Antibacterial ceramic marble brick and preparation method thereof

By introducing silver-loaded nano-titanium dioxide into the glaze layer and wax film layer of ceramic marble tiles, the problems of antibacterial agent loss and texture impact in the existing technology are solved, and long-lasting antibacterial effects and ideal texture effects are achieved.

CN118652138BActive Publication Date: 2024-10-29GUANGDONG NEWPEARL CERAMIC GRP CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411105155.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-29
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The antibacterial agent of existing ceramic marble tiles is easily lost during the firing process, resulting in an antibacterial effect that is not durable and may affect the texture and texture of the product.

Method used

Silver-loaded nano-titanium dioxide is introduced into the top glaze layer and wax film layer to achieve long-lasting and durable antibacterial effects through the synergy of specific chemical compositions while maintaining the marble texture and apparent texture.

Benefits of technology

It achieves the long-lasting and durable antibacterial effect of the product, and maintains the ideal marble texture and apparent texture effect. The glaze is clear and has a high sense of natural luxury.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652138B_ABST
    Figure CN118652138B_ABST
Patent Text Reader

Abstract

The invention discloses an antibacterial ceramic marble brick and a preparation method thereof, belonging to the field of ceramics. The invention is based on introducing a specific content of silver-loaded nano-titanium dioxide into the raw materials for preparing the surface glaze layer and the surface wax film. In the fired product, under the synergistic effect of the surface glaze layer and the surface wax film layer with a specific chemical composition, not only a long-lasting and durable antibacterial effect can be achieved, but also an ideal marble texture and apparent texture effect can be presented, with a clear glaze surface and a high sense of natural luxury.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramics, and in particular to an antibacterial ceramic marble brick and a preparation method thereof. Background Art

[0002] The existing preparation process of ceramic marble tiles generally involves first printing a marble texture pattern on the surface glaze layer of the body, then applying a protective glaze and a dry granular glaze in sequence, and finally firing the product. The resulting product has a realistic marble simulation texture and apparent texture.

[0003] However, as the frequency of application of ceramic marble tiles in the kitchen and bathroom fields gradually increases, the antibacterial ability of the products also needs to be gradually improved. Existing ceramic tiles achieve antibacterial effects by adding some antibacterial agents with antibacterial activity or catalytic antibacterial activity to the raw materials for preparation, but these antibacterial agents are extremely easy to be lost or transformed into crystal forms during the firing process of the product, and thus weaken or even fail to work, and the antibacterial effect is not durable, and it may also affect the marble simulation texture and apparent texture effect of the ceramic tiles. Summary of the invention

[0004] Based on the defects of the prior art, the purpose of the present invention is to provide an antibacterial ceramic marble tile, which is based on the introduction of a specific content of silver-loaded nano-titanium dioxide into the raw materials for preparing the surface glaze layer and the surface wax film. In the fired product, under the synergistic effect of the surface glaze layer and the surface wax film layer with a specific chemical composition, not only can a long-lasting antibacterial effect be achieved, but also an ideal marble texture and apparent texture effect can be presented, with a clear glaze surface and a high sense of natural luxury.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] An antibacterial ceramic marble brick comprises a body layer, a glaze layer, a dry particle layer and a wax film layer which are adjacent to each other in sequence, wherein the raw material for preparing the glaze layer comprises silver-loaded nano-titanium dioxide;

[0007] The glaze layer includes the following chemical components in percentage by weight:

[0008] SiO250~60%, Al2O317~23%, ZrO24~7%, K2O 2.5~4%, Na2O 2~5%, MgO 0.3~2%, CaO2~6%, ZnO 2~6%, BaO 0.5~1.5%, TiO20.42~0.8% and Ag0.04~0.12%; the Ag is Ag + Mass content meter;

[0009] The wax film layer comprises silver-loaded nano-titanium dioxide, and the mass percentage of the silver-loaded nano-titanium dioxide in the wax film layer is 2-5%.

