Preparation method and application of flexible carbon fiber membrane-based silicon-carbon negative electrode material

Preparing flexible carbon fiber membranes through electrospinning and performing vapor deposition and carbon coating solves the problem of insufficient flexibility of porous carbon fiber membranes, improves the cycle stability and electrochemical performance of lithium-ion batteries, and achieves high-capacity and long-life negative electrodes Material.

CN118600729BActive Publication Date: 2024-10-25BEIJING IAMETAL NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411067171.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-25
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The insufficient flexibility of porous carbon fiber membranes leads to problems with the cycle stability of lithium-ion batteries and easy breakage during battery assembly.

Method used

Polyacrylonitrile is prepared through electrospinning, the sacrificial agent and the phosphazene-based multi-arm boride are dissolved to form a spinning solution, which is pre-oxidized, carbonized and activated to create pores in an inert atmosphere to obtain a flexible carbon fiber membrane, which is then processed through vapor deposition and carbon coating. A flexible carbon fiber membrane-based silicon-carbon negative electrode material was prepared.

Benefits of technology

The flexibility and conductivity of the carbon fiber membrane are improved, forming a stable self-supporting structure, avoiding damage during bending, and enhancing the cycle stability and electrochemical performance of the battery. For the first time, the reversible capacity reaches more than 1800 mAh/g, and the cycle is 100 cycles. The capacity retention rate remains above 91%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118600729B_ABST
    Figure CN118600729B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a flexible carbon fiber membrane-based silicon-carbon negative electrode material, comprising the following steps: (S1) dissolving polyacrylonitrile, a sacrificial agent, and a phosphazene-based multi-arm boride in an organic solvent to form a spinning solution, and electrospinning to obtain a fiber membrane precursor; the phosphazene-based multi-arm boride is prepared by reacting raw materials including hexachlorocyclotriphosphazene and phenylboronic acid compounds, and the molar ratio of hexachlorocyclotriphosphazene to phenylboronic acid compounds is 1: (3.05-3.2); (S2) the fiber membrane precursor is sequentially pre-oxidized, carbonized, and activated to obtain a flexible carbon fiber membrane; (S3) the flexible carbon fiber membrane is subjected to vapor phase silicon deposition and carbon coating to obtain a flexible carbon fiber membrane-based silicon-carbon negative electrode material. The flexible carbon fiber membrane-based negative electrode material prepared by the method of the present invention has good flexibility and a high specific surface area, and the assembled lithium battery has a low capacity loss rate under a pressure of 10t and has excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary battery negative electrode materials, and in particular relates to a preparation method and application of a flexible carbon fiber film-based silicon-carbon negative electrode material. Background Art

[0002] As the next generation of negative electrode materials for lithium-ion batteries, silicon-carbon composites have shown great potential in the field of energy storage after years of research and development. They combine the advantages of silicon and carbon materials: silicon has a theoretical specific capacity of up to 4200 mAh / g, but has the problem of large volume expansion; while carbon materials have good conductivity and structural stability. By embedding silicon particles in a carbon matrix or coating them with a carbon layer, silicon-carbon composites can effectively alleviate the problem of silicon volume change and improve the cycle life and energy density of the battery. In the future, silicon-carbon composites are expected to be widely used in electric vehicles, portable electronic devices and energy storage systems, bringing more efficient and longer-lasting energy solutions.

[0003] At present, silicon-carbon composite materials mostly use granular porous carbon as a carbon substrate to deposit silicon particles, alleviate the volume expansion of silicon, and prevent the pulverization of silicon particles. Compared with granular porous carbon, the porous carbon fiber membrane obtained by electrospinning generally has a self-supporting structure, which can effectively release stress, thereby avoiding breakage during bending. When used as a negative electrode material, it does not require any conductive agent and binder, which simplifies the preparation process of the electrode; at the same time, since no inactive substances (binders, etc.) are used in the electrode material, it is beneficial to enhance the conductivity of the material. When preparing silicon-carbon negative electrode materials based on carbon fiber membranes, in order to alleviate the volume expansion of silicon, it is necessary to make pores in the carbon fiber. Generally, sacrificial agents are added during electrospinning and post-activation pores are made. Song Qi et al. prepared an activated carbon fiber flexible self-supporting electrode by electrospinning and air activation. The three-dimensional multi-porous network structure of the activated carbon fiber is conducive to improving the wettability of the electrode and the electrolyte and promoting the diffusion of potassium ions, but its cycle stability needs to be further improved.

