Bimodal medium-density polyethylene composition
By using a bimodal medium-density polyethylene composition, combined with high-molecular-weight and low-molecular-weight ethylene/α-olefin copolymers, the problem of insufficient processability of polyethylene resin for micro-irrigation drip tapes during processing has been solved, achieving higher processing speeds and improved service life.
Patent Information
- Application Number
- CN202380020009.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-11
- Filing Date
- 2023-02-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-02-09
AI Technical Summary
The polyethylene resin used in existing micro-irrigation drip tapes has limited processability during processing, making it impossible to produce products with suitable wall thickness and good tensile strength at the same time, resulting in insufficient service life.
The bimodal medium-density polyethylene composition, comprising high-molecular-weight and low-molecular-weight ethylene/α-olefin copolymers, achieves processing at higher extrusion speeds and maintains or improves tensile strength and service life through a combination of specific properties such as cross G'=G” and calculated low molecular weight density.
This technology enables the processing at higher speeds while maintaining or improving the tensile strength and service life of micro-irrigation drip tapes, thus meeting the production requirements of micro-irrigation drip tapes.
Smart Images

Figure CN118647262B_ABST
Abstract
Description
Technical Field
[0001] The embodiments disclosed herein generally relate to bimodal medium-density polyethylene compositions and micro-irrigation drip tapes comprising the bimodal medium-density polyethylene compositions. Background Technology
[0002] Micro-irrigation drip tape is a type of tubing used in irrigation systems to deliver and drip water, fertilizer, and / or nutrients. The US micro-irrigation drip tape market consumes over 120 mm pounds of polyethylene resin annually. Currently, micro-irrigation drip tape is primarily made of materials with a density of 0.939 g / cm³. 3 Up to 0.944 g / cm 3 The process involves forming unimodal polyethylene resins with a melt index (I2) of 0.2 g / 10 min to 0.3 g / 10 min and a molecular weight distribution greater than 15. However, existing polyethylene resins have limited processability because they lack certain properties that prevent processors from producing micro-irrigation drip tapes with suitable wall thicknesses while maintaining tensile strength and service life. Therefore, there remains a need for polyethylene compositions suitable for micro-irrigation drip tapes that possess the desired processability (e.g., can be processed faster at lower manufacturing costs) and maintain or improve tensile strength and service life as indicated by notched constant tensile load failure time. Summary of the Invention
[0003] Embodiments of this disclosure satisfy one or more of the aforementioned needs by providing a bimodal medium-density polyethylene composition that can be processed at higher extrusion speeds and exhibits improved or maintained tensile strength and notched constant tensile load failure time. Without being bound by any theory, in some embodiments, the bimodal medium-density polyethylene composition has specific properties, including, for example, cross G' = G (which indicates melt elasticity) and a calculated low molecular weight density, which, when compared to prior art compositions, allow the composition to be extruded at higher speeds. In some embodiments, the specific properties of the bimodal medium-density polyethylene composition (including its bimodality and calculated low molecular weight density) can help maintain or improve the service life of the bimodal medium-density polyethylene composition.
[0004] This document discloses a bimodal medium-density polyethylene composition. In one or more embodiments, the bimodal medium-density polyethylene composition comprises: (i) a high molecular weight (HMW) polyethylene component comprising an ethylene / α-olefin copolymer; and (ii) a low molecular weight (LMW) polyethylene component comprising an ethylene / α-olefin copolymer; the bimodal medium-density polyethylene composition has the following property: (a) 0.937 g / cm³ 3 Up to 0.949 g / cm 3(a) density; (b) melt index (I21) under high load from 12 g / 10 min to 30 g / 10 min; (c) isothermal crystallization half-life greater than 350 seconds at Tc+5 °C; (d) elongation at break greater than 3.6; (e) cross G' = G” at 30 kPa to 45 kPa; and (f) less than or equal to 0.974 g / cm³. 3 The calculated LMW density of the LMW polyethylene component; and the cross G' = G” and the calculated LMW density satisfy the following formula: [43.0 - cross G′ = G″] + 1230·(0.9731 - calculated LMW density) - 5.5745 ≥ 0.
[0005] In one or more embodiments, the bimodal medium-density polyethylene composition comprises: (i) a high molecular weight (HMW) polyethylene component comprising an ethylene / α-olefin copolymer; and (ii) a low molecular weight (LMW) polyethylene component comprising an ethylene / α-olefin copolymer; the bimodal medium-density polyethylene composition has the following property: (a) 0.937 g / cm³ 3 Up to 0.949 g / cm 3 (a) density; (b) high-load melt index (I21) of 12 g / 10 min to 30 g / 10 min; (c) isothermal crystallization half-life of greater than 360 seconds at Tc+5 °C; (d) elongation at break strain greater than 3.6; (e) cross G'=G” of 30 kPa to 45 kPa; (f) average SCB frequency of 2.4 to 10.0 short-chain branched (SCB) / 1000 carbons; and (g) average SCB frequency of LMW polyethylene components of 2.0 to 8.7 short-chain branched (SCB) / 1000 carbons; and wherein the cross G'=G” and the average short-chain branched (SCB) frequency of the LMW polyethylene component satisfy the following formula:
[0006] A micro-irrigation drip tape is also disclosed. This micro-irrigation drip tape comprises the bimodal medium-density polyethylene composition disclosed herein.
[0007] These and other implementation schemes are described in more detail in the Detailed Description of the Embodiments. Attached Figure Description
[0008] Figure 1 This is a perspective view of a micro-irrigation drip tape with a circular cross-section.
[0009] Figure 2 This is a graph of isothermal crystallization half-life (ICHT) measured at temperatures 3°C to 5°C above the crystallization temperature Tc. Detailed Implementation
[0010] The disclosed bimodal medium-density polyethylene composition is described in more detail below. The bimodal medium-density polyethylene composition is suitable for use as a micro-irrigation drip tape and can be used in a wide range of applications, including, for example, pipes, hoses, belts, etc. However, this disclosure should not be construed as limiting the embodiments set forth below, as this disclosure is an illustrative description of the embodiments described herein.
[0011] As used herein, the term "polymer" refers to a polymeric compound prepared by polymerizing monomers of the same or different types. Therefore, the general term polymer encompasses the term homopolymer (used to refer to a polymer prepared from only one type of monomer) and the term copolymer or interpolymer. Trace impurities (e.g., catalyst residues) may be incorporated into and / or within a polymer. A polymer can be a single polymer, a polymer blend, or a mixture of polymers comprising a mixture of polymers formed in situ during polymerization.
[0012] As used herein, the term "copolymer" refers to a polymer formed by the polymerization of at least two monomers with different structures. The term "copolymer" includes terpolymers.
[0013] As used herein, the terms "polyethylene" or "ethylene-based polymer" should mean a polymer comprising a majority (>50 mol%) unit derived from ethylene monomers. This includes polyethylene homopolymers and copolymers (meaning units derived from two or more comonomers). The terms "ethylene-based polymer" and "polyethylene" are used interchangeably. Generally, polyethylene can be produced in gas-phase fluidized bed reactors, liquid-phase slurry reactors, or liquid-phase solution reactors using heterogeneous catalyst systems (such as Ziegler-Natta catalysts) and homogeneous catalyst systems containing Group 4 transition metals and ligand structures (such as metallocenes, non-metallocene metal centers, heteroaryl groups, isovalent aryloxy ethers, phosphine imides, etc.). Combinations of heterogeneous and / or homogeneous catalysts can also be used in single-reactor or dual-reactor configurations.
[0014] As used herein, the term "composition" means a mixture of materials comprising the composition, as well as reaction products and decomposition products formed from the materials of the composition.
[0015] As used herein, the term "main chain" refers to the longest continuous polymer chain. All other polymer chains are referred to as side chains, branches, or graft polymer chains. As used herein, the term "short chain" or "short-chain branching" (SCB) refers to a branch derived from the main chain resulting from the polymerization of monomers containing three or more carbon atoms.
[0016] The terms “comprising,” “including,” “having,” and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether or not such components, steps, or procedures are specifically disclosed. For the avoidance of any doubt, unless stated to the contrary, all compositions claimed using the term “comprising” may include any additional additives, adjuvants, or compounds, whether polymerized or otherwise. In contrast, the term “consistently composed of” excludes any other components, steps, or procedures from any subsequently listed scope, except those that are not essential for operability. The term “composed of” excludes any ingredients, steps, or procedures not specifically described or listed.
[0017] The bimodal medium-density polyethylene composition of the present invention may include a combination of two or more embodiments as described herein. Some embodiments of the present invention relate to micro-irrigation drip tapes. Micro-irrigation drip tapes according to embodiments of the present invention comprise the bimodal medium-density polyethylene composition according to any one of the embodiments of the present invention disclosed herein. The micro-irrigation drip tape of the present invention may include a combination of two or more embodiments as described herein.
[0018] This document discloses a bimodal medium-density polyethylene composition. As used herein, the medium-density polyethylene composition has a content of 0.937 g / cm³. 3 Up to 0.949 g / cm 3 A medium-density polyethylene composition of a specific density. The bimodal medium-density polyethylene composition according to the embodiments disclosed herein comprises a high molecular weight (HMW) polyethylene component and a low molecular weight (LMW) polyethylene component. The HMW polyethylene component has a higher molecular weight than the LMW polyethylene component.