[0010] Silver salts or their oxides are common antibacterial active inorganic substances. In addition to the ceramic field, they are also common antibacterial agents in the medical field. They have strong inhibitory and killing effects on bacteria that are easily gathered in the kitchen and bathroom, such as Escherichia coli and Staphylococcus aureus. On the other hand, titanium dioxide can form a powerful photocatalyst under ultraviolet light. When this component is in ceramic tiles, ultraviolet rays will convert light into heat energy when it hits the surface of the ceramic tiles and release it outward, killing bacteria attached to the ceramic tiles and achieving self-cleaning. In theory, it is also a very ideal antibacterial ingredient. However, in actual research and development, the inventors found that when these two components are introduced into the glaze raw materials of the ceramic tile in the form of raw materials for preparation, after firing, on the one hand, these two antibacterial agents will affect the chemical composition of the glaze, which may affect the clarity of the glaze and even the texture and texture effect of the final product; on the other hand, other raw materials used in the preparation of the glaze will also affect the function of the antibacterial agent. In addition to uniformity, the chemical composition will also affect the refraction effect of ultraviolet rays on the glaze, and even the antibacterial components will be lost during the firing process, resulting in a decrease in the content and stability of the antibacterial agent, thereby affecting its antibacterial efficacy. If the antibacterial agent is simply covered on the outermost layer of the ceramic tile in the form of a coating, since the outermost layer of the ceramic marble tile is a dry particle layer, the uneven load matrix will not only lead to unsatisfactory uniformity and tightness of the coating, but also significantly reduce the antibacterial effect after washing, and the coating layer will also affect the appearance and texture of the product.

[0011] To this end, the inventors used silver-loaded nano-titanium dioxide as the raw material for preparing the glaze layer of ceramic marble tiles. The material has good stability. At the same time, the silver-loaded nano-titanium dioxide can prevent the recombination of electron-hole pairs and promote the effective separation of electron-hole pairs, thereby making the overall antibacterial performance more stable. At the same time, based on the specific chemical composition, other components of the glaze layer will not inhibit the antibacterial properties of the antibacterial ingredients, and the antibacterial ingredients will not affect the glaze clarity and glaze effect of the glaze layer, and the texture and texture effect of the product will not be affected. However, only the antibacterial glaze layer is not enough to ensure the strong antibacterial and durable antibacterial properties of the product, and the ultraviolet rays cannot exert the strongest bactericidal effect when entering the glaze layer after being refracted by the dry particle layer. Therefore, the inventor further set a wax film layer containing silver-loaded nano-titanium dioxide particles outside the dry particle layer. Due to the nano size of the particles, they can be easily filled into the tiny pores of the dry particle layer, which not only inhibits the attachment of bacteria, but also can exert the photocatalytic effect of titanium dioxide to a greater extent. At the same time, the wax layer can also maintain the unique marble texture effect of the product with a certain matte effect, avoiding texture distortion or texture changes caused by the setting of the external layer. However, as mentioned above, silver-loaded nano-titanium dioxide has a great influence on the texture and appearance of the product, so the content of this component in the wax film layer cannot be too much.

[0012] Preferably, the raw materials for preparing the surface glaze layer include the following components in parts by weight:

[0013] 5-12 parts of air knife soil, 15-25 parts of potassium feldspar, 20-30 parts of sodium feldspar, 8-15 parts of nepheline, 3-5 parts of wollastonite, 3-6 parts of calcined zinc oxide, 8-15 parts of zirconium silicate, 5-10 parts of calcined aluminum oxide, 5-10 parts of frit, 10-15 parts of quartz powder and 0.3-0.8 parts of silver-loaded nano-titanium dioxide;

[0014] The frit comprises the following components in parts by weight: 10-15 parts of kaolin, 15-20 parts of potassium feldspar, 20-30 parts of sodium feldspar, 10-15 parts of barium carbonate, 5-10 parts of dolomite, 5-10 parts of calcite, 1-3 parts of zinc oxide, 6-10 parts of aluminum oxide and 10-15 parts of quartz.

[0015] More preferably, in the raw materials for preparing the surface glaze layer, the weight portion of silver-loaded nano-titanium dioxide is 0.5-0.6 parts.

[0016] Although the amount of silver-loaded nano-titanium dioxide added in the preparation of the glaze layer is small, based on its physical refractive properties and chemical composition, when the amount of addition changes, the texture and apparent texture effect of the product will also be affected. After optimization, when silver-loaded nano-titanium dioxide is introduced in the above-mentioned addition ratio during the preparation process, the texture of the product and the apparent texture effect of simulated marble are the best.