[0004] When making holes in carbon fiber, if the porosity is too low, the deposited silicon content is limited, and the capacitance is low; if the porosity is too high, the carbon fiber membrane will often be damaged and brittle during battery assembly and use, that is, the porous carbon fiber membrane also has the problem of insufficient flexibility. The insufficient flexibility of the porous carbon fiber membrane will affect the cycle stability of the battery. Summary of the invention

[0005] The present invention provides a flexible carbon fiber membrane-based silicon-carbon negative electrode material to solve the problem of insufficient flexibility of the above-mentioned porous carbon fiber membrane.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a flexible carbon fiber film-based silicon-carbon negative electrode material comprises the following steps:

[0008] (S1) dissolving polyacrylonitrile, a sacrificial agent, and a phosphazene-based multi-arm boride in an organic solvent to form a spinning solution, and electrospinning to obtain a fiber membrane precursor; the phosphazene-based multi-arm boride is prepared by reacting raw materials including hexachlorocyclotriphosphazene and phenylboronic acid compounds, and the molar ratio of hexachlorocyclotriphosphazene to phenylboronic acid compounds is 1:(3.05-3.2);

[0009] (S2) The fiber membrane precursor is sequentially pre-oxidized, carbonized under an inert atmosphere, and activated to form pores to obtain a flexible carbon fiber membrane;

[0010] (S3) The flexible carbon fiber membrane is subjected to vapor phase silicon deposition and carbon coating to obtain a flexible carbon fiber membrane-based silicon-carbon negative electrode material.

[0011] The pre-oxidation of the fiber membrane precursor obtained by electrospinning is to convert the precursor fiber into a stable thermosetting fiber through complex physical and chemical reactions (such as dehydrogenation, cyclization and cross-linking, etc.), so that the fiber remains stable and does not melt during the subsequent carbonization process. The nitrile group (-C≡N) in polyacrylonitrile will be converted into a conjugated carbon-nitrogen double bond (-C=N) during the pre-oxidation process, that is, an aromatic heterocyclic structure is formed. The phosphazene group in the phosphazene-based multi-arm boride is a six-membered ring structure with alternating double bonds of P and N, which has good thermal stability and is often used in flame retardants. The inventors have found that the carbon fiber membrane prepared by electrospinning phosphazene-based multi-arm boride and polyacrylonitrile has good flexibility. The possible reason is that the phosphazene group of the phosphazene-based multi-arm boride and the aromatic heterocyclic structure formed by pre-oxidation of polyacrylonitrile during the high-temperature carbonization process form a network cross-linking, thereby constructing the cross-linking of carbon fiber at the microscopic scale. At the same time, the phosphazene-based multi-arm boride contains abundant B, N, and P, and multi-atom co-doping of carbon fiber is achieved at high temperature.

[0012] Furthermore, the phenylboronic acid compound in step (S1) is at least one of 2-formylphenylboronic acid, 4-formylphenylboronic acid, 4-(4-pyridine)phenylboronic acid, 4-nitrilephenylboronic acid, and 5-nitrile-2-fluorophenylboronic acid.

[0013] Furthermore, in step (S1), the mass ratio of the polyacrylonitrile, the sacrificial agent and the phosphazene-based multi-arm boride is 1: (0.1-0.4): (0.2-0.5), preferably 1: (0.2-0.4): (0.3-0.4).

[0014] Furthermore, in step (S1), the weight average molecular weight of the polyacrylonitrile is 50,000-150,000.

[0015] Furthermore, in step (S1), the sacrificial agent is at least one of polymethyl methacrylate and polyvinyl pyrrolidone, and the weight average molecular weight thereof is 5000-15000.

[0016] Furthermore, in step (S1), the organic solvent is at least one of N,N-dimethylacetamide (DMA) and N,N-dimethylformamide (DMF); and the total concentration of polyacrylonitrile, sacrificial agent and phosphazene-based multi-arm boride in the spinning solution is 10wt%~20wt%.

[0017] Furthermore, in step (S1), the conditions for electrospinning are: voltage 10-20 kV, distance between needle and receiving axis 10-20 cm, and propulsion speed of spinning solution 0.5-1.5 mL / h.

[0018] Furthermore, in step (S1), the phosphazene-based multi-arm boride is prepared by a preparation method comprising the following steps:

[0019] (L1) dissolving a phenylboronic acid compound and anhydrous carbonate in a solvent to form a mixed solution A; dissolving hexachlorocyclotriphosphazene in a solvent to form a solution B;

[0020] (L2) adding solution B dropwise to the mixed solution A, stirring and reacting at 50-70°C under inert gas protection for 24-36 hours to obtain a reaction mixture;

[0021] (L3) The reaction mixture is filtered, rotary evaporated, washed, and vacuum dried to obtain a phosphazene multi-arm boride.