[0019] The bimodal medium-density polyethylene composition according to the embodiments disclosed herein is bimodal. A “bimodal” polyethylene composition contains two polyethylene fractions (e.g., an HMW polyethylene fraction and an LMW polyethylene fraction) produced under different polymerization conditions, including differences in any process conditions and / or catalyst systems, resulting in different molecular weights and / or different comonomer contents of the fractions. According to the embodiments disclosed herein, the first polyethylene fraction is the HMW polyethylene fraction, and the second polyethylene fraction is the LMW polyethylene fraction. The bimodal medium-density polyethylene composition can be a mechanical blend or an in-reactor blend of a high molecular weight polyethylene fraction and a low molecular weight polyethylene fraction. In one embodiment, the bimodal medium-density polyethylene composition is an in-reactor blend of an HMW polyethylene fraction and an LMW polyethylene fraction. For the avoidance of any doubt, the bimodal medium-density polyethylene compositions disclosed herein do not include and are not unimodal polyethylene having a single polyethylene fraction.
[0020] HMW polyethylene component
[0021] This bimodal medium-density polyethylene composition comprises an HMW polyethylene component. In some embodiments, the HMW component comprises an ethylene / α-olefin copolymer.
[0022] In some embodiments, the ethylene / α-olefin copolymer of the HMW polyethylene component comprises ethylene and α-olefin comonomers. Non-limiting examples of suitable α-olefins include C3-C20 α-olefins, or C4-C20 α-olefins, or C3-C10 α-olefins, or C4-C10 α-olefins, or C4-C8 α-olefins. Representative α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene. In one embodiment, the ethylene / α-olefin copolymer does not contain aromatic comonomers polymerized therein. In another embodiment, the ethylene / α-olefin copolymer is an ethylene / 1-hexene copolymer. In one embodiment, the ethylene / α-olefin copolymer consists of ethylene, C4-C8 α-olefin comonomers, and optional additives.
[0023] In one embodiment, based on the weight of the ethylene / α-olefin copolymer, the ethylene / α-olefin copolymer contains more than 50% by weight of ethylene-derived units, or 51% by weight, or 55% by weight, or 60% to 70% by weight, or 80% by weight, or 90% by weight, or 95% by weight of ethylene-derived units. In one embodiment, based on the weight of the ethylene / α-olefin copolymer, the ethylene / α-olefin copolymer contains complementary amounts of α-olefin comonomer-derived units, or less than 50% by weight, or 49% by weight, or 45% by weight, or 40% to 30% by weight, or 20% by weight, or 10% by weight, or 5% by weight of α-olefin comonomer-derived units. The comonomer content can be measured using any suitable technique, such as techniques based on nuclear magnetic resonance (“NMR”) spectroscopy, for example, by 13C NMR analysis as described in U.S. Patent No. 7,498,282 (which is incorporated herein by reference).
[0024] In some implementations, the HMW polyethylene component has a content of 0.914 g / cm³. 3 Up to 0.935 g / cm 3 The density is disclosed and included in this document as 0.914 g / cm³. 3 Up to 0.935 g / cm 3 All individual values and sub-ranges. For example, the HMW polyethylene component can have 0.914 g / cm³. 3 Up to 0.934 g / cm 3 0.916 g / cm 3 Up to 0.934 g / cm 3 0.915g / cm3 Up to 0.933 g / cm 3 0.917 g / cm 3 Up to 0.935 g / cm 3 0.920g / cm 3 Up to 0.935 g / cm 3 0.922g / cm 3 Up to 0.935 g / cm 3 0.924 g / cm 3 Up to 0.935 g / cm 3 0.926 g / cm 3 Up to 0.935 g / cm 3 0.928g / cm 3 Up to 0.935 g / cm 3 Or 0.930 g / cm 3 Up to 0.935 g / cm 3 The density of the HMW polyethylene component is measured according to ASTM D792.
[0025] In some embodiments, the HMW polyethylene component has a high-load melt index (I21) of 0.5 g / 10 min to 0.9 g / 10 min. All individual values and sub-ranges of 0.5 g / 10 min to 0.9 g / 10 min are disclosed and included herein. In some embodiments, the HMW polyethylene component may have a high-load melt index (I21) of 0.5 g / 10 min to 0.8 g / 10 min, 0.5 g / 10 min to 0.7 g / 10 min, 0.5 g / 10 min to 0.9 g / 10 min, 0.6 g / 10 min to 0.9 g / 10 min, 0.6 g / 10 min to 0.8 g / 10 min, or 0.7 g / 10 min to 0.8 g / 10 min, wherein the high-load melt index (I21) of the HMW polyethylene component is measured according to ASTM D1238 (190°C / 21.6 kg).
[0026] In some embodiments, the HMW polyethylene component has a high load melt index (I21) of 0.5 g / 10 min to 0.9 g / 10 min and / or has 0.914 g / cm³. 3 Up to 0.935 g / cm 3 The density.
[0027] In some embodiments, the HMW polyethylene component is present in an amount of 48 wt% to 60 wt% based on the total weight of the bimodal medium-density polyethylene composition. This document includes and discloses all individual values and sub-ranges of 48 wt% to 60 wt%. For example, the HMW polyethylene component may be present in amounts of 48 wt% to 60 wt%, 50 wt% to 60 wt%, 52 wt% to 60 wt%, 53 wt% to 60 wt%, 48 wt% to 58 wt%, 48 wt% to 56 wt%, 50 wt% to 58 wt%, 50 wt% to 56 wt%, 52 wt% to 58 wt%, or 52 wt% to 56 wt% based on the total weight of the bimodal medium-density polyethylene composition.
[0028] In some embodiments, the HMW polyethylene component has an average SCB frequency of 2.3 to 10.0 short-chain branched (SCB) / 1000 carbons. This document discloses and includes all individual values and sub-ranges of 2.3 to 10.0 SCB / 1000 carbons. For example, the HMW polyethylene component may have average SCB frequencies of 2.4 to 9.5 short-chain branched (SCB) / 1000 carbons, 2.5 to 9.2 SCB / 1000 carbons, 2.6 to 9.0 SCB / 1000 carbons, 2.6 to 4.9 SCB / 1000 carbons, 2.6 to 4.8 SCB / 1000 carbons, 2.6 to 4.7 SCB / 1000 carbons, 2.6 to 4.6 SCB / 1000 carbons, and 2.6 to 4.5 SCB / 1000 carbons, wherein the average SCB frequency can be measured according to the test methods described below.
[0029] In some embodiments, the HMW polyethylene component has a weight-average molecular weight Mw of 300,000 g / mol to 550,000 g / mol. This document discloses and includes all individual values and sub-ranges of 300,000 g / mol to 550,000 g / mol. For example, the HMW polyethylene component may have a weight-average molecular weight Mw of 325,000 g / mol to 475,000 g / mol, 350,000 g / mol to 450,000 g / mol, or 350,000 g / mol to 425,000 g / mol, wherein the weight-average molecular weight Mw can be measured according to the GPC test method described below.
[0030] LMW polyethylene component
[0031] This bimodal medium-density polyethylene composition comprises an LMW polyethylene component. In some embodiments, the LMW component comprises an ethylene / α-olefin copolymer.
[0032] In some embodiments, the ethylene / α-olefin copolymer of the LMW polyethylene component comprises ethylene and α-olefin comonomers. Non-limiting examples of suitable α-olefins include C3-C20 α-olefins, or C4-C20 α-olefins, or C3-C10 α-olefins, or C4-C10 α-olefins, or C4-C8 α-olefins. Representative α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene. In one embodiment, the ethylene / α-olefin copolymer does not contain aromatic comonomers polymerized therein. In another embodiment, the ethylene / α-olefin copolymer is an ethylene / 1-hexene copolymer. In one embodiment, the ethylene / α-olefin copolymer consists of ethylene, C4-C8 α-olefin comonomers, and optional additives.
[0033] In one embodiment, based on the weight of the ethylene / α-olefin copolymer, the ethylene / α-olefin copolymer of the LMW polyethylene component contains more than 50% by weight of ethylene-derived units, or 51% by weight, or 55% by weight, or 60% to 70% by weight, or 80% by weight, or 90% by weight, or 95% by weight, or 99% by weight of ethylene-derived units. In one embodiment, based on the weight of the ethylene / α-olefin copolymer, the ethylene / α-olefin copolymer contains complementary amounts of units derived from α-olefin comonomers, or less than 50% by weight, or 49% by weight, or 45% by weight, or 40% to 30% by weight, or 20% by weight, or 10% by weight, or 5% by weight, or 1% by weight of units derived from α-olefin comonomers.
[0034] The ethylene / α-olefin copolymers of the LMW polyethylene component and the HMW polyethylene component differ at least in terms of the molecular weight of the respective components. In one embodiment, the weight-average molecular weight Mw of the LMW polyethylene component is less than that of the HMW polyethylene component, and the density of the LMW polyethylene component is greater than that of the HMW polyethylene component.