[0017] More preferably, the glaze layer comprises the following chemical components in percentage by weight:

[0018] SiO2 50~60%, Al2O3 20~23%, ZrO2 5~6%, K2O 2.5~3%, Na2O 3~4%, MgO 0.3~0.5%, CaO2~3%, ZnO5~6%, BaO 0.6~1.5%, TiO2 0.4~0.9% and Ag 0.04~0.1%.

[0019] It should be noted that the chemical composition of the glaze layer of the present invention also includes trace impurities. It is well known to those skilled in the art that the impurities do not actually affect the performance of the product, so they are not listed one by one.

[0020] More preferably, in the chemical composition of the glaze layer, the mass percentage of TiO2 is 0.58-0.65%, and the mass percentage of Ag is 0.06-0.08%.

[0021] Preferably, the particle size of the silver-loaded nano-titanium dioxide is 10-100 nm.

[0022] More preferably, the mass percentage of nano-titanium dioxide in the silver-loaded nano-titanium dioxide is 96-99%.

[0023] More preferably, it is 97~98%.

[0024] Nano-titanium dioxide is a carrier of silver, and its content not only affects the uniformity of silver loading, but also affects the photocatalytic effect of the overall silver-loaded nano-titanium dioxide. The inventors have found that when the content is within the above range, the product has the best silver loading uniformity and can achieve the best photocatalytic effect, thereby obtaining better antibacterial properties.

[0025] More preferably, the preparation method of the silver-loaded nano-titanium dioxide is:

[0026] (1) adding 0.03-0.05 mol of tetrabutyl titanate into water and stirring, then adding alkali solution and mixing until the pH value of the resulting mixed solution reaches 10, thereby obtaining a titanium dioxide solution, wherein the titanium element concentration in the titanium dioxide solution is 0.4-0.6 mol / L, then performing a hydrolysis precipitation reaction at 120-130° C., filtering the precipitate, and washing to obtain hydrated titanium dioxide;

[0027] (2) Adding hydrated titanium dioxide to the silver nitrate solution, impregnating and stirring the mixture, drying the obtained solid, and then keeping the mixture at 450-500° C. for 0.5-1.5 h, and crushing the solid to obtain the silver-loaded nano-titanium dioxide.

[0028] It should be noted that the preparation method of silver-loaded nano-titanium dioxide of the present invention is not limited to the above scheme. For example, technicians in this field can also choose other methods such as solid phase method or spray method to carry out silver loading treatment on nano-titanium dioxide according to needs or actual conditions, as long as it is further applied in the preparation of antibacterial ceramic marble tiles to obtain similar effects to the products prepared by the above scheme.

[0029] More preferably, the concentration of the silver nitrate solution is 0.05-0.5 mol / L, and the ratio of the volume of the silver nitrate solution to the mass of hydrated titanium dioxide is (5-15) mL:1 g.

[0030] Preferably, the dry particle layer comprises dry particle particles, and the dry particle particles comprise the following chemical components in percentage by weight:

[0031] SiO2 45~55%, Al2O3 15~20%, SrO4~7%, K2O2~5%, Na2O2~5%, MgO1~3%, CaO3~6%, ZnO3~6% and BaO 8~11%.

[0032] More preferably, the dry granules include the following raw materials in parts by weight:

[0033] 25-40 parts of potassium feldspar, 10-25 parts of sodium feldspar, 5-10 parts of air knife clay, 5-15 parts of barium carbonate, 5-15 parts of calcite, 3-10 parts of zinc oxide, 4-10 parts of strontium carbonate, 2-5 parts of quartz and 2-5 parts of aluminum oxide.

[0034] More preferably, the method for preparing the dry granules comprises the following steps:

[0035] The prepared raw materials are mixed and melted at 1400-1550° C., cooled, and crushed to obtain the dry granular particles.

[0036] More preferably, the mesh size of the dry granules is 250-300 meshes.

[0037] Preferably, the green body layer comprises the following raw materials in parts by weight:

[0038] 20-25 parts of potassium and sodium sand, 15-25 parts of ball clay, 3-10 parts of bentonite, 5-10 parts of sodium sand, 1-10 parts of talc, 10-15 parts of kaolin, 20-25 parts of potassium and sodium aqueous abrasive, 1-5 parts of pyrophyllite, 0.5-1 parts of debonding agent, 0.1-0.5 parts of sodium tripolyphosphate, and 0.1-0.5 parts of water glass.

