A modified lithium iron phosphate positive electrode material and preparation method thereof and battery

By combining manganese and nitrogen doping technology with carbon nanotube-modified titanium dioxide powder, the problem of poor rate performance of lithium iron phosphate cathode materials at high rates has been solved, achieving improvements in high rate performance and high energy density, and significantly improving The electrochemical performance of lithium-ion batteries.

CN118598109BActive Publication Date: 2024-10-22SICHUAN UNIVERSITY OF SCIENCE AND ENGINEERING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411082492.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-22
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Existing lithium iron phosphate cathode materials exhibit low electronic conductivity and limited ion transmission channels at high rates, resulting in poor rate performance in power battery applications, and nanotechnology will reduce the compaction density and energy density of the material. .

Method used

Using a combination of manganese and nitrogen doping technology, LiFe1-xMnxPO4/C composite materials were prepared through ball milling and multiple sintering processes, and carbon nanotube-modified titanium dioxide powder was introduced to improve the electronic conductivity and ion mobility of the material to form Lithium iron phosphate cathode material with high rate performance.

Benefits of technology

It significantly improves the electrochemical performance of lithium iron phosphate cathode materials at high rates, increases the lithium ion diffusion rate and discharge specific capacity, maintains high compaction density, and exhibits excellent rate performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118598109B_ABST
    Figure CN118598109B_ABST
Patent Text Reader

Abstract

The invention discloses a modified lithium iron phosphate positive electrode material and a preparation method thereof and a battery, which relates to the technical field of lithium batteries, comprising: putting a lithium source, anhydrous iron phosphate, a carbon source, titanium dioxide powder, phosphoric acid, and manganese carbonate into a nylon ball mill, adding anhydrous ethanol and zirconium oxide grinding balls for ball milling to obtain a mixed slurry; putting the mixed slurry into a vacuum drying oven for drying, calcining after drying, cooling and grinding to obtain LiFe 1‑x Mn x PO 4 / C composite material, where 0<x≤3%; to LiFe 1‑x Mn x PO 4 A nitrogen source is added to the / C composite material, ground, and calcined twice to obtain a modified lithium iron phosphate positive electrode material. The present invention prepares a nitrogen-manganese co-doped lithium iron phosphate electrode material with high compaction density and high rate performance. After introducing carbon nanotube-modified titanium dioxide, the discharge specific capacity of the modified lithium iron phosphate positive electrode material is significantly improved. The maximum discharge specific capacity at 5C can reach 140.94mAh / g, further improving the rate performance of the lithium iron phosphate positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and more specifically, the present invention relates to a modified lithium iron phosphate positive electrode material and a preparation method thereof and a battery. Background Art

[0002] The development of existing lithium-ion batteries began with lithium cobalt oxide batteries, and then developed into ternary nickel cobalt manganese, lithium iron phosphate, etc. As one of the important components of lithium-ion batteries, the positive electrode material initially used lithium salt oxides, such as lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium iron phosphate, etc.; the negative electrode usually uses some carbon materials, such as graphite, graphene, etc. Lithium-ion batteries are mainly composed of positive and negative electrode materials, electrolytes that can transfer lithium ions, diaphragms, and shells. Among them, the electrolyte is lithium salt dissolved in a specific organic solvent, which can provide a path for the transfer of lithium ions. The diaphragm is an ion conductor that can prevent the transfer of electrons and also prevent short circuits caused by direct contact between the positive and negative electrodes. The essence of the lithium battery during operation is the process of lithium ions transporting between the positive and negative electrodes. During the charging process, lithium ions are released from the positive electrode material, transferred to the negative electrode material through the electrolyte and embedded, thereby storing energy. At the same time, electrons diffuse from the positive electrode to the negative electrode of the battery. The discharge process is the opposite process and releases energy.

[0003] At present, lithium iron phosphate cathode materials still face the disadvantage of poor rate performance during use. The reason is the intrinsic low electronic conductivity and limited ion transmission channels of lithium iron phosphate materials. Under the existing mature technical conditions, it is usually improved by carbon coating, and the ion conductivity and ion mobility of the material are improved by doping or nano-technology. However, there is currently a lack of effective methods to improve the rate and ion mobility of ultra-high rate lithium iron phosphate cathode materials used in power batteries. If existing lithium iron phosphate wants to obtain excellent performance at high rates, it is usually nano-sized, but this usually reduces the compaction density of the material, resulting in low energy density. Summary of the invention

[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0005] In order to achieve these purposes and advantages according to the present invention, a method for preparing a modified lithium iron phosphate positive electrode material is provided, comprising the following steps:

[0006] Step 1: Put lithium source, anhydrous iron phosphate, carbon source, titanium dioxide powder, phosphoric acid and manganese carbonate into a nylon ball mill, add anhydrous ethanol and zirconium oxide grinding balls for ball milling to obtain a mixed slurry;

[0007] Step 2: Place the mixed slurry in a vacuum drying oven for drying, calcine after drying, and grind to obtain LiFe 1-x Mn x PO 4 / C composite material, where 0<x≤3%;

[0008] Step 3: LiFe 1-x Mn x PO 4 A nitrogen source is added to the MgO / C composite material, which is ground and then calcined twice to obtain a modified lithium iron phosphate positive electrode material.