[0035] The LMW polyethylene component has a calculated LMW density. In some embodiments, the calculated LMW density of the LMW polyethylene component is less than or equal to 0.974 g / cm³. 3 This document discloses and includes values less than or equal to 0.974 g / cm³. 3 All individual values and sub-ranges. For example, the LMW polyethylene component can have a value less than or equal to 0.973 g / cm³. 3 Less than or equal to 0.972 g / cm³ 3 Less than or equal to 0.971 g / cm³ 3 Less than or equal to 0.969 g / cm³ 3 Less than or equal to 0.968 g / cm³ 3Less than or equal to 0.967 g / cm³ 3 Less than or equal to 0.966 g / cm³ 3 Less than or equal to 0.965 g / cm³ 3 or less than or equal to 0.964 g / cm³ 3 Or at 0.960 g / cm 3 Up to 0.973 g / cm 3 0.960 g / cm 3 Up to 0.972 g / cm 3 0.960 g / cm 3 Up to 0.971 g / cm 3 Or 0.960 g / cm 3 Up to 0.970 g / cm 3 The LMW density is calculated within the specified range. The LMW density of the polyethylene component is calculated using Formula 1:
[0036]
[0037] Wherein “HMW density” is the density of the HMW polyethylene component, “HMW weight fraction” is the weight fraction of the HMW polyethylene component, and “density” is the density of the bimodal medium-density polyethylene composition.
[0038] In some embodiments, the LMW polyethylene component has an average SCB frequency of 2.0 to 8.7 short-chain branching (SCB) / 1000 carbons. This document discloses and includes all individual values and sub-ranges of 2.0 to 8.7 SCB / 1000 carbons. For example, LMW polyethylene components may have an average SCB frequency of 2.0 to 8.5 short-chain branching (SCB) / 1000 carbon, 2.0 to 8.3 SCB / 1000 carbon, 2.0 to 8.1 SCB / 1000 carbon, 2.0 to 7.9 SCB / 10000 carbon, 2.0 to 7.7 SCB / 1000 carbon, 2.2 to 7.5 SCB / 1000 carbon, 2.4 to 7.5 SCB / 1000 carbon, 2.6 to 7.3 SCB / 1000 carbon, 2.8 to 7.2 SCB / 1000 carbon, or 2.9 to 7.3 SCB / 1000 carbon, wherein the average short-chain branching (SCB) frequency can be measured according to the test methods described below.
[0039] In some embodiments, the LMW polyethylene component has a weight-average molecular weight (Mw) of 15,000 g / mol to 40,000 g / mol. This document discloses and includes all individual values and sub-ranges of 15,000 g / mol to 40,000 g / mol. For example, the LMW polyethylene component may have a weight-average molecular weight (Mw) of 20,000 g / mol to 40,000 g / mol, 20,000 g / mol to 35,000 g / mol, or 20,000 g / mol to 30,000 g / mol, wherein the weight-average molecular weight (Mw) can be measured according to the GPC test method described below.
[0040] In some embodiments, the ratio of the average short-chain branching frequency of the LMW polyethylene component to that of the HMW polyethylene component (LMW SCB / HMW SCB) is greater than 0.7. This document includes and discloses all individual values and sub-ranges greater than 0.7. For example, the ratio of the average short-chain branching frequency of the LMW polyethylene component to that of the HMW polyethylene component (LMW SCB / HMW SCB) may be greater than 0.75 or greater than 0.80, or may be in the range of 0.75 to 2.00 or 0.75 to 1.80.
[0041] Characteristics of bimodal medium-density polyethylene compositions
[0042] In some embodiments, the bimodal medium-density polyethylene composition has a content of 0.937 g / cm³. 3 Up to 0.949 g / cm 3 The density, total high-load melt index (I21) from 12 g / 10 min to 30 g / 10 min, and cross G' = G from 30 kPa to 45 kPa.
[0043] In some embodiments, the bimodal medium-density polyethylene composition has a content of 0.937 g / cm³. 3 Up to 0.949 g / cm 3 The density is disclosed and included in this document as 0.937 g / cm³. 3 Up to 0.949 g / cm 3 All individual values and sub-ranges. For example, a bimodal medium-density polyethylene composition can have 0.938 g / cm³. 3 Up to 0.949 g / cm 3 0.939 g / cm 3 Up to 0.949 g / cm 3 0.940 g / cm 3 Up to 0.949 g / cm 3 0.941 g / cm 3 Up to 0.949 g / cm 3 0.942 g / cm3 Up to 0.949 g / cm 3 0.938g / cm 3 Up to 0.947 g / cm 3 0.940 g / cm 3 Up to 0.947 g / cm 3 0.941 g / cm 3 Up to 0.947 g / cm 3 Or 0.943 g / cm 3 Up to 0.947 g / cm 3 The density, where the density is measured according to ASTM D792.
[0044] In some embodiments, the bimodal medium-density polyethylene composition has a high-load melt index (I21) of 12 g / 10 min to 30 g / 10 min. All individual values and sub-ranges of 12 g / 10 min to 30 g / 10 min are disclosed and included herein. For example, the bimodal medium-density polyethylene composition may have a high-load melt index (I21) of 12 g / 10 min to 28 g / 10 min, 12 g / 10 min to 26 g / 10 min, 12 g / 10 min to 24 g / 10 min, 14 g / 10 min to 30 g / 10 min, 14 g / 10 min to 28 g / 10 min, 14 g / 10 min to 26 g / 10 min, or 14 g / 10 min to 24 g / 10 min, wherein the high-load melt index (I21) of the bimodal medium-density polyethylene composition is measured according to ASTM D1238 (190°C / 21.6 kg).
[0045] In some embodiments, the bimodal medium-density polyethylene composition has a cross G' = G" of 30 kPa to 45 kPa. This document discloses and includes all individual values and sub-ranges of 30 kPa to 45 kPa. For example, the bimodal medium-density polyethylene composition may have a cross G' = G" of 32 kPa to 45 kPa, 30 kPa to 43 kPa, 34 kPa to 45 kPa, or 30 kPa to 42 kPa, wherein the cross G' = G" is measured according to the test methods described below.
[0046] In some implementations, the cross G' = G” and the calculated LMW density satisfy the following formula (Formula 2):
[0047] [43.0 – Cross G′=G″]+1230(0.9731 – Calculate LMW density) – 5.5745≥0 Formula 2
[0048] Wherein “cross G’=G” means “cross G’=G” for the bimodal medium-density polyethylene composition, and “calculate LMW density” means “calculate LMW density” for the LMW polyethylene component. In some embodiments, the left side of Formula 2 is greater than or equal to 1, or greater than or equal to 2, or greater than or equal to 3, or greater than or equal to 4.
[0049] In some implementations, the average short-chain branching frequency of the cross-linked G' = G” and LMW polyethylene components satisfies the following formula (Formula 3):
[0050]
[0051] Wherein “cross G’=G” is the cross G’=G of the bimodal medium-density polyethylene composition, and “LMW SCB” is the average short-chain branching frequency of the LMW polyethylene component. In some embodiments, the left side of Formula 3 is greater than or equal to 1, or greater than or equal to 2, or greater than or equal to 3, greater than or equal to 4, greater than or equal to 5, or greater than or equal to 6.
[0052] In some embodiments, the bimodal medium-density polyethylene composition has a molecular weight distribution (Mw / Mn) of 12 to 30. This document includes all individual values and sub-ranges of 12 to 30. For example, the bimodal medium-density polyethylene composition may have a molecular weight distribution (Mw / Mn) of 12 to 28, 12 to 26, 12 to 24, 12 to 22, 12 to 20, 14 to 28, 14 to 26, 14 to 24, 14 to 22, or 14 to 20, wherein the molecular weight distribution (Mw / Mn) can be measured according to the test methods described below.
[0053] In some embodiments, the bimodal medium-density polyethylene composition has an average SCB frequency of 2.4 to 10.0 short-chain branchings (SCBs) per 1000 carbons. This document discloses and includes all individual values and sub-ranges of 2.4 to 10.0 SCBs per 1000 carbons. For example, the bimodal medium-density polyethylene composition may have an average SCB frequency of 2.4 to 9.5 short-chain branchings (SCBs) per 1000 carbons, 2.6 to 9.5 SCBs per 1000 carbons, 2.8 to 9.5 SCBs per 1000 carbons, 3.0 to 9.5 SCBs per 1000 carbons, 3.5 to 9.5 SCBs per 1000 carbons, 3.0 to 9.0 SCBs per 1000 carbons, or 3.5 to 9.0 SCBs per 1000 carbons, wherein the average short-chain branching (SCB) frequency can be measured according to the test methods described below.
[0054] In some embodiments, the bimodal medium-density polyethylene composition has a notched constant tensile load (NCTL) failure time greater than 100 hours at 30% yield stress. In some embodiments, the bimodal medium-density polyethylene composition has an NCTL failure time greater than 110 hours, or 120 hours, or 140 hours, or 160 hours, or 180 hours at 30% yield stress, wherein the NCTL failure time at 30% yield stress is measured according to the test methods described below.