[0039] Preferably, the wax film layer comprises the following components in percentage by mass:

[0040] Carrier wax 95~98% and silver-loaded nano-titanium dioxide 2~5%.

[0041] More preferably, the carrier wax is a silicon dioxide solution.

[0042] Another object of the present invention is to provide a method for preparing the antibacterial ceramic marble brick, comprising the following steps:

[0043] The green body layer is pressed and dried to a moisture content of ≤0.3%;

[0044] Printing a marble effect pattern on the body layer;

[0045] Arranging a glaze layer on the body layer;

[0046] Printing patterns and digital glaze ink on the surface glaze layer;

[0047] A dry particle layer is provided on the pattern and digital glaze ink to prepare a blank to be fired;

[0048] The blank to be fired is fired, and then a wax film layer is provided through polishing and edge grinding to obtain the antibacterial ceramic marble tile.

[0049] In addition to the use of special glaze layers and wax layers, the technical solution of the present invention also creatively pre-prints the marble effect pattern on the body layer, then sets the glaze layer, and further prints the pattern and digital glaze ink on the glaze layer. This approach can effectively improve the texture simulation of the product without destroying the texture of the glaze.

[0050] Preferably, the glaze layer is provided by spraying glaze slurry on the body layer.

[0051] More preferably, the glaze slurry comprises raw materials for preparing the glaze layer and water, the particle size of the raw materials for preparing the glaze layer is 50-80 μm, and the mass percentage of water in the glaze slurry is 28-32%.

[0052] Preferably, the glaze amount of the surface glaze layer is 250-300 g / m 2 The dry particle amount of the dry particle layer is 200-300 g / m 2 .

[0053] Preferably, the dry particle layer is provided by spraying dry particle slurry on the pattern and the digital glaze ink.

[0054] More preferably, the dry particle slurry comprises dry particle particles and a suspending agent, and the suspending agent comprises the following components in parts by weight:

[0055] 2-4 parts of dispersant, 2-4 parts of thickener, 1-2 parts of anti-precipitation agent, 0.5-1 parts of defoamer, 90-95 parts of water, and the mass percentage of the suspending agent in the dry particle slurry is 70-80%.

[0056] The beneficial effect of the present invention is that the present invention provides an antibacterial ceramic marble tile, which is based on introducing a specific content of silver-loaded nano-titanium dioxide into the raw materials for preparing the surface glaze layer and the surface wax film. In the fired product, under the synergistic effect of the surface glaze layer and the surface wax film layer with a specific chemical composition, not only can a long-lasting and durable antibacterial effect be achieved, but also an ideal marble texture and apparent texture effect can be presented, with a clear glaze surface and a high sense of natural luxury. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 This is a schematic diagram of the ceramic marble tile described in Example 1 of the present invention.

[0058] Figure 2 This is a schematic diagram of the ceramic marble brick described in Comparative Example 6 of the present invention.

[0059] Figure 3 This is a schematic diagram of the ceramic marble brick described in Comparative Example 1 of the present invention.

[0060] Figure 4 This is a schematic diagram of the ceramic marble brick described in Comparative Example 2 of the present invention.

[0061] Figure 5 This is an elemental analysis test diagram of the glaze composition described in Example 1 of the present invention after firing.

[0062] Figure 6 This is the EDS spectrum of the glaze composition described in Example 1 of the present invention after firing. DETAILED DESCRIPTION

[0063] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.

[0064] Example 1

[0065] An embodiment of an antibacterial ceramic marble tile and a preparation method thereof according to the present invention comprises the following preparation steps:

[0066] (1) Pressing the green body layer and drying it to a moisture content of ≤0.3% and a strength of ≥1.8MPa;

[0067] The green body layer comprises the following raw materials in parts by weight:

[0068] 23 parts of potassium sodium sand, 21 parts of ball clay, 6 parts of bentonite, 6 parts of sodium sand, 4 parts of talc, 12 parts of kaolin, 23 parts of potassium sodium water abrasive, 4 parts of pyrophyllite, 0.6 parts of degumming agent, 0.2 parts of sodium tripolyphosphate, and 0.35 parts of water glass;

[0069] The green body layer is obtained by mixing various raw materials, drying at 115° C., and pressing for 40 minutes;

[0070] (2) Printing a marble effect pattern on the green body layer;