[0009] Preferably, in step 1, the lithium source is lithium hydroxide or anhydrous lithium carbonate, and the mixing ratio of anhydrous iron phosphate, lithium source and manganese carbonate is: mixing according to the molar ratio of the total molar amount of iron and manganese to lithium of 1:1.05.

[0010] Preferably, in step 1, the carbon source is glucose, and the amount of glucose used is 15% to 25% of the mass of anhydrous ferric phosphate.

[0011] Preferably, in the step 1, the amount of titanium dioxide powder used is 0.1% to 0.5% of the mass of anhydrous iron phosphate; and the amount of phosphoric acid used is 0.05 to 0.1 ml.

[0012] Preferably, in the step 1, the mass of anhydrous ethanol is the same as the total mass of the lithium source, anhydrous ferric phosphate, carbon source, titanium dioxide powder, phosphoric acid and manganese carbonate, the ratio of the mass of zirconium oxide grinding balls to the mass of the lithium source, anhydrous ferric phosphate, carbon source, titanium dioxide powder, phosphoric acid and manganese carbonate is 3-6:1; the ball milling time is 4-12 hours, and the ball milling speed is 300-2000 rpm.

[0013] Preferably, in the step 2, the drying temperature is 50-80°C and the drying time is 6-18h; the calcination conditions are: after nitrogen is introduced at room temperature for 20-60min, the temperature is increased to 330-400°C at a heating rate of 2-8°C / min, and kept warm for 1-4h, and then the temperature is increased to 600-800°C at the same heating rate, and kept warm for 8-18h.

[0014] Preferably, in step 2, the nitrogen source is one of polydopamine, melamine, gelatin, and polybenzoxazine; the mass of the nitrogen source is LiFe 1-x Mn x PO 4 / C composite material mass 10%~15%; the secondary calcination conditions are: after nitrogen is introduced at room temperature for 20~60min, the temperature is increased to 330~400℃ at a heating rate of 2~8℃ / min, and kept warm for 1~4h, and then the temperature is increased to 600~800℃ at the same heating rate and kept warm for 2~6h.

[0015] Preferably, in the step 1, titanium dioxide powder modified with carbon nanotubes is used to replace titanium dioxide powder, wherein the preparation method of titanium dioxide powder modified with carbon nanotubes comprises:

[0016] S11, dissolving tetrabutyl titanate in anhydrous ethanol to obtain a tetrabutyl titanate solution, adding the carbon nanotube dispersion to the tetrabutyl titanate solution, and uniformly dispersing by ultrasonication, wherein the ultrasonic frequency is 80-150 kHz, and the ultrasonic time is 20-40 min; the mass ratio of tetrabutyl titanate to carbon nanotubes is 10-15:1, the concentration of the tetrabutyl titanate solution is 20-30 wt %, and the mass volume ratio of carbon nanotubes to anhydrous ethanol in the carbon nanotube dispersion is 1-15 g:200-1000 mL;

[0017] S12, mixing the tetrabutyl titanate solution with the carbon nanotube dispersion, and then adding a 1 mol / L cerium nitrate solution, wherein the amount of cerium nitrate is 5% to 15% of the mass of the tetrabutyl titanate; after stirring evenly, adding 0.5 to 1.5 mol / L nitric acid, polyethylene glycol-400, and sodium dodecyl sulfate in an amount equal to the volume of the cerium nitrate solution in sequence, stirring magnetically at a speed of 2000 to 4400 rpm for 1 to 5 hours, and aging statically for 24 to 72 hours to obtain a gel; wherein the mass ratio of polyethylene glycol-400 and sodium dodecyl sulfate to tetrabutyl titanate is 0.4 to 0.9:0.01 to 0.1:1;

[0018] S13. In an argon atmosphere, the gel is calcined at a temperature of 500-900° C. for 2-5 hours. After cooling to room temperature, the calcined solid is ground to obtain carbon nanotube-modified titanium dioxide powder.

[0019] A modified lithium iron phosphate positive electrode material is prepared by a method for preparing a modified lithium iron phosphate positive electrode material.

[0020] A lithium-ion battery comprises a battery cell prepared from a modified lithium iron phosphate positive electrode material.