[0055] In some embodiments, the bimodal medium-density polyethylene composition has a yield tensile stress of 19 MPa to 28 MPa. All individual values and sub-ranges of 19 MPa to 28 MPa are disclosed and included herein. For example, the bimodal medium-density polyethylene composition may have a yield tensile stress of 19 MPa to 27 MPa, 19 MPa to 26 MPa, 19 MPa to 25 MPa, 19 MPa to 24 MPa, 20 MPa to 27 MPa, 20 MPa to 26 MPa, 20 MPa to 25 MPa, or 20 MPa to 24 MPa, wherein the yield tensile stress is measured according to the test methods described below.
[0056] In some embodiments, the bimodal medium-density polyethylene composition has a DSC melt temperature Tm in the range of 125°C to 135°C. All individual values and sub-ranges of 125°C to 135°C are disclosed and included herein. For example, the bimodal medium-density polyethylene composition may have a DSC melt temperature Tm in the ranges of 126°C to 134°C, 127°C to 133°C, 125°C to 132°C, 125°C to 131°C, or 125°C to 130°C, wherein the DSC melt temperature Tm can be measured according to the test methods described below.
[0057] In some embodiments, the bimodal medium-density polyethylene composition has a DSC crystallization temperature Tc in the range of 110°C to 125°C. All individual values and sub-ranges of 110°C to 125°C are disclosed and included herein. For example, the bimodal medium-density polyethylene composition may have a DSC crystallization temperature Tc in the range of 111°C to 124°C, 113°C to 122°C, 115°C to 120°C, or 116°C to 118°C, wherein the DSC crystallization temperature Tc can be measured according to the test methods described below.
[0058] In some embodiments, the bimodal medium-density polyethylene composition has an isothermal crystallization half-life at Tc+5°C greater than 360 seconds (sec). This document discloses and includes all individual values and sub-ranges greater than 360 seconds. For example, the bimodal medium-density polyethylene composition may have an isothermal crystallization half-life at Tc+5°C greater than 361 seconds, greater than 362 seconds, greater than 380 seconds, greater than 400 seconds, or greater than 410 seconds, or may have an isothermal crystallization half-life at Tc+5°C from 360 seconds to 500 seconds, wherein the isothermal crystallization half-life at Tc+5°C is measured according to the test methods described below.
[0059] In some embodiments, the bimodal medium-density polyethylene composition has an elongation at break greater than 3.6. All individual values and sub-ranges greater than 3.6 are disclosed and included herein. For example, the bimodal medium-density polyethylene composition may have an elongation at break greater than 3.7, greater than 3.8, greater than 3.9, or greater than 4.0, or in the range of 3.8 to 7.0, wherein the elongation at break can be measured according to the test methods described below.
[0060] In some embodiments, the bimodal medium-density polyethylene composition can be extruded at a processing speed greater than 300 m / min. In some embodiments, the bimodal medium-density polyethylene composition can be extruded at a processing speed greater than 325 m / min, 350 m / min, or 375 m / min, wherein the processing speed at which the polyethylene composition can be extruded is measured according to the test methods described below.
[0061] Bimodal medium-density polyethylene compositions can be produced by a variety of methods. For example, such methods can include, but are not limited to, gas-phase polymerization processes, slurry-phase polymerization processes, liquid-phase polymerization processes, and combinations thereof using one or more conventional reactors (e.g., fluidized bed gas-phase reactors, circulating reactors, stirred tank reactors, parallel, series batch reactors, and / or any combination thereof). Alternatively, bimodal medium-density polyethylene compositions can be produced in a high-pressure reactor via a coordination catalyst system. For example, bimodal medium-density polyethylene compositions can be produced in a gas-phase reactor via a gas-phase polymerization process; however, any of the polymerization processes described above can be used. In one embodiment, the polymerization reactor can comprise two or more reactors in series, parallel, or in combination thereof, wherein each polymerization occurs in solution, in a slurry, or in the gas phase. In another embodiment, a dual-reactor configuration is used, wherein the polymer produced in the first reactor can be a high-molecular-weight polyethylene component or a low-molecular-weight polyethylene component. The polymer produced in the second reactor can have a density and melt flow rate that conform to the total density and melt flow rate of the bimodal medium-density polyethylene composition. Similar polymerization processes are described, for example, in USP 7,714,072, which is incorporated herein by reference.
[0062] In one embodiment, a method of producing a bimodal medium-density polyethylene composition includes polymerizing a high molecular weight (HMW) polyethylene component as previously described herein in a reactor, and polymerizing a low molecular weight (LMW) polyethylene component as previously described herein in a separate reactor, thereby producing a bimodal medium-density polyethylene composition. The two reactors may be operated in series. In some embodiments, the HMW polyethylene component is polymerized in a first reactor, and the LMW polyethylene component is polymerized in a second reactor. In other embodiments, the LMW polyethylene component is polymerized in a first reactor, and the HMW polyethylene component is polymerized in a second reactor.
[0063] In one embodiment, the weight ratio of the copolymer prepared in the high molecular weight reactor to the copolymer prepared in the low molecular weight reactor is in the range of 30:70 to 70:30, or in the range of 40:60 to 60:40. This is also referred to as polymer split.
[0064] In one embodiment, a bimodal medium-density polyethylene (MDPE) composition is produced using at least one Ziegler-Natta (ZN) catalyst system. In other embodiments, the MDPE composition is produced using multiple reactors in series, wherein a ZN catalyst is fed into each reactor or only into the first reactor. In other embodiments, the ZN catalyst system may be fed into one or two sequentially configured, independently controlled reactors and operated in a solution, slurry, or gas phase. In even further embodiments, the ZN catalyst system may be fed into one or two sequentially configured, independently controlled reactors and operated in the gas phase. Sequential polymerization can be performed such that a freshly prepared catalyst is injected into one reactor, and an active catalyst is carried from the first reactor to the second reactor. The resulting MDPE composition can be characterized as comprising component polymers, each having a distinct unimodal molecular weight distribution. As used herein, when “distinct” refers to the molecular weight distributions of the high-molecular-weight polyethylene component and the low-molecular-weight polyethylene component, it indicates the presence of two corresponding molecular weight distributions in the GPC curve of the resulting MDPE composition. As used herein, when “single peak” is used to refer to the molecular weight distribution of the component polymers in a bimodal medium-density polyethylene composition, it indicates that the molecular weight distribution in the GPC curve of the component polymers will not present multiple molecular weight distributions.
[0065] The terms “primary catalyst” or “precursor” are used interchangeably herein and refer to compounds comprising ligands, transition metals, and optionally electron donors. A primary catalyst may be additionally halogenated by contact with one or more halogenating agents. Upon activation, the primary catalyst can be converted into a catalyst. Such catalysts are commonly referred to as Ziegler-Natta catalysts. Suitable Ziegler-Natta catalysts are known in the art and include, for example, catalysts taught in U.S. Patent Nos. 4,302,565; 4,482,687; 4,508,842; 4,990,479; 5,122,494; 5,290,745; and 6,187,866B1, the disclosure of which is incorporated herein by reference. A collection of catalyst components (such as one or more primary catalysts, one or more co-catalysts) is called a catalyst system.
[0066] The transition metal compounds in the main catalyst composition can include various classes of compounds. The most common are organic or inorganic titanium compounds with an oxidation state of 3 or 4. Other transition metals, such as vanadium, zirconium, hafnium, chromium, molybdenum, cobalt, nickel, tungsten, and many rare earth metals, are also suitable for use in Ziegler-Natta catalysts. Transition metal compounds are typically halides or halide oxides, organometallic halides, or pure organometallic compounds. In the last mentioned compounds, only the organic ligand is attached to the transition metal.
[0067] In one embodiment, the main catalyst has the formula Mg d Me(OR) e X f (ED) g In the form of a COR', R is an aliphatic or aromatic hydrocarbon group having 1 to 14 carbon atoms; each OR group may be the same or different; X is independently chlorine, bromine, or iodine; ED is an electron donor; d is 0.5 to 56; e is 0, 1, or 2; f is 2 to 116; and g > 1 to 1.5(d); Me is a transition metal selected from the group consisting of titanium, zirconium, hafnium, and vanadium. Some specific examples of suitable titanium compounds are: TiCl3, TiCl4, Ti(OC2H5)2Br2, Ti(OC6H5)Cl3, Ti(OCOCH3)Cl3, Ti(acetylacetate)2Cl2, TiCl3(acetylacetate), and TiBr4.
[0068] Magnesium compounds include magnesium halides such as MgCl2 (including anhydrous MgCl2), MgBr2, and MgI2. Other suitable compounds, without limitation, include Mg(OR)2, Mg(OCO2Et), and MgRCl, where R is as defined above. Use 0.5 to 56 moles or 1 to 20 moles of magnesium compound per mole of transition metal compound. Mixtures of these compounds may also be used.
[0069] With or without a packing agent, the main catalyst compound can be recovered in solid form using techniques known in the art, such as deposition of the main catalyst or by spray drying. Spray drying is a particularly preferred method for recovering the main catalyst compound. Spray drying is taught in U.S. Patent 5,290,745 and is incorporated herein by reference. Another main catalyst comprising magnesium halides or alkoxides, transition metal halides, alkoxides or mixed ligand transition metal compounds, an electron donor, and optionally a packing agent can be prepared by spray drying a solution of said compound from an electron donor solvent.
