCl electrolyte (potassium chloride electrolyte), the potential range was -1.1V~-1.6V, and CO2 was reduced to HCOOH.
[0057] Results and analysis:
[0058] Table 1 Comparison of the performance of Bi-MOFs catalysts in the examples and prior art
[0059]
[0060] The method of the present invention successfully obtains a Bi-based MOFs catalyst material. Figure 1-Figure 3 Can be verified. Figure 1-Figure 2It can be found that the catalyst of the present invention is composed of a number of minimum asymmetric repeating structural units connected in sequence, wherein the minimum asymmetric repeating unit uses trivalent bismuth in a spatial coordination configuration of a seven-coordinated capped triangular pyramid as a metal node, and three N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligands and one water molecule ligand are connected around the metal node; the Bi atom of the current minimum asymmetric repeating structural unit forms a Bi-O bond with the O atom of the N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligand in the adjacent repeating structural unit, and the final three-dimensional framework structure of the catalyst is doubly interlaced, that is, Figure 3 structure.
[0061] exist Figure 4 It can be found that the infrared spectrum of Bi-BTD in the present invention compared with N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalene diimide (H4BTD) shows that the -1 The characteristic peak corresponding to the -C=O stretching vibration is red-shifted, indicating that the -COOH in the ligand is coordinated with the Bi ion.
[0062] exist Figure 5 , which are the XRD characteristic diffraction peaks of the catalyst of the present invention. The XRD of the catalytic material is represented by an X-ray powder diffraction pattern with a diffraction angle of 2θ, and has characteristic diffraction peaks at 6.2°, 7.4°, 7.6°, 8.2°, 8.5°, 10.9°, and 12.8°.
[0063] Through the method of the present invention, a new Bi-based MOFs catalyst material is successfully obtained. The catalyst of the present invention is compared with the catalyst in the prior art, and the results are shown in Table 1. It can be found from Table 1 that the catalyst of the present invention has a lower coordination number than common classical Bi-MOFs catalytic materials such as CAU-17 (see Li F, Gu GH et al., Appl Catal B, 2020, 277:119241), Bi(bit) (see Lamagni P, Miola M et al., Advanced Functional Materials, 30, No. 16 (2020) 1910408) and V12 (see Zhu ZH, Liang ZL et al., Energy Chemistry (English Edition), 63 (2021) 328-335). 2021, 63: 328-335.)) etc., and the lower coordination number of the present invention is not only conducive to the interaction between the reaction substrate and the metal active site, promoting the activation of CO2 molecules, thereby increasing the catalytic reaction rate; and the low coordination number is conducive to reducing the bismuth site The formation energy of the intermediates can change the CO2 reduction pathway and improve the selectivity of the reaction. The FE in Table 1 can be used to calculate the HCOOH The data (Faraday efficiency) show that the higher the Faraday efficiency, the higher the selectivity of the catalyst. It can be seen that the catalyst of the present invention has a higher selectivity for formic acid. HCOOHData (current density), the greater the current density, the better the activity of the catalyst. The present invention has N, N'-bis (terphenyl-4,4''-dicarboxylic acid) naphthalene diimide ligands, which have redox properties and are conducive to improving charge transfer in the catalytic process. It can be seen that the catalytic activity of the catalyst of the present invention is significantly better than the prior art, even 10-26 times that of the prior art. Finally, it can be found in Table 1 that the catalyst of the present invention also has a wider optional voltage range and can be applied to more environments. In summary, the catalyst of the present invention has higher selectivity, catalytic activity and a wide application environment due to the selection of ligands, unit cell structure, morphology and structure. Excellent catalytic potential. In addition, the catalyst of the present invention also has a higher porosity. The porosity of the catalyst of the present invention is as high as 73%, while the porosity of CAU-17 in the prior art is 44.1%, the porosity of Bi (bit) is 53.6% and the porosity of V12 is 69.8%. The improvement of porosity is conducive to the enrichment and transmission of CO2 molecules in the catalytic process.