[0021] The present invention has at least the following beneficial effects:

[0022] The present invention uses lithium hydroxide or anhydrous lithium carbonate as a lithium source, first performs manganese doping to broaden the lithium ion diffusion channel and increase the ion diffusion rate, and then performs nitrogen doping to increase the lithium ion diffusion rate while increasing the electronic conductivity of the lithium iron phosphate positive electrode material, thereby improving its electrochemical performance at high rates. Through one or two sinterings, a nitrogen-manganese co-doped lithium iron phosphate electrode material with a large compaction density and high rate performance is obtained. 1-x Mn x PO 4 The / C composite material was mixed with melamine and then calcined to introduce nitrogen. The electrochemical properties of the two samples were compared by cyclic voltammetry, AC impedance test and constant current charge and discharge test. The experimental results showed that the nitrogen-manganese co-doped lithium iron phosphate positive electrode material showed the best rate performance, with the lowest charge and discharge platform voltage difference of 157mV at 1C and the highest lithium ion diffusion rate of 2.14×10 -12 cm 2 ·s -1 , and the best high rate performance, among which the highest discharge capacity at 5C is 73.77mAh / g, which is 55.3% of the discharge capacity at 1C. The best performance of LFP1% / N may be attributed to the fact that manganese doping broadens the lithium ion diffusion channel and increases the lithium ion diffusion rate, while nitrogen doping forms an electron-rich conductive layer on the surface to improve the performance of lithium iron phosphate positive electrode materials. The present invention provides a reference idea for manganese and nitrogen doping of lithium iron phosphate.

[0023] The present invention not only prepares manganese-nitrogen co-doped lithium iron phosphate positive electrode materials, but also introduces carbon nanotube-modified titanium dioxide into the lithium iron phosphate materials, thereby significantly improving the discharge specific capacity of the modified lithium iron phosphate positive electrode materials. The highest discharge specific capacity at 5C can reach 142.94 mAh / g, which is 86.03% of the discharge specific capacity at 1C, thereby further improving the rate performance of the lithium iron phosphate positive electrode materials.

[0024] The advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the SEM image of LFP-0% prepared in Comparative Example 5;

[0026] Figure 2 This is the SEM image of LFP-1% prepared in Comparative Example 2;

[0027] Figure 3 XRD diagrams of comparative examples 2, 4 and 5 doped with different manganese contents;

[0028] Figure 4 This is the SEM image of LFP1% / N prepared in Example 1;

[0029] Figure 5 XRD diagrams of LFP 1% / N prepared in Example 1 and LFP 0% / N prepared in Comparative Example 1. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0031] It should be understood that terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more elements or combinations thereof.

[0032] Example 1

[0033] This embodiment provides a method for preparing a modified lithium iron phosphate positive electrode material, comprising the following steps:

[0034] Step 1: put 775.85g lithium carbonate, 1493.08g anhydrous iron phosphate, 298.62g glucose, 2.99g titanium dioxide powder, 0.1ml phosphoric acid, and 11.50g manganese carbonate into a nylon ball mill, add 2582.23g anhydrous ethanol and 10328.91g zirconium oxide grinding balls for ball milling to obtain a mixed slurry;

[0035] Step 2: Place the mixed slurry in a vacuum drying oven and dry it at 60°C for 12 hours. After drying, calcine it in a nitrogen atmosphere. After nitrogen is introduced into the room temperature for 30 minutes, heat it to 350°C at a rate of 3°C / min and keep it for 2 hours. Then heat it to 700°C at the same rate and keep it for 10 hours. After cooling, grind it with agate to obtain LiFe 1-x Mn x PO 4 / C composite material, where x = 1%;

[0036] Step 3: LiFe 1-x Mn x PO 4 The / C composite material was doped with 15% melamine by weight, ground with agate for 30 minutes, and then calcined twice. After nitrogen was introduced into the room temperature for 30 minutes, the temperature was raised to 350°C at a rate of 3°C / min and kept for 2 hours, and then the temperature was raised to 700°C at the same rate and kept for 4 hours. After cooling, the modified lithium iron phosphate positive electrode material was ground with agate again to obtain the modified lithium iron phosphate positive electrode material. The modified lithium iron phosphate positive electrode material prepared in this embodiment is recorded as LFP1% / N.

[0037] Example 2

[0038] This embodiment provides a method for preparing a modified lithium iron phosphate positive electrode material, comprising the following steps:

[0039] Step 1: put 775.85g lithium carbonate, 1478.04g anhydrous iron phosphate, 295.66g glucose, 2.96g titanium dioxide powder, 0.1ml phosphoric acid, and 22.99g manganese carbonate into a nylon ball mill, add 2575.69g anhydrous ethanol and 10302.75g zirconium oxide grinding balls for ball milling to obtain a mixed slurry;

[0040] Step 2: Place the mixed slurry in a vacuum drying oven and dry it at 60°C for 12 hours. After drying, calcine it in a nitrogen atmosphere. After nitrogen is introduced into the room temperature for 30 minutes, heat it to 350°C at a rate of 3°C / min and keep it for 2 hours. Then heat it to 700°C at the same rate and keep it for 10 hours. After cooling, grind it with agate to obtain LiFe 1-x Mn x PO 4 / C composite material, where x=2%;