[0070] Electron donors are typically organic Lewis bases, liquids in the temperature range of 0°C to 200°C, wherein magnesium and transition metal compounds are soluble. Electron donors can be alkyl esters, fatty ketones, fatty amines, fatty alcohols, alkyl ethers, or cycloalkyl ethers of aliphatic or aromatic carboxylic acids, or mixtures thereof, each having 2 to 20 carbon atoms. Among these electron donors, preferred are alkyl and cycloalkyl monoethers having 2 to 20 carbon atoms; dialkyl, diaryl, and alkylaryl ketones having 3 to 20 carbon atoms; and alkyl, alkoxy, and alkylalkoxy esters of alkyl and aryl carboxylic acids having 2 to 20 carbon atoms. A monoether is defined herein as a compound containing only one ether functional group in its molecule. For ethylene homopolymerization and copolymerization, tetrahydrofuran is the most preferred electron donor. Other examples of suitable electron donors are methyl formate, ethyl acetate, butyl acetate, diethyl ether, dioxane, di-n-propyl ether, dibutyl ether, ethanol, 1-butanol, ethyl formate, methyl acetate, ethyl anisinate, ethylene carbonate, tetrahydropyran, and ethyl propionate.
[0071] Initially, an excess of electron donors can be used to provide the reaction products of the transition metal compound and the electron donor, and the final reaction products contain 1 to 20 moles of electron donors per mole of the transition metal compound, or 1 to 10 moles of electron donors per mole of the transition metal compound. Ligands include halogens, alkoxides, aryl oxides, acetylacetonates, and amide anions.
[0072] Partial activation of the main catalyst can occur before it is introduced into the reactor. While a partially activated catalyst can function as a polymerization catalyst on its own, its catalyst productivity is significantly reduced and it is not commercially viable. Full activation with an additional co-catalyst is required to achieve adequate activity. Full activation is achieved in the polymerization reactor by adding a co-catalyst.
[0073] The catalyst can be used in dry powder form or as a slurry in an inert liquid. The inert liquid is typically mineral oil. A slurry prepared from the catalyst and the inert liquid can withstand temperatures up to 1 second at 20°C. -1 The viscosity measured below must be at least 500 cp (500 mPa·s). A non-limiting example of a suitable mineral oil is Kaydol from Crompton. TM and Hydrobrite TM Mineral oil.
[0074] In one embodiment of the polymerization process, the main catalyst is continuously reduced using one or more reducing agents. The main catalyst is introduced into a slurry feed tank; the slurry is then pumped to a first reaction zone immediately downstream of a reagent inlet, where it is mixed with a first reagent as described below. Optionally, the mixture is then passed to a second reaction zone immediately downstream of a second reagent inlet, where it is mixed with a second reagent (as described below). Although only two reagent inlets and reaction zones are described above, additional reagent inlets and reaction zones may be included depending on the number of steps required to thoroughly activate and modify the catalyst to allow control of the polymer molecular weight distribution of a specified portion. Methods for controlling the temperature of the main catalyst feed tank and the individual mixing and reaction zones are provided.
[0075] Depending on the activator compound used, the reaction between the activator compound and the catalyst may require a certain reaction time. This is preferably achieved using a residence time zone, which can consist of either an extra-long slurry feed pipe or a vessel that essentially maintains plug flow. The residence time zone can be used with two activator compounds, with only one, or with neither, depending entirely on the reaction rate between the activator compound and the catalyst.
[0076] The exemplary continuous reducing agent is of formula AlR x Cl y Aluminum alkyl groups and aluminum alkyl chlorides, wherein X+Y = 3, and y is 0 to 2, and R is C1 to C14 alkyl or aryl. Non-limiting examples of continuous reducing agents include diethylaluminum chloride, ethylaluminum dichloride, diisobutylaluminum chloride, dimethylaluminum chloride, methylaluminum sesquichloride, ethylaluminum sesquichloride, triethylaluminum, trimethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, and dimethylaluminum chloride.
[0077] The entire mixture is then introduced into a reactor that has been activated by a co-catalyst. Additional reactors may be sequenced with the first reactor; however, typically only the catalyst is injected into the first of these connected, sequenced reactors, where the active catalyst is transferred from the first reactor to the subsequent reactor as part of the polymer thus produced.
[0078] Commonly used co-catalysts for reducing agents are composed of aluminum compounds, but compounds of lithium, sodium, and potassium, alkaline earth metals, and other earth metals are also possible. The compounds are typically hydrides, organometallic compounds, or halide compounds. Typically, co-catalysts are selected from the group comprising trialkylaluminum, alkylaluminum halides, alkylaluminum alkoxides, and alkylaluminum halides. Specifically, alkylaluminum and alkylaluminum chlorides are used. Examples of these compounds include trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, dimethylaluminum chloride, diethylaluminum chloride, ethylaluminum dichloride, diisobutylaluminum chloride, and isobutylaluminum dichloride. Butyllithium and dibutylmagnesium are examples of other useful metal compounds.
[0079] The bimodal medium-density polyethylene composition may include two or more embodiments discussed herein.
[0080] This document also discloses a micro-irrigation drip tape. The micro-irrigation drip tape comprises the bimodal medium-density polyethylene composition described herein. A “micro-irrigation drip tape” is an extruded structure having an annular wall composed of a bimodal medium-density polyethylene composition, which defines an annular channel. In other words, a micro-irrigation drip tape is a pipe through which water or another liquid can pass. Figure 1 A micro-irrigation drip tape 10 is depicted having an annular wall 12 defining an annular channel 14. The annular wall 12 has an outer surface 16 and an inner surface 18. In an embodiment, the annular wall 12 of the micro-irrigation drip tape 10 is composed solely of a bimodal medium-density polyethylene composition.
[0081] The emitters 20 are arranged at intervals along the inner surface 18 of the annular wall 12. An "emitter" is an insert that controls the rate at which water or another liquid passes through an opening 22 (e.g., a hole, slit, or perforation), which is formed in the annular wall by mechanical drilling, cutting, or laser cutting. After the micro-irrigation drip tape 10 exits the extruder, the emitters 20 are placed on the inner surface 18 of the annular wall 12 while the formulation is transitioning from a molten state to a rigid state, allowing the emitters 20 to adhere to the micro-irrigation drip tape 10 via welding. The adhesion of the emitters 20 to the annular wall 12 is sufficient to hold the emitters 20 in place and maintain a leak-proof seal between the annular wall 12 and the emitters 20.
[0082] Micro-irrigation drip tape has a cross-sectional shape. Non-limiting examples of suitable cross-sectional shapes for micro-irrigation drip tape include ellipses, polygons, and combinations thereof. A "polygon" is a closed planar figure defined by at least three boundaries. A polygon can be a regular polygon or an irregular polygon with three, four, five, six, seven, eight, nine, ten, or more sides. Non-limiting examples of suitable polygonal shapes include triangles, squares, rectangles, rhombuses, trapezoids, parallelograms, hexagons, and octagons. An "ellipse" is a plane curve such that the sum of the distances from each point on its perimeter to two fixed points (foci) is equal. The center of the ellipse is the midpoint of the line segment connecting the two foci. An ellipse has a major axis (the longest diameter passing through the center). The minor axis is the shortest line passing through the center. The center of the ellipse is the intersection of the major and minor axes. A "circle" is a specific form of ellipse in which the two foci are located in the same position (at the center of the circle). Non-limiting examples of elliptical shapes include circles, ovals, and oval shapes. Figure 1 Depict a micro-irrigation drip tape 10 with a circular cross-sectional shape.
[0083] Test methods
[0084] density
[0085] Density was measured according to ASTM D792 and expressed in grams per cubic centimeter. 3 (g / cm 3 (or g / cc) indicates.
[0086] Melt flow rates (I2, I5, and I21)
[0087] Melt flow rate was determined according to the procedure described in ASTM D1238. This test method involves determining the extrusion rate of molten thermoplastic resin using an extruder. After a specific preheating time of 7 (+ / - 0.5) minutes, the resin was extruded through a die with a specific length and orifice diameter under specified temperature, load, and piston position in the barrel. Method B of ASTM D1238 was used. Method B is an automated timing method. Here, the sample is extruded from a melt indexer, and the piston stroke is timed over a predetermined distance, automatically controlled by the position of a movable arm located below the load frame. For I2 up to 10 g / 10 min, the predetermined distance is 6.35 mm; for I2 > 10 g / 10 min, the predetermined distance is 25.4 mm. The weight of the extrudate was determined by volume (distance × orifice area) and melt density. The melt density of polyethylene was taken as 0.7636 g / cm³. 3 Data are reported as MFR in g / 10min or dg / min. Samples can be run at loads of 21.6 kg, 5.0 kg, or 2.16 kg (i.e., I21, I5, or I2, respectively).
[0088] Notched Constant Tensile Load (NCTL)
[0089] According to ASTM D5397, the notched constant tensile load (NCTL) failure time is measured in hours at 30% yield stress. The test is performed at 50°C in a 10% Igepal solution. The sample thickness is 0.075" and the notch is to a depth of 20% of the thickness. The applied stress is equal to 30% of the resin yield stress measured at room temperature.