[0064] The catalyst of the present invention was tested, and the test results are as follows Figure 6 Based on the above structural characteristics, Bi-BTD can achieve a Faraday efficiency of more than 90% for the conversion of CO2 to formic acid in a wide potential range of -1.1 V to -1.6 V using Hg / HgO electrodes under the reaction conditions of a liquid flow cell and 1M KCl (potassium chloride) electrolyte. In particular, the Faraday efficiency of formic acid can reach 99.3% at -1.1 V, and the current density of formic acid can reach 160 mA cm at -1.6 V. -2 According to the comparison, the catalytic performance of the present invention is better than most of the Bi-MOF catalysts reported so far.
[0065] It should be noted that the terms used in the present invention are only for describing specific embodiments, rather than limiting the scope of the present application. As shown in the present specification, unless the context clearly indicates an exception, the words "one", "a", "a kind of" and / or "the" do not specifically refer to the singular, but may also include the plural. The terms "include", "comprise" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method or device. In the absence of more restrictions, the elements defined by the sentence "include one..." do not exclude the presence of other identical elements in the process, method or device including the elements.
[0066] It should also be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. Unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", etc. should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the technical solutions of the embodiments of the present invention.
Claims
1. A bismuth MOFs catalytic material, characterized in that: The catalytic material is formed by double interlacing of a three-dimensional framework structure, and the catalytic material structure is formed by sequentially connecting a number of minimum asymmetric repeating structural units; the minimum asymmetric repeating unit uses trivalent bismuth in a spatial coordination configuration of a seven-coordinated capped triangular pyramid as a metal node, and connects three N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligands and one water molecule ligand around the metal node; the Bi atom of the current minimum asymmetric repeating structural unit forms a Bi-O bond with the O atom of the N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide ligand in the adjacent repeating structural unit to achieve three-dimensional connection to form a three-dimensional framework structure; The unit cell parameters of the catalytic material are a =47.3857Å, b =17.3285Å, c =49.1655Å, α=β=90°, γ=118.178°, unit cell volume is 35586.37Å 3 .
2. The bismuth-containing MOFs catalytic material according to claim 1, characterized in that: The porosity of the catalytic material is 70%-76%.
3. The bismuth-containing MOFs catalytic material according to claim 1, characterized in that: The XRD of the catalytic material has characteristic diffraction peaks at 6.2°, 7.4°, 7.6°, 8.2°, 8.5°, 10.9° and 12.8° in an X-ray powder diffraction pattern represented by a diffraction angle 2θ.
4. The method for preparing the bismuth MOFs catalytic material according to any one of claims 1 to 3, characterized in that: The preparation method comprises: Bismuth nitrate, N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide, formic acid, and N,N'-dimethylformamide are uniformly mixed and reacted to obtain an intermediate product, and the intermediate product is washed and dried with N,N'-dimethylformamide to obtain a bismuth MOFs catalytic material; The molar concentration of the bismuth nitrate is 0.003 mol / L-0.013 mol / L; The molar ratio of the bismuth nitrate to N,N'-bis(terphenyl-4,4''-dicarboxylic acid)naphthalenediimide is 0.01-0.04:0.005-0.02; The volume ratio of formic acid to N,N'-dimethylformamide is 0.01-0.1:3; The specific steps of the reaction are: heating to 60°C-120°C at a heating rate of 5°C / h-10°C / h, conducting a constant temperature reaction for 70h-80h, and then cooling to 25°C-35°C at a cooling rate of 25°C / 36h-95°C / 36h.
5. Use of the bismuth-containing MOFs catalytic material according to any one of claims 1 to 3 in the catalytic reduction of CO2 to formic acid.
Citation Information
Patent Citations
Bismuth-based metal organic framework and preparation method and application thereof
CN115028848A
Bismuth metal organic framework single crystal material and preparation method thereof
CN117069952A
Copper-based metal-organic framework and preparation method thereof