[0041] Step 3: LiFe 1-x Mn x PO 4 The / C composite material was doped with 15% melamine by weight, ground with agate for 30 minutes, and then calcined twice. After nitrogen was introduced at room temperature for 30 minutes, the temperature was raised to 350°C at a rate of 3°C / min and kept for 2 hours, and then the temperature was raised to 700°C at the same rate and kept for 4 hours. After cooling, the modified lithium iron phosphate positive electrode material was ground with agate again to obtain the modified lithium iron phosphate positive electrode material. The modified lithium iron phosphate positive electrode material prepared in this embodiment is recorded as LFP2% / N.

[0042] Example 3

[0043] This embodiment provides a method for preparing a modified lithium iron phosphate positive electrode material, comprising the following steps:

[0044] Step 1: put 775.85g lithium carbonate, 1462.95g anhydrous iron phosphate, 292.59g glucose, 2.93g titanium dioxide powder, 0.1ml phosphoric acid, and 34.49g manganese carbonate into a nylon ball mill, add 2569.00g anhydrous ethanol and 10276.00g zirconium oxide grinding balls for ball milling to obtain a mixed slurry;

[0045] Step 2: Place the mixed slurry in a vacuum drying oven and dry it at 60°C for 12 hours. After drying, calcine it in a nitrogen atmosphere. After nitrogen is introduced into the room temperature for 30 minutes, heat it to 350°C at a rate of 3°C / min and keep it for 2 hours. Then heat it to 700°C at the same rate and keep it for 10 hours. After cooling, grind it with agate to obtain LiFe 1-xMn x PO 4 / C composite material, where x=3%;

[0046] Step 3: LiFe 1-x Mn x PO 4 The / C composite material was doped with 15% melamine by weight, ground with agate for 30 minutes, and then calcined twice. After nitrogen was introduced into the room temperature for 30 minutes, the temperature was raised to 350°C at a rate of 3°C / min and kept for 2 hours, and then the temperature was raised to 700°C at the same rate and kept for 4 hours. After cooling, the modified lithium iron phosphate positive electrode material was ground with agate again to obtain the modified lithium iron phosphate positive electrode material. The modified lithium iron phosphate positive electrode material prepared in this embodiment is recorded as LFP3% / N.

[0047] Example 4

[0048] This embodiment provides a method for preparing a modified lithium iron phosphate positive electrode material. Compared with Example 1, titanium dioxide powder modified with carbon nanotubes is used to replace titanium dioxide powder, and the remaining process parameters are the same as those of Example 1; wherein the method for preparing titanium dioxide powder modified with carbon nanotubes includes:

[0049] S11, dissolving 20 g of tetrabutyl titanate in 80 g of anhydrous ethanol to obtain a tetrabutyl titanate solution, adding 200 ml of a dispersion containing 2 g of carbon nanotubes to the tetrabutyl titanate solution, and uniformly dispersing by ultrasonication at an ultrasonic frequency of 80 kHz and an ultrasonic time of 40 min;

[0050] S12, the tetrabutyl titanate solution and the carbon nanotube dispersion were mixed, and then 10 ml of a 1 mol / L cerium nitrate solution was added; after stirring evenly, 10 ml of 1 mol / L nitric acid, 10 g of polyethylene glycol-400, and 1 g of sodium dodecyl sulfate were added in sequence, and magnetic stirring was performed at 2000 rpm for 2 h, and the mixture was aged for 24 h to obtain a gel;

[0051] S13. The gel was calcined under an argon atmosphere at a temperature of 600° C. for 5 h. After cooling to room temperature, the calcined solid was ground to obtain carbon nanotube-modified titanium dioxide powder.

[0052] Example 5

[0053] This embodiment provides a method for preparing a modified lithium iron phosphate positive electrode material. Compared with Example 1, titanium dioxide powder modified with carbon nanotubes is used to replace titanium dioxide powder, and the remaining process parameters are the same as those of Example 1; wherein the method for preparing titanium dioxide powder modified with carbon nanotubes includes:

[0054] S11, dissolving 30 g of tetrabutyl titanate in 70 g of anhydrous ethanol to obtain a tetrabutyl titanate solution, adding 200 ml of a carbon nanotube dispersion containing 2 g of carbon nanotubes to the tetrabutyl titanate solution, and uniformly dispersing by ultrasonication at an ultrasonic frequency of 100 kHz and an ultrasonic time of 20 min;

[0055] S12, the tetrabutyl titanate solution and the carbon nanotube dispersion were mixed, and then 10 ml of 1 mol / L cerium nitrate solution was added; after stirring evenly, 10 ml of 1.5 mol / L nitric acid, 27 g of polyethylene glycol-400, and 3 g of sodium dodecyl sulfate were added in sequence, and magnetic stirring was performed at 4400 rpm for 5 h, and the gel was obtained after static aging for 36 h;

[0056] S13. The gel was calcined under an argon atmosphere at a temperature of 900° C. for 2 h. After cooling to room temperature, the calcined solid was ground to obtain carbon nanotube-modified titanium dioxide powder.