[0090] Yield tensile stress
[0091] According to ASTM D638 (crosshead speed 2 inches / min) (crosshead speed 5.08 cm / min), the yield tensile stress (in MPa) of bimodal medium-density polyethylene compositions was measured using samples prepared from compression-molded pellets.
[0092] Dynamic mechanical spectrum (crossing G' = G”)
[0093] Each sample was compressed and molded into a disc for rheological measurements. Discs were prepared by pressing the sample into a 3.0 mm thick plate and then cutting it into 25 mm diameter discs. Resin rheology was measured on an ARES-G2 rheometer from TA Instruments. ARES is a strain-controlled rheometer. A rotary actuator (servo motor) applied shear deformation in the form of strain to the sample. In response, the sample generated torque, which was measured by a transducer. Strain and torque were used to calculate dynamic mechanical properties such as modulus and viscosity. Viscoelastic properties of the sample were measured in the melt using a 25 mm diameter parallel plate apparatus at 190 °C as a function of the frequency of change (range 0.01 s⁻¹ to 100 s⁻¹). A small, constant strain (5%) was applied to ensure the measurements were performed in the linear viscoelastic region. The storage modulus (G'), loss modulus (G"), tanδ(G" / G'), and complex viscosity (η) of the resin were determined. The cross G' = G” is recorded in kPa as a measure of melt elasticity, where the lower the value, the higher the melt elasticity.
[0094] Differential scanning calorimetry (DSC)
[0095] DSC thermal analysis plots were obtained using a TA Instrument Discover DSC instrument and used to measure the melt temperature (Tm) and crystallization temperature (Tc) of polyethylene samples. 5 mg to 8 mg of coiled sample was heated to 150 °C for PE at a rate of 10 °C / min. The sample was held at the desired temperature for five minutes. The sample was then cooled to -40 °C at a rate of 10 °C / min to obtain cooling profile data. The sample was held at the desired temperature for five minutes. The sample was then heated to the temperature required for a second heating profile at a rate of 10 °C / min. The melt peak (Tm) and crystallization peak (Tc) of each polymer sample were processed using Universal Analysis software provided by TA Instruments and recorded.
[0096] To determine the isothermal crystallization half-life (ICHT), individual 5 mg to 8 mg coiled samples were heated to 150 °C for PE at a rate of 10 °C / min. The samples were held at the desired temperature for five minutes. The samples were then rapidly cooled to the desired isothermal temperature and held isothermally for 60 minutes. ICHT is taken as the time, in seconds, taken from the start of the crystallization isotherm to its peak. ICHT was measured at at least three temperatures 3 to 5 °C higher than the crystallization peak temperature Tc and at least 0.5 °C apart. The ICHT reported at Tc+5 °C was obtained from the measured ICHT temperatures using linear regression. Figure 2 A graph showing the isothermal crystallization half-life (ICHT) measured at temperatures 3 to 5 °C above the crystallization temperature Tc is presented. Extrapolated ICHT to Tc+5 °C is reported.
[0097] Absolute GPC (molecular weight distribution)
[0098] The chromatographic system consisted of a PolymerChar GPC-IR (Valencia, Spain) high-temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5) connected to a Precision Detector (now an Agilent Technologies 2040 model 2-angle laser scattering (LS) detector. A 15-degree angle was used for all light scattering measurements. The autosampler oven chamber was set to 160°C, and the column and detector chambers were set to 150°C. The columns used were four Agilent "Mixed A" 30 cm 20 μm linear mixed-bed columns. The chromatographic solvent used was 1,2,4-trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was nitrogen injection. The injection volume used was 200 μL, and the flow rate was 1.0 mL / min.
[0099] The calibration of the GPC column assembly was performed using 21 narrow molecular weight distribution polystyrene standards ranging from 580 g / mol to 8,400,000 g / mol, arranged in six “mixture” formulations with individual molecular weights spaced at least tenfold apart. The standards were purchased from Agilent Technologies. For molecular weights equal to or greater than 1,000,000 g / mol, the polystyrene standards were prepared at a concentration of 0.025 g per 50 mL of solvent, and for molecular weights less than 1,000,000 g / mol, at a concentration of 0.05 g per 50 mL of solvent. The polystyrene standards were dissolved by gentle stirring at 80 °C for 30 minutes. The molecular weights of the polystyrene standard peaks were converted to those of vinyl polymers using Formula 4 (as described by Williams and Ward in *Journal of Polymer Science: Polymer Reviews*, 6, 621 (1968)).
[0100] M 聚苯乙烯 =A×(M) 聚苯乙烯 ) B Formula 4
[0101] Where M is the molecular weight, A has a value of 0.4315, and B equals 1.0.
[0102] A fifth-order polynomial was used to fit the corresponding ethylene-based polymer-equivalent calibration point.
[0103] Total plate counts were performed on the GPC column using decane without further dilution. Plate counts and symmetry were measured at 200 μL injections according to the following formulas (Formula 5 and Formula 6):
[0104]
[0105] Where RV is the retention volume in milliliters, peak width is in milliliters, peak maximum is the maximum height of the peak, and half height is half the height of the peak maximum.
[0106]
[0107] Where RV is the retention volume in milliliters, and peak width is in milliliters, peak maximum is the position of the peak maximum, one-tenth height is one-tenth of the peak maximum height, and a subsequent peak refers to the tail of a peak at a retention volume later than the peak maximum, while a preceding peak refers to the front of a peak at a retention volume earlier than the peak maximum. The plate count of the chromatographic system should be greater than 18,000, and the symmetry should be between 0.98 and 1.22.
[0108] Samples were prepared semi-automatically using PolymerChar "Instrument Control" software, with a target sample weight of 2 mg / ml. Solvent (containing 200 ppm BHT) was added to a pre-bubbled, diaphragm-capped vial using a PolymerChar high-temperature autosampler. The sample was dissolved at 160°C for 3 hours with "low-speed" oscillation.
[0109] To monitor deviations over time, a flow rate marker (decane) was introduced into each sample via a micropump controlled by a PolymerChar GPC-IR system. This flow rate marker (FM) was used to linearly correct the pump flow rate (nominal flow rate) for each sample by comparing the RV (RV(FM sample)) of the corresponding decane peak within the sample with the RV (RV(FM calibrated)) of the decane peak within the narrow standard calibration. It was then assumed that any variation in the decane marker peak time was linearly related to the flow rate (effective flow rate) over the entire run. To facilitate the highest accuracy in RV measurement of the flow marker peak, a least-squares fitting procedure was used to fit the peak values of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation was then used to solve for the true peak position. After calibration based on the flow marker peak, the effective flow rate (relative to the narrow standard calibration) was calculated according to Equation 7. (Supported by PolymerChar GPCOne) TM The software processes the flow marker peaks. Acceptable flow rate correction ensures that the effective flow rate is within 0.5% of the nominal flow rate.
[0110] Flow rate 有效 =flow rate 标称 ×(RV(FM 校准 ) / RV(FM 样品 )) Formula 7
[0111] A systematic method for determining multi-detector offset was developed in conjunction with Balke, Mourey et al. (Mourey and Balke, Chromatography Polym. Chapter 12, (1992)) (Balke, Thitiratsakul, Lew, Cheung, Mourey, Chromatography Polym. Chapter 13, (1992)), thereby using PolymerChar GPCOne. TM The software optimizes the triple detector logarithmic (MW and IV) results from wide homopolymer polyethylene standards (Mw / Mn>3) with the narrow standard column calibration results from the narrow standard calibration curve.
[0112] Absolute molecular weight data were obtained using PolymerChar GPCOne. TM The software was obtained in a manner consistent with the following publications: Zimm (Zimm, BH, Journal of Physical Chemistry, Phys., 16, 1099 (1948)) and Kratochvil (Kratochvil, P., Classical Light Scattering from Polymer Solutions, Elsevier, Oxford, NY (1987)). The total injection concentration used for determining the molecular weight was obtained from the mass detector area and the mass detector constant, which was derived from one of suitable linear polyethylene homopolymers or polyethylene standards with known weight-average molecular weights. The calculated molecular weight (using GPCOne) TM The light scattering constants and a refractive index concentration coefficient of dn / dc of 0.104 from one or more polyethylene standards mentioned below are typically obtained. The mass detector response (IR5) and light scattering constants (using GPCOne) are also used. TM The determination should be performed using linear standards with a molecular weight exceeding approximately 50,000 g / mol. Viscometer calibration (using GPCOne) TM The determination can be performed using the method described by the manufacturer, or alternatively, by using published values of a suitable linear standard (such as Standard Reference Material (SRM) 1475a), which are available from the National Institute of Standards and Technology (NIST). The viscometer constant is calculated (using GPCOne). TM The specific viscosity area (DV) of the calibration standard and the injection mass are related to its intrinsic viscosity. It is assumed that the chromatographic concentration is low enough to eliminate the effect of the second viral coefficient (the effect of concentration on molecular weight).