[0022] Furthermore, in step (L1), the solvent is tetrahydrofuran (THF), and the anhydrous carbonate is anhydrous K2CO3 or anhydrous Na2CO3.

[0023] Furthermore, in step (L1), the mass ratio of the phenylboric acid compound to the anhydrous carbonate is 1:(1.5~3); the total concentration of the mixed solution A is 20wt%~30wt%; and the concentration of the solution B is 5 wt%~10wt%.

[0024] Furthermore, in step (L2), the inert gas is at least one of nitrogen, argon and helium.

[0025] Furthermore, in step (L3), the vacuum drying is performed at 50-70° C. for 12-24 hours.

[0026] Furthermore, in step (S2), the pre-oxidation temperature is 220°C~270°C, and the time is 1 h~4 h; the carbonization temperature is 700°C~950°C, and the time is 0.5~2 h; and the inert atmosphere is at least one of nitrogen, argon, and helium.

[0027] Furthermore, in step (S2), the activating agent used for the activation pore formation is at least one of water vapor, carbon dioxide and air, and the activation pore formation conditions are: temperature 500°C to 1000°C, time 1h to 4h.

[0028] Furthermore, the fiber diameter of the flexible carbon fiber membrane obtained in step (S2) is 0.1 μm~1.5 μm.

[0029] Furthermore, in step (S3), the vapor-deposited silicon is chemically vapor deposited on the flexible carbon fiber membrane using an organic silicon source gas, so that the nano silicon particles are attached to the fiber pores of the flexible carbon fiber membrane; the organic silicon source gas is selected from at least one of monosilane, disilane, dichlorosilane, trichlorosilane, silicon tetrachloride, silicon tetrafluoride, etc.; the conditions of the chemical vapor deposition are: deposition for 2h to 8h under an inert atmosphere at 500°C to 800°C, and the inert atmosphere is at least one of nitrogen, argon, and helium.

[0030] The carbon coating process in step (S3) is well known to those skilled in the art, such as the carbon source gas is selected from at least one of C1-4 alkanes (such as methane, ethane, propane), C2-4 olefins (such as ethylene, propylene, 1-butene), and C2-4 alkynes (such as acetylene, propyne); for example, the process conditions are: reaction at 400°C~1000°C in an inert atmosphere for 1h~8h.

[0031] Furthermore, in the flexible carbon fiber film-based silicon-carbon negative electrode material, the flexible carbon fiber film content is 40wt%~65wt%, the silicon content is 30 wt%~55wt%, and the rest is a carbon coating layer.

[0032] In a second aspect, the present invention further provides a lithium battery, the negative electrode of which includes the above-mentioned flexible carbon fiber film-based silicon-carbon negative electrode material.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1) The present invention uses phosphazene-based multi-arm boride and sacrificial agent, polyacrylonitrile to form a fiber membrane through electrospinning; then, a porous flexible carbon fiber membrane is obtained through pre-oxidation, carbonization, and activation; finally, a flexible carbon fiber membrane-based negative electrode material is obtained through silicon deposition and carbon coating. In the high-temperature carbonization stage, the phosphazene group of the phosphazene-based multi-arm boride forms a network crosslink with the aromatic structure in the pre-oxidized polyacrylonitrile, constructing the crosslinking of the carbon fiber on a microscopic scale, thereby improving the flexibility of the carbon fiber membrane; on the other hand, the addition of the phosphazene-based multi-arm boride in situ incorporates N, P, and B into the carbon fiber, realizing multi-atom co-doping and improving the conductivity of the carbon fiber membrane base. That is, the phosphazene-based multi-arm boride plays a crosslinking role, improves the flexibility of the carbon fiber membrane, and is also a multi-atom dopant. The flexible carbon fiber membrane has a stable self-supporting structure, and will not be damaged and unable to form a membrane during the bending and winding process. It does not need to add any conductive agent and binder, and can be directly used as a negative electrode material; when it is used as a negative electrode material for lithium batteries, the capacity loss rate is less than 3% under a pressure of 10t.