[0057] Comparative Example 1

[0058] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material, which is not doped with manganese compared to Example 1, and the remaining process methods are the same as Example 1. The lithium iron phosphate positive electrode material prepared in this example is LFP0% / N.

[0059] Comparative Example 2

[0060] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material. Compared with Example 1, nitrogen doping and secondary calcination in step three are not performed, and the remaining process methods are the same as those in Example 1. The lithium iron phosphate positive electrode material prepared in this comparative example is LFP-1%.

[0061] Comparative Example 3

[0062] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material. Compared with Example 2, nitrogen doping and secondary calcination in step three are not performed, and the remaining process methods are the same as Example 2. The lithium iron phosphate positive electrode material prepared in this comparative example is LFP-2%.

[0063] Comparative Example 4

[0064] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material. Compared with Example 3, nitrogen doping and secondary calcination in step three are not performed, and the remaining process methods are the same as Example 3. The lithium iron phosphate positive electrode material prepared in this comparative example is LFP-3%.

[0065] Comparative Example 5

[0066] This comparative example provides a method for preparing a lithium iron phosphate positive electrode material. Compared with Example 1, manganese doping, nitrogen doping and secondary calcination in step 3 are not performed, and the remaining process methods are the same as those in Example 1. The lithium iron phosphate positive electrode material prepared in this comparative example is LFP-0%

[0067] The modified lithium iron phosphate positive electrode materials prepared in Examples 1 to 5 and the lithium iron phosphate positive electrode materials prepared in Comparative Examples 1 to 5 were respectively prepared into lithium iron phosphate positive electrode sheets, and the preparation method thereof was as follows:

[0068] First, take 1g of polyvinylidene fluoride (PVDF) and 18.5ml of NMP (N-methylpyrrolidone) and stir them under a magnetic stirrer for 12h to obtain a glue solution. Then, the ground modified lithium iron phosphate positive electrode material is sieved through a 400-mesh sieve, and then mixed according to the mass ratio of each substance such as modified lithium iron phosphate positive electrode material: acetylene black: PVDF of 8:1:1, and appropriately add NMP to stir it under a magnetic stirrer for 12h to obtain a slurry. Then, use a 20um scraper to evenly coat it on aluminum foil, dry it in a vacuum drying oven for 6h, and then roll it under a roller press, and then cut it into 14mm thin slices to obtain lithium iron phosphate positive electrode sheets. Weigh the cut positive electrode, take several slices with similar mass and flat back and store them for later use.

[0069] The sliced ​​lithium iron phosphate positive electrode sheet and the diaphragm are sent to a glove box with a nitrogen atmosphere, and the springs, gaskets, etc. are prepared. During the installation process, it is best to place the materials in the center, press the seal, and then move to the hydraulic press to press and compact to obtain a button battery. The battery shell model is CR2032.

[0070] The crystal size and morphology of the material can directly affect the electrochemical performance of the material. Therefore, the LFP-0% prepared in Comparative Example 5 and the LFP-1% prepared in Comparative Example 2 were subjected to scanning electron microscopy (SEM) test for physical characterization of the material. Figure 1 and Figure 2 As shown, it can be seen that the particle shape of LPF-0% without manganese doping is uneven, there are large-sized particles, serious agglomeration, and the surface is rough; the particle size of LFP-1% is relatively uniform and the surface is smooth, with a clear particle morphology. This shows that manganese doping can effectively improve the particle size of the material, reduce the agglomeration of the material, and reduce the resistance of ions moving in the material. Figure 1 and Figure 2 The scale bars in the graphs are all 2 μm.

[0071] Figure 3The XRD diagrams of Comparative Examples 2, 4 and 5 with different manganese contents are shown. It can be clearly seen that each material has a significant peak height at the position of the characteristic peak, without other impurity peaks, and shows good purity and a good olivine structure, which all affect the electrochemical properties of the material. For the LFP-1% sample, it has a stronger diffraction peak, and a small amount of doping will not affect the original structure of the material. A small amount of manganese doping can obtain a better and more complete crystal, but the diffraction peak of LFP-3% is weaker than that of LFP-1%, indicating that excessive manganese doping will also affect the formation of material grains.