[0113] Absolute weight-average molecular weight (MW) (Abs) (using GPCOne) TM The molecular weight and intrinsic viscosity responses are obtained by dividing the area of the light scattering (LS) integral chromatogram (calculated from the light scattering constant) by the mass recovered from the mass constant and the area of the mass detector (IR5). The molecular weight and intrinsic viscosity responses are obtained at the chromatographic ends where the signal-to-noise ratio decreases (using GPCOne). TM Linear extrapolation.
[0114] Absolute number average molecular weight (Mn) (Abs) ), weight average (Mw) (Abs) ) and absolute z-average molecular weight (Mz) (Abs) Calculate according to the following formula 8-10:
[0115]
[0116] Average short chain branching frequency
[0117] Calibration of the IR5 detector ratio method was performed using at least ten vinyl polymer standards (vinyl polymer homopolymers and ethylene / octene copolymers) with known short-chain branching (SCB) frequencies (the comonomer content of the reference materials was determined using 13C NMR analysis according to the techniques described in the following literature: e.g., U.S. Patent No. 5,292,845 (Kawasaki et al.) and J. C. Landall, *Review of the Chemical Physics of Polymers*, C29, 201-317, which is incorporated herein by reference). These frequencies ranged from 0 SCB / 1000 total C for homopolymers to approximately 50 SCB / 1000 total C, where total C equals the carbon in the main chain plus the carbon in the branches. Each standard had a weight-average molecular weight of 36,000 g / mol to 126,000 g / mol and a molecular weight distribution of 2.0 to 2.5, as determined by GPC.
[0118] For each of the copolymer standards, calculate the "IR5 height ratio (or "IR5") of the "area response of the IR5 methyl channel sensor minus the baseline" to the "area response of the IR5 measurement channel sensor minus the baseline". 甲基通道高度 / IR5 测量通道高度 (Including standard filters and filter wheels supplied by PolymerChar: part number IR5_FWM01 as part of the GPC-IR instrument). The linear fit of the wt% comonomer frequency relative to the "IR5 height ratio" is constructed in the form of the following formula 11:
[0119] % comonomer by weight = A0 + [A1(IR5)] 甲基通道面积 / IR5 测量通道面积 Formula 11, where the coefficients A0 = -51.08 and A1 = 250.1.
[0120] Therefore, a GPC-CC (GPC-comonomer content) plot (comonomer weight % vs. lgMW) can be obtained. If there is significant spectral overlap between the molecular weight determined at each chromatographic slice and the comonomer end-capping (methyl) group, then end-group correction of the % comonomer weight data can be performed by decapping the end-capping mechanism. The SCB frequency for each slice is lgMw. i SCB i It can be calculated using the following relationship:
[0121] For ethylene-octene copolymers
[0122] SCB i =∑ i (0.8 * comonomer weight %) i ) Formula 12
[0123] and
[0124] For ethylene-hexene copolymers
[0125]
[0126] Then the average SCB frequency over the entire distribution can be calculated.
[0127] Average SCB = ∑ i (wtGPC i *SCB i ). Formula 14
[0128] Deconvolution of GPC chromatography
[0129] The chromatogram was fitted to high molecular weight (HMW) fractions and low molecular weight (LMW) fractions using a Flory distribution, which was broadened using the following normal distribution function:
[0130] For the log M axis, 501 equally spaced Log(M) points with a spacing of 0.01 are established between 2 and 7 to represent the molecular weight range between 100 and 10,000,000, where Log is a logarithmic function to the base 10.
[0131] For any given Log(M), the population of the Flory distribution takes the form of Equation 15:
[0132]
[0133] Where Mw is the weight-average molecular weight of the Flory distribution, and M is the molecular weight point on the x-axis (10^[Log(M)]).
[0134] The Flory distribution weighted score is widened at each equidistant Log(M) exponent based on the normal distribution function, with the width denoted by Log(M),σ; and the current M exponent is denoted as Log(M),μ.
[0135]
[0136] It should be noted that the area of the distribution (dW) before and after applying the diffusion function differs. f / dLogM) is normalized to one as a function of Log(M).
[0137] The two weight fraction distributions of LMW and HMW components, or components 1 and 2, dW f 1 and dW f 2. Represented by two unique objective values Mw1 and Mw2, and total components A1 and A2. Both distributions are broadened by the same width σ. The two distributions are summed as follows:
[0138] dW f =A1 dW f1 +A2 dW f2 Formula 17
[0139] Where: A1 + A2 = 1
[0140] The weighted fraction results of the measured GPC molecular weight distribution (from conventional GPC) were interpolated along 501 logM points using a second-order polynomial. Microsoft Excel was used. TM The 2010 Solver was used to minimize the sum of squares of the residuals of the equisional spatial ranges of the interpolated molecular weight distribution and the two broadened Flory distribution components (σ1 and σ2) at 501 LogM points, weighted by their respective components A1 and A2.
[0141] The initial values for iteration of each component are as follows:
[0142] Component 1: Mw = 30,000, σ = 0.300, and A = 0.475
[0143] Component 2: Mw = 250,000, σ = 0.300, and A = 0.475
[0144] (Note that σ1 = σ2 and A1 + A2 = 1)
[0145] The boundaries between components 1 and 2 are: σ is restricted such that σ > 0.001 yields approximately 2.00 Mw / Mn, and σ < 0.450 yields approximately 5.71 Mw / Mn. Component A is restricted between 0.000 and 1.000. Mw is restricted between 2,500 and 2,000,000.
[0146] In Excel Solver TM Select the "GRG Nonlinear" engine, set the precision to 0.00001, and the convergence to 0.0001. Obtain the converged solution (in all cases shown, the solution converges within 60 iterations).
[0147] The average short-chain branching frequency distributions of the LMW and HMW components were obtained based on the dW values of the two components.f 1 and dW f The weight fraction distribution of 2 is estimated by taking the proportion of short chain branching, which is obtained from the above deconvolution and averaged for each component.
[0148] Extrusion line speed
[0149] Extrusion line speed is a critical parameter in the production of micro-irrigation drip tape because it determines the machine utilization rate per production unit. Therefore, high line speeds are beneficial for tape manufacturers. The line has been optimized in terms of die and pin geometry to allow for the highest possible line speed. To measure the maximum extrusion line speed, the line speed was incrementally increased from 200 m / min to 250 m / min, 300 m / min, 350 m / min, and 400 m / min. The line speed was recorded using extrusion parameters displayed by the control unit. The highest line speed recorded after the tape had been running stably for several minutes (e.g., 30 minutes) was considered the maximum extrusion line speed for this embodiment. Lower line speeds (where the product still runs stably) where the extrudate breaks at this speed are considered the maximum extrusion line speed.
[0150] Example
[0151] Materials used
[0152] The following materials are included in the embodiments discussed below.
[0153] FINGERPRINT TM DFDC 7525NT (unimodal ethylene / 1-hexene copolymer medium-density polyethylene) was used as Comparative Example (CE) 1 and is commercially available from The Dow Chemical Company (Midland, MI) of Midland, Michigan.
[0154] Preparation of Comparative Examples 2 to 5 and Examples 6 to 8 of the present invention
[0155] In gas-phase polymerization processes, the use of pre-catalysts including UCAT is employed. TM The catalyst system of J (commercially available from Univation Technologies, LLC, Houston, TX) and the co-catalyst triethylaluminum (TEAL) was used to produce exemplary bimodal medium-density polyethylene compositions designated as Comparative Examples 2, 3, 4, and 5, and Examples 6, 7, and 8 of the present invention. TMThe J catalyst was partially activated by contacting a suitable amount of a 50% mineral oil solution of tri-n-hexyl aluminum (TNHA) at room temperature. The catalyst slurry was added to a mixing vessel. While stirring, the 50% mineral oil solution of TNHA was added at a ratio of 0.17 moles of TNHA to the moles of residual THF in the catalyst, and stirring was continued for at least 1 hour before use. Ethylene (C2) and optionally 1-hexene (C6) were polymerized in two fluidized bed reactors. Each polymerization was carried out continuously after reaching equilibrium, under the corresponding conditions, as shown in Tables 1A and 1B below. In the first reactor, polymerization was initiated by continuously feeding the catalyst and co-catalyst (trialkylaluminum, specifically triethylaluminum or TEAL) along with ethylene, hydrogen, and 1-hexene into a fluidized bed of polyethylene particles. The resulting polymer, mixed with the activated catalyst, was withdrawn from the first reactor and transferred to the second reactor using gas from the second reactor as a transfer medium. The second reactor also contained a fluidized bed of polyethylene particles. Ethylene, hydrogen, and hexene are introduced into a second reactor, where these gases contact the polymer and catalyst from the first reactor. Inert gases, nitrogen, and isopentane constitute the residual pressure in both the first and second reactors. A co-catalyst (TEAL) is introduced again into the second reactor. The final product blend is continuously removed. Table 1A lists the polymerization conditions for CE 2, CE 3, CE 4, and CE 5. Table 1B lists the polymerization conditions for IE 6, IE 7, and IE 8.
[0156] The product was mixed with additives (500 ppm calcium stearate, 1300 ppm Irganox). TM 1010 and 1300ppm Irgafos TM 168) combined and fed into a continuous mixer (Kobe Steel, Ltd. LCM-100 continuous mixer), which is closely coupled to a gear pump and equipped with a melt filter and an underwater granulation system.