[0071] The effect pattern is obtained by scanning the marble with a scanner to obtain a preliminary appearance effect pattern, then the color separation process is performed to superimpose the color arrangement channel, and finally the marble effect pattern is obtained by manual drawing in the range of 0.3~0.6mm and 35~50% grayscale;

[0072] (3) Arranging a glaze layer on the body layer;

[0073] The glaze layer is formed by spraying a glaze slurry onto the green body layer after the effect pattern is printed, wherein the slurry comprises 70 wt % of the glaze layer preparation raw material with an average particle size of 65 μm and 30 wt % of water, and the slurry is sprayed at a flow rate of 33-38 s / 100 mL;

[0074] The raw materials for preparing the surface glaze layer include the following components in parts by weight: 8 parts of air knife soil, 20 parts of potassium feldspar, 22 parts of sodium feldspar, 8 parts of nepheline powder, 4 parts of wollastonite, 5 parts of calcined zinc oxide, 8 parts of zirconium silicate, 0.5 parts of silver-loaded nano-titanium dioxide, 10 parts of quartz powder, 5 parts of frit, and 10 parts of calcined alumina. The raw materials are mixed and then crushed and ground.

[0075] The frit includes the following components in parts by weight: 12 parts of kaolin, 16 parts of potassium feldspar, 22 parts of sodium feldspar, 13 parts of barium carbonate, 8 parts of dolomite, 6 parts of calcite, 2 parts of zinc oxide, 8 parts of aluminum oxide and 13 parts of quartz.

[0076] The glaze amount of the surface glaze layer is 250g / m 2 ;

[0077] (4) Print patterns and digital glaze ink on the top glaze layer, with the grayscale set to 15-40%;

[0078] (5) A dry particle layer is provided on the pattern and digital glaze ink to prepare the blank for firing;

[0079] The dry particle layer is achieved by spraying dry particle slurry onto the pattern and digital glaze ink, wherein the dry particle slurry comprises 25 parts of dry particles and 75 parts of suspending agent, and the mass ratio of the two is 1:3;

[0080] The suspending agent comprises the following components in parts by weight: 4 parts of suspending agent magnesium aluminum silicate, 2 parts of thickening agent cellulose ether, 2 parts of anti-precipitation agent fumed silica, 0.5 parts of organosilicon defoaming agent and 91.5 parts of water;

[0081] The mesh size of the dry granules is 300 mesh;

[0082] The raw materials for preparing the dry granules include the following materials in parts by weight:

[0083] 28 parts of potassium feldspar, 18 parts of sodium feldspar, 8 parts of air knife clay, 10 parts of barium carbonate, 11 parts of calcite, 7 parts of zinc oxide, 10 parts of strontium carbonate, 4 parts of quartz and 4 parts of aluminum oxide;

[0084] The dry granules are obtained by mixing various raw materials, melting them at 1500°C, cooling them, and crushing them;

[0085] The chemical composition of the dry granules is:

[0086] SiO248.53%, Al2O316.34%, SrO4.12%, K2O3.44%, Na2O2.08%, MgO1.12%, CaO5.83%, ZnO4.15%, BaO10.56% and the remainder impurities and loss on ignition;

[0087] The dry particle amount of the dry particle layer is 250g / m 2 ;

[0088] (6) firing the to-be-fired blank at 1200° C., and then providing a wax film layer by polishing and grinding the edges, thereby obtaining the antibacterial ceramic marble brick;

[0089] The specific steps of setting the wax film layer are: spreading wax water on the dry particle layer, and then using a polishing grinding head to perform a grinding process, the wax water is obtained by mixing and stirring 3 parts of silver-loaded nano-titanium dioxide and 97 parts of carrier wax silica solution gel (oily matte silica sol wax water YH150BY) in a mass ratio of 3:97, and the thickness of the wax film layer is 2um;

[0090] The silver-loaded nano-titanium dioxide is a homemade product, and the preparation method is as follows:

[0091] (a) 0.04 mol of tetrabutyl titanate was added to 25 ml of deionized water and stirred for 30 min, and then 1 M sodium hydroxide was slowly added dropwise to the reaction system and stirred until the pH value reached 10, and stirring was continued until a titanium dioxide solution was formed. In this way, the titanium concentration in the obtained mixed solution was 0.5 mol / L, and then a hydrolysis precipitation reaction was carried out at 120-130 ° C, and the precipitate was filtered and washed to obtain hydrated titanium dioxide;

[0092] (2) Add 2 g of hydrated titanium dioxide to a 20 mL volume solution with a concentration of 0.1 mol / L silver nitrate solution, mix, immerse and stir, dry at 80° C., then keep warm at 480° C. for 1 hour, and crush to an average particle size of 50 nm to obtain the silver-loaded nano-titanium dioxide, wherein the mass content of nano-titanium dioxide in the silver-loaded nano-titanium dioxide is 98%.