[0072] The unit cell parameters of the material were calculated by Jade software. The V of the unit cells of LFP-0%, LFP-1%, and LFP-3% are 287.23Å, 292.06Å, and 293.69Å, respectively. It can be seen that with the increase of manganese content, the unit cell volume increases, which inevitably leads to the lengthening of the Li-O bond length in the material, reducing the Li-O bond energy, making it easier for Li to escape from the material, enhancing the diffusion of Li, and further improving the performance of the material. However, the structure size of the crystal will also directly affect the diffusion path of Li in the material. The increase in the unit cell volume will also lengthen the diffusion path of Li, thereby affecting the electrochemical properties of the material. In order to determine the comprehensive influence of this factor on the material.

[0073] For the CV comparison of different manganese doping amounts in Comparative Examples 2, 4 and 5, the oxidation peak potential of LFP-0% is 3.660V, the current is 1.92mA, the reduction peak potential is 3.219V, the current is -1.62mA, and the two peak potential difference is 441mV; the oxidation peak potential of LFP-1% is 3.615V, the peak current is 1.79mA, the reduction peak potential is 3.260V, the peak current is 1.46mA, and the peak potential difference is 355mV; the oxidation peak voltage of LFP-3% is 3.634V, the peak current is 1.60mA, the reduction peak potential is 3.277V, the peak current is 1.24mA, and the peak potential difference is 357mV. The peak potential difference after manganese doping is less than that of LFP-0%. After manganese doping, the reversibility of the positive electrode material is better, the polarization degree is smaller during the electrochemical reaction, and the material is more stable.

[0074] For the first charge and discharge performance of different manganese doping amounts at 1C in Comparative Examples 2, 4 and 5, the charge specific capacity of LFP-0% is 108.94mAh / g, the discharge specific capacity is 82.94mAh / g, the first efficiency is 76.1%, and the charge and discharge platform voltage difference is 253mV; the charge specific capacity of LFP-1% is 104.27mAh / g, the discharge specific capacity is 82.10mAh / g, the first efficiency is 78.7%, and the charge and discharge platform voltage difference is 212 mV; the charge specific capacity of LFP-3% is 103.15mAh / g, the discharge specific capacity is 75.93mAh / g, the first efficiency is 73.6%, and the charge and discharge platform voltage difference is 252mV. It can be clearly seen that although the discharge specific capacity of the positive electrode material doped with manganese is inferior to that of LFP-0%, it has better charge and discharge efficiency and a smaller charge and discharge platform voltage difference, indicating that the battery reaction has a smaller degree of polarization after doping with manganese. At the same time, as the manganese content increases, the polarization degree of the battery increases, and the discharge performance of the battery decreases. This may be because as the manganese content increases, more manganese enters the iron position and destroys the olivine structure of lithium iron phosphate, thereby affecting the performance of the material. At the same time, doping with manganese can significantly increase the voltage platform of the LFP material during discharge, because the LMP material has a higher voltage platform than the LFP.

[0075] The discharge specific capacities of the three materials in Comparative Examples 2, 4 and 5 are compared at 0.1C, 0.2C, 0.5C, 1C, 2C and 5C, and finally return to the discharge performance at 0.1C, as shown in Table 1:

[0076] Table 1 Discharge capacity of LFP-0%, LFP-1%, and LFP3% at various rates (mAh / g)

[0077]

[0078] It can be seen from the above table that the discharge specific capacity of manganese-doped materials at different rates is lower than LFP-0%. This may be because after manganese is doped into the iron position, it tends to transform into a layered structure, affecting the crystal structure of the material and thus affecting the battery performance. At the same time, excessive manganese doping will aggravate the performance of the material.

[0079] Example 1: SEM of LFP1% / N obtained by nitrogen doping Figure 4 As shown in the figure, LFP-1% has a more uniform particle size after being doped with nitrogen, especially at 10kx, LFP1% / N has a significantly more uniform particle size, showing good dispersion and spherical morphology. The obvious changes before and after nitrogen doping indicate that nitrogen is effectively doped into the material surface, reducing the agglomeration of the material and significantly improving the morphology and particle size of the material.

[0080] Figure 5From the XRD diagrams of LFP1% / N prepared in Example 1 and LFP0% / N prepared in Comparative Example 1, it can be clearly seen that the di-calcination after nitrogen doping has no effect on the crystal structure of the product, and there is no obvious impurity peak in the spectrum, indicating that nitrogen doping does not introduce other impurities and has no obvious effect on the crystal structure of the material, and it still exhibits a good olivine structure.

[0081] The CV of LFP0% / N prepared in Comparative Example 1 and LFP1% / N prepared in Example 1 are compared, wherein the oxidation peak potential of LFP0% / N is at 3.65V, the peak current is 1.62mA, the reduction peak potential is at 3.275V, the peak current is 1.33mA, the peak voltage difference of the sample is 375mV, and the value of the reduction peak to the oxidation peak is 82.1%; for LFP-1% / N, the oxidation peak potential is at 3.685V, the peak current is 1.96mA, the reduction peak potential is at 3.257V, the peak current is 1.39mA, the peak potential difference of the sample is 428mV, and the peak current ratio is 70.9%. The above data show that LFP0% / N has a smaller degree of polarization and better reversibility, but the peak current is less than LFP1% / N, and the capacity in electrochemical performance is smaller, especially the capacity decay is serious at high rates, and both materials have their own advantages.