[0035] 2) The flexible carbon fiber membrane-based silicon-carbon negative electrode material prepared by the present invention is used in lithium batteries and has excellent electrochemical properties. The first reversible capacity reaches more than 1800 mAh / g, the first coulombic efficiency reaches more than 89%, and the capacity retention rate after 100 cycles remains above 91%. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A flexible carbon fiber film negative electrode material prepared by the present invention;

[0037] Figure 2 This is a SEM image of the flexible carbon fiber membrane prepared in Example 1;

[0038] Figure 3 The first cycle charge and discharge curve of a lithium battery assembled with the flexible carbon fiber film-based silicon-carbon negative electrode material prepared in Example 6 at a rate of 0.1C. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with specific examples, but the present invention is not limited to the following examples.

[0040] Unless otherwise specified, the experimental methods in the following examples are all conventional methods; the reagents and materials described can be obtained from commercial sources.

[0041] Polyacrylonitrile, polymethyl methacrylate, and polyvinyl pyrrolidone were purchased from Aladdin; the weight average molecular weight of polyacrylonitrile was 150,000, the weight average molecular weight of polymethyl methacrylate was 15,000, and the weight average molecular weight of polyvinyl pyrrolidone was 12,000.

[0042] Preparation of phosphazene-based multi-arm boron compounds

[0043] Preparation Example 1

[0044] (L1) 10 g of 4-formylphenylboronic acid and 20 g of anhydrous K2CO3 were dissolved in 100 g of tetrahydrofuran (THF) to form a mixed solution A; 7.6 g of hexachlorocyclotriphosphazene was dissolved in 100 g of THF at a molar ratio of hexachlorocyclotriphosphazene to 4-formylphenylboronic acid of 1:3.05 to form a solution B;

[0045] (L2) Slowly add solution B dropwise to mixed solution A over 1-2 h, and stir and reflux the mixture at 55 °C for 36 h under N2 protection to obtain a reaction mixture;

[0046] (L3) The reaction mixture was filtered, rotary evaporated, washed with deionized water, and dried under vacuum at 50°C for 12 h to obtain phosphazene multi-arm boride a.

[0047] Preparation Example 2

[0048] The rest is the same as Preparation Example 1, except that in step (L1), 4-(4-pyridine)phenylboronic acid is used instead of 4-formylphenylboronic acid to obtain phosphazene multi-arm boride b.

[0049] Preparation Example 3

[0050] The rest is the same as Preparation Example 1, except that in step (L1), 5-nitrile-2-fluorophenylboronic acid is used instead of 4-formylphenylboronic acid to obtain phosphazene multi-arm boride c.

[0051] Example 1

[0052] (S1) Dissolving 10 g of polyacrylonitrile, 1 g of polyvinyl pyrrolidone, and 2 g of phosphazene-based multi-arm boride a in 75 g of N,N-dimethylformamide (DMF) to form a spinning solution with a total concentration of 15 wt%; transferring the spinning solution into a syringe, placing the syringe in an electrospinning device, controlling the static voltage to 13 kV, the distance from the needle to the receiver to 15 cm, and the propulsion speed of the spinning solution to 0.9 mL / h, and performing electrospinning to obtain a fiber membrane precursor;

[0053] (S2) placing the fiber membrane precursor in a muffle furnace for pre-oxidation at a pre-oxidation temperature of 250 °C for a pre-oxidation time of 2 h to obtain a pre-oxidized film; placing the pre-oxidized film in a tubular furnace for carbonization at 800 °C for 1 h under a nitrogen atmosphere;

[0054] Then, the temperature of the tubular furnace was maintained, and the nitrogen was replaced with water vapor to activate and pore the carbonized sample. After activation for 1.5 hours, the water vapor was replaced with nitrogen, and the heating was stopped and the temperature was naturally cooled. After the temperature of the tubular furnace reached room temperature, the sample was taken out to obtain a flexible carbon fiber membrane with a fiber diameter of 0.8 μm.

[0055] (S3) Place the flexible carbon fiber film on a deposition table in a vacuum chamber and reduce the vacuum degree to 10 -5 Pa, and the temperature is raised to 600 ℃ at the same time; the gas delivery system is turned on, and dimethylsilane gas and carrier gas argon are introduced into the vacuum chamber at a flow rate of 1.5L / min; the plasma generator is started, and chemical vapor deposition is carried out for 6 hours; after the silicon deposition is completed, the flexible carbon fiber film with deposited silicon is placed in a deposition furnace, and the temperature of the deposition furnace is raised to 800 ℃ under a nitrogen atmosphere, and ethane gas is introduced at a flow rate of 3L / min for carbon coating for 2 hours to obtain a flexible carbon fiber membrane-based silicon-carbon negative electrode material.