[0093] The chemical composition of the glaze layer is shown in Table 1.

[0094] Example 2

[0095] An embodiment of an antibacterial ceramic marble tile and a preparation method thereof described in the present invention is different from Example 1 only in that the raw materials for preparing the surface glaze layer include the following components in parts by weight: 12 parts of air knife clay, 15 parts of potassium feldspar, 22 parts of sodium feldspar, 8 parts of nepheline powder, 3 parts of wollastonite, 5 parts of calcined zinc oxide, 10 parts of zirconium silicate, 0.3 parts of silver-loaded nano-titanium dioxide, 12 parts of quartz powder, 8 parts of frit, and 5 parts of 325 mesh calcined alumina. The chemical composition of the surface glaze layer is shown in Table 1.

[0096] Example 3

[0097] An embodiment of an antibacterial ceramic marble tile and a preparation method thereof described in the present invention is different from Embodiment 1 only in that the weight portion of silver-loaded nano-titanium dioxide in the preparation raw materials of the surface glaze layer is adjusted to 0.8 parts, and the chemical composition of the surface glaze layer is shown in Table 1.

[0098] Example 4

[0099] An embodiment of an antibacterial ceramic marble tile and a preparation method thereof described in the present invention is different from Example 1 only in that the weight portion of silver-loaded nano-titanium dioxide in the preparation raw materials of the surface glaze layer is adjusted to 0.6 parts, and the chemical composition of the surface glaze layer is shown in Table 1.

[0100] Example 5

[0101] An embodiment of an antibacterial ceramic marble tile and a preparation method thereof described in the present invention is different from Example 1 only in that the weight portion of silver-loaded nano-titanium dioxide in the preparation raw materials of the surface glaze layer is adjusted to 0.3 parts, and the chemical composition of the surface glaze layer is shown in Table 1.

[0102] Example 6

[0103] An embodiment of the antibacterial ceramic marble brick and the preparation method thereof described in the present invention is different from Embodiment 1 only in that the wax water is obtained by mixing and stirring silver-loaded nano-titanium dioxide and carrier wax in a mass ratio of 5:95.

[0104] Example 7

[0105] An embodiment of the antibacterial ceramic marble brick and the preparation method thereof described in the present invention is different from Embodiment 1 only in that the wax water is obtained by mixing and stirring silver-loaded nano-titanium dioxide and carrier wax in a mass ratio of 2:98.

[0106] Example 8

[0107] An embodiment of the antibacterial ceramic marble brick and the preparation method thereof of the present invention is different from the embodiment 1 only in that:

[0108] The silver-loaded nano-titanium dioxide is a homemade product, and the preparation method is as follows:

[0109] (a) 0.04 mol of tetrabutyl titanate was added to 25 ml of deionized water and stirred for 30 min, and then 1 M sodium hydroxide was slowly added dropwise to the reaction system and stirred until the pH value reached 10, and stirring was continued until a titanium dioxide solution was formed. In this way, the titanium concentration in the obtained mixed solution was 0.5 mol / L, and then a hydrolysis precipitation reaction was carried out at 120-130 ° C, and the precipitate was filtered and washed to obtain hydrated titanium dioxide;

[0110] (2) Add 1.5 g of hydrated titanium dioxide to a 20 mL volume solution with a concentration of 0.1 mol / L silver nitrate solution, mix, immerse and stir, dry at 80° C., then keep warm at 480° C. for 1 hour, and crush to an average particle size of 50 nm to obtain the silver-loaded nano-titanium dioxide, wherein the mass content of nano-titanium dioxide in the silver-loaded nano-titanium dioxide is 97%.