[0082] The first charge and discharge comparison of LFP0% / N, LFP1% / N, LFP-0% and LFP-1% was carried out. Among them, LFP1% / N has the longest charge and discharge platform and the smallest platform voltage difference of 157mV, with excellent battery specific capacity and minimum polarization degree, showing excellent electrochemical performance. Compared with the discharge specific capacity before nitrogen doping, it increased by 19.7%, and its charge specific capacity was 134.67mAh / g, discharge specific capacity was 98.74mAh / g, and charge and discharge efficiency was 73.3%; compared with LFP-0%, nitrogen doping has little effect on the platform voltage difference, and nitrogen doping has further improved the specific capacity by about 2.4%, and its discharge specific capacity is 124.09mAh / g, discharge specific capacity is 84.96mAh / g, and charge and discharge efficiency is 68.5%. It can be seen that nitrogen doping has further improved the material performance, and the improvement effect is the best for LFP-1%, and it shows the best electrochemical performance and charge and discharge efficiency.

[0083] The discharge capacity of LFP0% / N and LFP1% / N at different rates were compared. The discharge capacity of LFP0% / N at 0.1C, 0.2C, 0.5C, 1C, 2C, and 5C was 136.83, 134.63, 112.93, 98.42, 84.89, and 65.00 mAh / g, respectively, and 144.54 mAh / g when it returned to 0.1C; the discharge capacity of LFP1% / N at different rates was 133.47, 132.71, 119.14, 108.95, 99.69, and 73.77 mAh / g, and 137.34 mAh / g when it returned to 0.1C. The above data compare the discharge performance of the two samples at various rates before nitrogen doping modification, and the discharge capacity of the two samples at various rates has been significantly improved.

[0084] It can be seen that LFP0% / N has a slightly higher discharge capacity at low rates, 2.5% and 1.5% higher than LFP1% / N at 0.1C and 0.2C, respectively. However, LFP1% / N has a better discharge capacity at high rates such as 0.5C, 1C, 2C and 5C, especially at 2C, where the discharge capacity is about 17.4% higher than LFP0% / N. The above data show that LFP1% / N has better stability and rate performance at high rates.

[0085] The discharge specific capacities of LFP1% / N and LFP0% / N after 100 cycles at 1C were compared. LFP1% / N showed a higher discharge specific capacity during the cycle, but the two were almost the same under stable cycle conditions. The capacity retention rate of LFP0% / N after 100 cycles was 95.2%, while the specific capacity of LFP1% / N increased by 20.7% after 100 cycles. This may be because as the charge and discharge test proceeds, the active material is more fully activated and the reaction is more complete, so it can show a higher discharge specific capacity in subsequent cycles than in the first charge and discharge.

[0086] The discharge specific capacities of the modified lithium iron phosphate positive electrode materials prepared in Example 1, Example 4 and Example 5 at various rates are compared to obtain Table 2:

[0087] Table 2 Comparison of the discharge specific capacities of the modified lithium iron phosphate positive electrode materials prepared in Example 1, Example 4 and Example 5

[0088]

[0089] It can be seen from the above table that compared with Example 1 and Comparative Example 1, the modified lithium iron phosphate positive electrode materials in Examples 4 and 5 are doped with carbon nanotube-modified silicon dioxide, and have a larger discharge specific capacity. Therefore, the modified lithium iron phosphate positive electrode materials prepared in Examples 4 and 5 have better rate performance.

[0090] The compaction densities of the modified lithium iron phosphate positive electrode materials prepared in Examples 1 to 5 and the lithium iron phosphate positive electrode materials prepared in Comparative Examples 1 to 5 were measured respectively, and the results are shown in Table 3:

[0091] Table 3 Compacted density of various lithium iron phosphate cathode materials

[0092]

[0093] It can be seen from the above table that the compaction density of the modified lithium iron phosphate positive electrode materials prepared in Examples 1 to 5 is significantly greater than that in Comparative Examples 1 to 5, while the compaction density of the modified lithium iron phosphate positive electrode materials prepared in Examples 4 and 5 is significantly better than that in Examples 1 to 3.

[0094] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.