[0056] Example 2

[0057] The rest is the same as Example 1, except that in step (S1), phosphazene multi-arm boride b is used instead of phosphazene multi-arm boride a; and the fiber diameter of the flexible carbon fiber membrane prepared in step (S2) is 1.0 μm.

[0058] Example 3

[0059] The rest is the same as Example 1, except that in step (S1), phosphazene multi-arm boride c is used instead of phosphazene multi-arm boride a; and the fiber diameter of the flexible carbon fiber membrane prepared in step (S2) is 0.9 μm.

[0060] Example 4

[0061] The rest is the same as Example 3, except that polymethyl methacrylate is used instead of polyvinyl pyrrolidone in step (S1); and the fiber diameter of the flexible carbon fiber membrane prepared in step (S2) is 0.8 μm.

[0062] Example 5

[0063] The rest is the same as Example 4, except that the amount of each material in step (S1) is different, specifically: 10g polyacrylonitrile, 2g polymethyl methacrylate, 3g phosphazene-based multi-arm boride c; the fiber diameter of the flexible carbon fiber membrane obtained in step (S2) is 0.7 μm.

[0064] Example 6

[0065] The rest is the same as Example 4, except that the amount of each material used in step (S1) is different, specifically: 10g polyacrylonitrile, 3g polymethyl methacrylate, 4g phosphazene multi-arm boride c; the fiber diameter of the flexible carbon fiber membrane obtained in step (S2) is 0.6 μm.

[0066] Example 7

[0067] The rest is the same as Example 4, except that the amount of each material used in step (S1) is different, specifically: 10g polyacrylonitrile, 4g polymethyl methacrylate, 5g phosphazene multi-arm boride c; the fiber diameter of the flexible carbon fiber membrane obtained in step (S2) is 0.5μm.

[0068] Comparative Example 1

[0069] The rest is the same as Example 1, except that the phosphazene multi-arm boride a is not used in step (S1).

[0070] Figure 1 The invention discloses a flexible carbon fiber membrane negative electrode material.

[0071] Figure 2 This is the SEM image of the flexible carbon fiber membrane prepared in Example 1.

[0072] Figure 3 The first cycle charge and discharge curve of a lithium battery assembled with the flexible carbon fiber film-based silicon-carbon negative electrode material prepared in Example 6 at a rate of 0.1C.

[0073] Testing and analysis

[0074] Pore ​​size distribution and specific surface area determination: According to the gas adsorption BET method of GB / T 19587-2017, a low-temperature nitrogen adsorption experiment was carried out on the flexible porous carbon fiber membrane-based negative electrode material prepared in the embodiment and the comparative example using a fully automatic specific surface area and micropore analyzer (BET) to determine its pore size distribution, pore volume and specific surface area. The data are shown in Table 1.

[0075] Table 1 Pore size distribution and specific surface area

[0076] .

[0077] It can be seen from Table 1 that the specific surface area of ​​the flexible porous carbon fiber membrane prepared in the embodiment of the present invention is as high as 1200 m 2 / g or more, pore volume is 0.4~0.6 cm 3 / g, which belongs to micro-mesopores.

[0078] Electrochemical performance test: The flexible carbon fiber membrane-based negative electrode materials prepared in the embodiment and the comparative example were subjected to electrochemical performance test. The specific method is as follows: the flexible porous carbon fiber membrane-based negative electrode material was cut into a pole piece with a diameter of 10 mm and used directly, metallic lithium was used as the counter electrode, and the electrolyte was 1 M LiPF6 (the solvent was a mixture of EC and DEC with a volume ratio of 1:1, and 5% volume of FEC was added) to assemble the battery; during the test, the discharge cut-off voltage was 0.005 V, the charge cut-off voltage was 1.5V, and the charge and discharge test was carried out under 0.1 C rate conditions; the test sample was kept at 10 t pressure for 10 s, and the capacitance test was carried out after compaction, and the capacity loss rate was obtained by comparison. The electrochemical performance test of the flexible carbon fiber membrane-based negative electrode materials prepared in the embodiment and the comparative example is shown in Table 2.

[0079] Table 2 Electrochemical performance test

[0080] .

[0081] As can be seen from Table 2, compared with Comparative Example 1, the flexible carbon fiber film-based negative electrode material prepared by the method of the present invention is directly used as the negative electrode of the lithium battery, and the capacity loss rate of the assembled lithium battery under a pressure of 10t is significantly lower, all lower than 3%, indicating that the carbon fiber film-based negative electrode material of the present invention has good flexibility and structural stability. At the same time, the assembled lithium battery also has good electrochemical properties, with an initial reversible capacity of more than 1800 mAh / g, an initial coulombic efficiency of more than 89%, and a capacity retention rate of more than 91% after 100 cycles.