[0111] Example 9

[0112] An embodiment of the antibacterial ceramic marble brick and the preparation method thereof of the present invention is different from the embodiment 1 only in that:

[0113] The silver-loaded nano-titanium dioxide is a homemade product, and the preparation method is as follows:

[0114] (a) 0.04 mol of tetrabutyl titanate was added to 25 ml of deionized water and stirred for 30 min, and then 1 M sodium hydroxide was slowly added dropwise to the reaction system and stirred until the pH value reached 10, and stirring was continued until a titanium dioxide solution was formed. In this way, the titanium concentration in the obtained mixed solution was 0.5 mol / L, and then a hydrolysis precipitation reaction was carried out at 120-130 ° C, and the precipitate was filtered and washed to obtain hydrated titanium dioxide;

[0115] (2) Add 2.5 g of hydrated titanium dioxide to a 20 mL volume solution with a concentration of 0.1 mol / L silver nitrate solution, mix, immerse and stir, dry at 80° C., then keep warm at 480° C. for 1 hour, and crush to an average particle size of 50 nm to obtain the silver-loaded nano-titanium dioxide, wherein the mass content of nano-titanium dioxide in the silver-loaded nano-titanium dioxide is 99%.

[0116] Example 10

[0117] An embodiment of the antibacterial ceramic marble brick and the preparation method thereof of the present invention is different from the embodiment 1 only in that:

[0118] The silver-loaded nano-titanium dioxide is a homemade product, and the preparation method is as follows:

[0119] (a) 0.04 mol of tetrabutyl titanate was added to 25 ml of deionized water and stirred for 30 min, and then 1 M sodium hydroxide was slowly added dropwise to the reaction system and stirred until the pH value reached 10, and the stirring was continued until a titanium dioxide solution was formed. In this way, the titanium concentration in the obtained mixed solution was 0.5 mol / L, and then a hydrolysis precipitation reaction was carried out at 120-130 ° C, and the precipitate was filtered and washed to obtain hydrated titanium dioxide;

[0120] (2) Add 1 g of hydrated titanium dioxide to a 20 mL volume solution with a concentration of 0.1 mol / L silver nitrate solution, mix, immerse and stir, dry at 80° C., then keep warm at 480° C. for 1 hour, and crush to an average particle size of 50 nm to obtain the silver-loaded nano-titanium dioxide, wherein the mass content of nano-titanium dioxide in the silver-loaded nano-titanium dioxide is 96%.

[0121] Comparative Example 1

[0122] An antibacterial ceramic marble tile and a preparation method thereof, which differs from Example 1 only in that the weight portion of silver-loaded nano-titanium dioxide in the preparation raw materials of the surface glaze layer is adjusted to 0 part, and the chemical composition of the surface glaze layer is shown in Table 1.

[0123] Comparative Example 2

[0124] An antibacterial ceramic marble tile and a preparation method thereof, the only difference from Example 1 is that the weight portion of silver-loaded nano-titanium dioxide in the preparation raw materials of the surface glaze layer is adjusted to 2 parts, and the chemical composition of the surface glaze layer is shown in Table 1.

[0125] Comparative Example 3

[0126] An antibacterial ceramic marble brick and a preparation method thereof, the difference from Example 1 is that the wax water is obtained by mixing and stirring silver-loaded nano-titanium dioxide and carrier wax in a mass ratio of 0.5:99.5.

[0127] Comparative Example 4

[0128] An antibacterial ceramic marble brick and a preparation method thereof, the difference from Example 1 is that the wax water is obtained by mixing and stirring silver-loaded nano-titanium dioxide and carrier wax in a mass ratio of 10:90.

[0129] Comparative Example 5

[0130] An antibacterial ceramic marble brick and a preparation method thereof, which differs from Example 1 only in that the raw materials for preparing the surface glaze layer include the following components in parts by weight: 15 parts of air knife clay, 10 parts of potassium feldspar, 30 parts of sodium feldspar, 5 parts of nepheline powder, 10 parts of wollastonite, 5 parts of calcined zinc oxide, 5 parts of zirconium silicate, 0.3 parts of silver-loaded nano-titanium dioxide, 13 parts of quartz powder, 5 parts of frit, and 2 parts of calcined alumina. The chemical composition of the surface glaze layer is shown in Table 1.