[0095] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing a modified lithium iron phosphate positive electrode material, It is characterized in that The following steps are involved: Step 1: Put lithium source, anhydrous iron phosphate, carbon source, titanium dioxide powder, phosphoric acid and manganese carbonate into a nylon ball mill, add anhydrous ethanol and zirconium oxide grinding balls for ball milling to obtain a mixed slurry; Step 2: Place the mixed slurry in a vacuum drying oven for drying, calcine after drying, and grind to obtain LiFe 1-x Mn x PO 4 / C composite material, where 0<x≤3%; Step 3: LiFe 1-x Mn x PO 4 A nitrogen source is added to the / C composite material, and the mixture is ground and then calcined twice to obtain a modified lithium iron phosphate positive electrode material; In the step 1, the amount of titanium dioxide powder used is 0.1% to 0.5% of the mass of anhydrous iron phosphate; the amount of phosphoric acid used is 0.05 to 0.1 ml; In the step 1, titanium dioxide powder modified with carbon nanotubes is used to replace titanium dioxide powder, wherein the preparation method of titanium dioxide powder modified with carbon nanotubes comprises: S11, dissolving tetrabutyl titanate in anhydrous ethanol to obtain a tetrabutyl titanate solution, adding the carbon nanotube dispersion to the tetrabutyl titanate solution, and uniformly dispersing by ultrasonication, wherein the ultrasonic frequency is 80-150 kHz, and the ultrasonic time is 20-40 min; the mass ratio of tetrabutyl titanate to carbon nanotubes is 10-15:1, the concentration of the tetrabutyl titanate solution is 20-30 wt%, and the mass volume ratio of carbon nanotubes to anhydrous ethanol in the carbon nanotube dispersion is 1-15 g:200-1000 mL; S12, mixing the tetrabutyl titanate solution with the carbon nanotube dispersion, and then adding a 1 mol / L cerium nitrate solution, wherein the amount of cerium nitrate is 5% to 15% of the mass of the tetrabutyl titanate; after stirring evenly, adding 0.5 to 1.5 mol / L nitric acid, polyethylene glycol-400, and sodium dodecyl sulfate in an amount equal to the volume of the cerium nitrate solution in sequence, stirring magnetically at a speed of 2000 to 4400 rpm for 1 to 5 hours, and aging statically for 24 to 72 hours to obtain a gel; wherein the mass ratio of polyethylene glycol-400 and sodium dodecyl sulfate to tetrabutyl titanate is 0.4 to 0.9:0.01 to 0.1:1; S13. In an argon atmosphere, the gel is calcined at a temperature of 500-900° C. for 2-5 hours. After cooling to room temperature, the calcined solid is ground to obtain carbon nanotube-modified titanium dioxide powder.

2. The method for preparing the modified lithium iron phosphate positive electrode material according to claim 1, It is characterized in that In the step 1, the lithium source is lithium hydroxide or anhydrous lithium carbonate, and the mixing ratio of anhydrous iron phosphate, lithium source and manganese carbonate is: mixing according to the molar ratio of the total molar amount of iron and manganese to lithium of 1:1.

05.

3. The method for preparing the modified lithium iron phosphate positive electrode material according to claim 1, It is characterized in that In the step 1, the carbon source is glucose, and the amount of glucose used is 15% to 25% of the mass of anhydrous ferric phosphate.

4. The method for preparing the modified lithium iron phosphate positive electrode material according to claim 1, It is characterized in that In the step 1, the mass of anhydrous ethanol is the same as the total mass of the lithium source, anhydrous ferric phosphate, carbon source, titanium dioxide powder, phosphoric acid, and manganese carbonate; the ratio of the mass of zirconium oxide grinding balls to the total mass of the lithium source, anhydrous ferric phosphate, carbon source, titanium dioxide powder, phosphoric acid, and manganese carbonate is 3-6:1; the ball milling time is 4-12 hours, and the ball milling speed is 300-2000 rpm.

5. The method for preparing the modified lithium iron phosphate positive electrode material according to claim 1, It is characterized in that In the step 2, the drying temperature is 50-80°C, and the drying time is 6-18h; the calcination conditions are: after nitrogen is introduced at room temperature for 20-60min, the temperature is increased to 330-400°C at a heating rate of 2-8°C / min, and kept warm for 1-4h, and then the temperature is increased to 600-800°C at the same heating rate, and kept warm for 8-18h.

6. The method for preparing the modified lithium iron phosphate positive electrode material according to claim 1, It is characterized in that In the step 2, the nitrogen source is one of polydopamine, melamine, gelatin, and polybenzoxazine; the mass of the nitrogen source is LiFe 1- x Mn x PO 4 / C composite material mass 10%~15%; the secondary calcination conditions are: after nitrogen is introduced at room temperature for 20~60min, the temperature is increased to 330~400℃ at a heating rate of 2~8℃ / min, and kept warm for 1~4h, and then the temperature is increased to 600~800℃ at the same heating rate and kept warm for 2~6h.

7. A modified lithium iron phosphate positive electrode material, It is characterized in that The modified lithium iron phosphate positive electrode material is prepared by the method for preparing the modified lithium iron phosphate positive electrode material according to any one of claims 1 to 6.

8. A lithium ion battery, It is characterized in that It comprises a battery cell prepared from the modified lithium iron phosphate positive electrode material as claimed in claim 7.