[0157] The characteristics of comparative examples and embodiments of the present invention are provided in Tables 2A and 2B below. In Tables 2A and 2B, "HMW" refers to the high molecular weight polyethylene component and "LMW" refers to the low molecular weight polyethylene component.
[0158] Micro-irrigation drip tapes were formed from a bimodal medium-density polyethylene composition using a Mailefer International Oy Extruder MXC 60-36D with a diameter of 60 mm and a length / diameter (L / D) ratio of 36. The extruder employed a suitable temperature distribution to achieve a melt temperature of 240°C. The extruder was equipped with a 34.5 mm diameter annular die and 32.5 mm diameter pins (1 mm gap). The inner diameter of each micro-irrigation drip tape was 16 mm. The thickness of the annular wall was adjusted by varying the extruder's rotational speed (rpm) and linear speed. Each micro-irrigation drip tape was then calibrated and water-cooled. During tape cooling, just after exiting the extruder, the emitter was placed on the inner surface of the annular wall. A perforation was made in-line along this line at the emitter in the annular wall before passing through a mechanical drilling device or laser-cutting the wound tape. Maximum extrusion linear speeds are provided in Tables 2A and 2B.
[0159] High-speed tape processing is a key characteristic and requirement for the efficient production of drip irrigation tape. Processing tests were conducted on the Merafell test line PIL032-miniFT. This line reflects an entry-level model for the drip irrigation market that is readily available from Merafell upon ordering. The line has been modified with an RCI 32 type tape traction device, enabling higher line speeds of 300 m / min to 400 m / min for development purposes. For calibration, a BRI 32-16m type Merafell vacuum chamber with a dryer was used.
[0160] Table 1A - Polymerization conditions of Comparative Examples 2 to 5
[0161]
[0162] Table 1B - Polymerization conditions of Examples 6 to 8 of the present invention
[0163]
[0164]
[0165] Table 2A - Characteristics of Comparative Examples 1 to 5
[0166]
[0167] 1 Comparative Example 1 is a single-peak resin, and therefore these parameters are not applicable.
[0168] 2 The low molecular weight density is the calculated LMW density using formula A:
[0169]
[0170] Table 2B - Characteristics of Embodiments 6 to 8 of the present invention
[0171]
[0172]
[0173] 1 The low molecular weight density is the calculated LMW density using the following formula A:
[0174]
[0175] As can be seen from Tables 1A and 1B, for embodiments of the present invention, a higher amount of comonomer is added to the second reactor for producing the LMW polyethylene component. This, in turn, results in a lower LMW polyethylene component density and a higher average short-chain branching frequency in the LMW polyethylene component, as can be seen from Tables 2A and 2B. Unbound by any theory, these properties, along with cross G' = G”, contribute to processability advantages by altering the crystallization rate (as measured by the isothermal crystallization half-life at Tc+5°C). As can be seen from Tables 2A and 2B, the embodiments of the present invention exhibit a significantly longer isothermal crystallization half-life at Tc+5°C compared to the comparative embodiments. Furthermore, the embodiments of the present invention satisfy the formula: [43.0 - cross G' = G”] + 1230 * (0.9731 - calculated LMW density) - 5.5745 ≥ 0 (Formula 2) and the formula [43 - cross G' = G”] - (54.5 / LMW SCB)+16.9≥0 (Formula 3). Embodiments 6, 7, and 8 of this invention provide values of 5.24, 7.85, and 4.91 for the left side of Formula 2, respectively. Meanwhile, Comparative Embodiments 2, 3, 4, and 5 provide values of -5.25, -23.23, -14.95, and -4.82 for the left side of Formula 2, respectively. Embodiments 6, 7, and 8 of this invention provide values of 7.82, 6.39, and 7.71 for the left side of Formula 3, respectively. Meanwhile, Comparative Embodiments 2, 3, 4, and 5 provide values of -6.64, -30.82, -... Values of 18.43 and -6.59. The embodiments of the invention exhibit better processability and a longer crystallization rate, resulting in less cracking and pinholes during processing. Embodiment 6 of the invention can be extruded at a linear velocity of 350 m / min, and Embodiments 7 and 8 of the invention can be extruded at a linear velocity of 400 m / min. Comparative embodiments cannot be extruded at these higher speeds. Without being bound by any theory, the combination of characteristics of the embodiments of the invention (including a specific cross G' = G (which indicates melt elasticity), lower calculated low molecular density, higher average SCB frequency, and a longer isothermal crystallization half-life at Tc+5°C) allows for extrusion of the composition at higher speeds compared to comparative embodiments.
[0176] Unless expressly excluded or otherwise limited, every document cited herein (if any), including any cross-referenced or related patent or application and any patent application or patent claiming priority or benefit thereof, is incorporated herein by reference in its entirety. No reference to any document acknowledges it as prior art to any invention disclosed or claimed herein, or as teaching, indicating, or disclosing any such invention, alone or in combination with any other referenced document. Furthermore, in the event of any conflict between the meaning or definition of any term in this document and the meaning or definition of the same term in any document incorporated by reference, the meaning or definition given to the term in this document shall prevail.
[0177] While specific embodiments of the invention have been described and illustrated, it will be apparent to those skilled in the art that many other changes and modifications can be made without departing from the spirit and scope of the invention. Therefore, it is intended that all such changes and modifications falling within the scope of the invention be covered in the appended claims.
Claims
1. A bimodal medium-density polyethylene composition comprising: (i) a high molecular weight (HMW) polyethylene component comprising an ethylene / α-olefin copolymer; and (ii) a low molecular weight (LMW) polyethylene component comprising an ethylene / α-olefin copolymer; the bimodal medium-density polyethylene composition having the following properties: (a) 0.937 g / cm³ 3 Up to 0.949 g / cm 3 The density; (b) High-load melt index I from 12 g / 10 min to 30 g / 10 min 21 ; (c) Isothermal crystallization half-life at Tc+5℃ greater than 350 seconds; (d) Elongation at break greater than 3.6; (e) Crossover G'=G'' at 30kPa to 45kPa; and (f) The calculated LMW density of the low molecular weight LMW polyethylene component is less than or equal to 0.974 g / cm³. 3 ;and The cross G'=G'' and the calculated LMW density satisfy the following formula:
2. A bimodal medium-density polyethylene composition comprising: (i) a high molecular weight (HMW) polyethylene component comprising an ethylene / α-olefin copolymer; and (ii) a low molecular weight (LMW) polyethylene component comprising an ethylene / α-olefin copolymer; the bimodal medium-density polyethylene composition having the following properties: (a) 0.937 g / cm³ 3 Up to 0.949 g / cm 3 The density; (b) High-load melt index I from 12 g / 10 min to 30 g / 10 min 21 ; (c) Isothermal crystallization half-life at Tc+5℃ greater than 360 seconds; (d) Elongation at break greater than 3.6; (e) Crossing at 30 kPa to 45 kPa: G' = G''; (f) Average short-chain branched SCB frequency from 2.4 to 10.0 short-chain branched SCBs per 1000 carbons; and (g) The average short-chain branched SCB frequency of the low molecular weight LMW polyethylene component of 2.0 to 8.7 short-chain branched SCBs / 1000 carbons; and The cross G'=G'' and the average short-chain branched SCB frequency of the low molecular weight LMW polyethylene component satisfy the following formula:
3. The bimodal medium-density polyethylene composition according to claim 1 or 2, wherein the high molecular weight (HMW) polyethylene component has a high-load melt index I of 0.5 g / 10 min to 0.9 g / 10 min. 21 And / or has 0.914 g / cm 3 Up to 0.935 g / cm 3 The density.
4. The bimodal medium-density polyethylene composition according to claim 1 or 2, wherein the high molecular weight (HMW) polyethylene component is present in an amount of 48% to 60% by weight based on the total weight of the bimodal medium-density polyethylene composition.
5. The bimodal medium-density polyethylene composition according to claim 1 or 2, wherein the bimodal medium-density polyethylene composition has a molecular weight distribution of 12 to 30 Mw / Mn.
6. The bimodal medium-density polyethylene composition according to claim 1 or 2, wherein the bimodal medium-density polyethylene composition has a notched constant tensile load failure time of more than 100 hours at 30% yield stress as measured according to ASTM D5397.
7. The bimodal medium-density polyethylene composition according to claim 1 or 2, wherein the high molecular weight (HMW) polyethylene component has an average short-chain branched SCB frequency, and the ratio of the average short-chain branched SCB frequency of the low molecular weight (LMW) polyethylene component to the average short-chain branched SCB frequency of the high molecular weight (HMW) polyethylene component is greater than 0.
70.
8. A micro-irrigation drip tape comprising a bimodal medium-density polyethylene composition according to any one of claims 1-7.
Citation Information
Patent Citations
Impregnated polymerization catalyst, process for preparing, and use for ethylene copolymerization
US4302565A
Preparation of low-density ethylene copolymers in fluid bed reactor
US4482687A
Ethylene polymerization using supported vanadium catalyst
US4508842A
Process for polymerizing olefins and polymerization catalyst therefor
US4990479A
Olefin polymerization catalyst
US5122494A