[0082] In summary, the flexible carbon fiber membrane-based negative electrode material prepared by the present invention has good flexibility and high specific surface area and contains boron, nitrogen and phosphorus doped elements. It is directly used as the negative electrode of a lithium battery. The capacity loss rate of the assembled lithium battery under a pressure of 10t is less than 3%, and it has good electrochemical properties.

[0083] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A method for preparing a flexible carbon fiber membrane-based silicon-carbon negative electrode material, It is characterized in that The following steps are involved: (S1) dissolving polyacrylonitrile, a sacrificial agent, and a phosphazene-based multi-arm boride in an organic solvent to form a spinning solution, and electrospinning to obtain a fiber membrane precursor; the phosphazene-based multi-arm boride is prepared by reacting raw materials including hexachlorocyclotriphosphazene and phenylboronic acid compounds, and the molar ratio of hexachlorocyclotriphosphazene to phenylboronic acid compounds is 1:(3.05-3.2); the mass ratio of the polyacrylonitrile, the sacrificial agent, and the phosphazene-based multi-arm boride is 1:(0.1-0.4):(0.2-0.5); the phenylboronic acid compound is at least one of 2-formylphenylboronic acid, 4-formylphenylboronic acid, 4-(4-pyridine)phenylboronic acid, 4-nitrilephenylboronic acid, and 5-nitrile-2-fluorophenylboronic acid; (S2) The fiber membrane precursor is sequentially pre-oxidized, carbonized under an inert atmosphere, and activated to form pores to obtain a flexible carbon fiber membrane; (S3) The flexible carbon fiber membrane is subjected to vapor phase silicon deposition and carbon coating to obtain a flexible carbon fiber membrane-based silicon-carbon negative electrode material.

2. The preparation method according to claim 1, It is characterized in that The weight average molecular weight of the polyacrylonitrile in step (S1) is 50,000 to 150,000; and / or The sacrificial agent is at least one of polymethyl methacrylate and polyvinyl pyrrolidone, and has a weight average molecular weight of 5000 to 15000; and / or The organic solvent is at least one of N,N-dimethylacetamide (DMA) and N,N-dimethylformamide (DMF); the total concentration of polyacrylonitrile, sacrificial agent and phosphazene-based multi-arm boride in the spinning solution is 10wt%-20wt%.

3. The preparation method according to claim 1, It is characterized in that In step (S1), the conditions for electrospinning are: voltage 10-20 kV, distance between needle and receiving axis 10-20 cm, and propulsion speed of spinning solution 0.5-1.5 mL / h.

4. The preparation method according to claim 1, It is characterized in that In step (S1), the phosphazene-based multi-arm boride is prepared by a preparation method comprising the following steps: (L1) dissolving a phenylboronic acid compound and anhydrous carbonate in a solvent to form a mixed solution A; dissolving hexachlorocyclotriphosphazene in a solvent to form a solution B; (L2) adding solution B dropwise to the mixed solution A, stirring and reacting at 50-70°C under inert gas protection for 24-36 hours to obtain a reaction mixture; (L3) The reaction mixture is filtered, rotary evaporated, washed, and vacuum dried to obtain a phosphazene multi-arm boride.

5. The preparation method according to claim 1, It is characterized in that In step (S2), the pre-oxidation temperature is 220°C~270°C, and the time is 1 h~4 h; the carbonization temperature is 700°C~950°C, and the time is 0.5~2 h; the inert atmosphere is at least one of nitrogen, argon, and helium; the activator used in the activation pore making is at least one of water vapor, carbon dioxide, and air, and the conditions for the activation pore making are: temperature 500°C~1000°C, and time 1 h~4 h.

6. The preparation method according to claim 1, It is characterized in that The fiber diameter of the flexible carbon fiber membrane obtained in step (S2) is 0.1 μm~1.5 μm.

7. The preparation method according to claim 1, It is characterized in that In the flexible carbon fiber film-based silicon-carbon negative electrode material, the flexible carbon fiber film content is 40wt%~65wt%, the silicon content is 30 wt%~55wt%, and the rest is a carbon coating layer.

8. A lithium battery, It is characterized in that The negative electrode comprises a flexible carbon fiber membrane-based silicon-carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 7.