[0131] Comparative Example 6

[0132] An antibacterial ceramic marble brick and a preparation method thereof, which differs from Example 1 only in that the raw materials for preparing the surface glaze layer include the following components in parts by weight: 6 parts of nepheline, 7 parts of zirconium silicate, 10 parts of potassium feldspar, 25 parts of sodium feldspar, 16 parts of air knife clay, 5 parts of zinc oxide, 8 parts of wollastonite, 15 parts of frit and 10 parts of calcined alumina. The chemical composition of the surface glaze layer is shown in Table 1.

[0133] Comparative Example 7

[0134] An antibacterial ceramic marble brick and a preparation method thereof, which differs from Example 1 only in that the raw materials for preparing the surface glaze layer include the following components in parts by weight: 15 parts of calcined talc, 7 parts of zirconium silicate, 15 parts of potassium feldspar, 27 parts of sodium feldspar, 10 parts of air knife clay, 5 parts of zinc oxide, 8 parts of wollastonite, 10 parts of frit, 3 parts of calcined alumina, and 0.8 parts of silver-loaded nano-titanium dioxide. The chemical composition of the surface glaze layer is shown in Table 1.

[0135] Comparative Example 8

[0136] An antibacterial ceramic marble brick and a preparation method thereof, the difference from Example 1 is only that the preparation method comprises the following steps:

[0137] (1) Pressing the green body layer and drying it to a moisture content of ≤0.3% and a strength of ≥1.8MPa;

[0138] (2) providing a glaze layer on the body layer;

[0139] (3) Print the marble effect pattern on the top glaze layer, then print the pattern and digital glaze ink, with the grayscale set to 15~40%;

[0140] (4) A dry particle layer is provided on the pattern and digital glaze ink to prepare the blank for firing;

[0141] (5) The to-be-fired blank is fired, and then a wax film layer is provided by polishing and grinding the edges, thereby obtaining the antibacterial ceramic marble brick.

[0142] Comparative Example 9

[0143] An antibacterial ceramic marble tile and a preparation method thereof, the difference from Example 1 is that in the preparation raw materials of the surface glaze layer, the silver-loaded nano-titanium dioxide is replaced by a mixture of nano-titanium dioxide and silver nitrate of equal mass (the mass ratio of the two is 98:2).

[0144] Each glaze composition in Table 1 also contains a small amount of impurities, which have almost no effect on product performance and the content is trace, so they are not listed one by one.

[0145] Table 1

[0146]

[0147] Effect Example 1

[0148] In order to verify the use effect of the antibacterial ceramic marble bricks of the present invention, the products prepared in each embodiment and comparative example were subjected to the following tests:

[0149] (1) Antibacterial test: The antibacterial performance was tested by the JC / T897-2014 test method, and the antibacterial durability was tested by the GB / T9266 test method; the antibacterial test strains: Escherichia coli AS1.90, Staphylococcus aureus AS1.89, a blank control was set during the test, the test culture time was 24 hours, and the antibacterial rate was tested; the antibacterial durability test strains were the same as the antibacterial performance test, but 5% (W / V) sodium hypochlorite disinfectant was used for washing, the washing times were 500 times, a blank control was set during the test, the test culture time was 24 hours, and the antibacterial rate was tested;

[0150] (2) Texture test: 10 testers were selected and asked to touch the real marble sample with their palms first, and then touch each product and rate the texture they touched (blindfolded). The score ranged from 1 to 10 (integer points). The larger the score, the closer the texture is to the real marble, and the better the texture. To avoid subjectivity and randomness, the order of samples was only informed to the testers by numbers. After one round of testing was completed and the average score was recorded, the order was shuffled and the same test was repeated twice. The average score of the three rounds of testing was recorded and only the middle score was recorded (for example, if the average score of a sample in the three rounds was 9.0, 9.5 and 9.8, 9.5 would be recorded).

[0151] (3) Grain evaluation test: 10 testers were selected to evaluate the surface grain of each product under reflected light, using real marble as a control. The score ranged from 1 to 10 (integer points). The clearer the grain and the closer it is to the natural grain of natural marble under reflected light, the higher the score. The average score of each sample was calculated and recorded.

[0152] (4) Tile glaze condition: Confirm whether the glaze surface of the product is flat and smooth.

[0153] The test results are shown in Table 2.

[0154] Table 2

[0155]

[0156] It can be seen from Table 2 that the antibacterial ceramic marble tiles of the present invention have ideal antibacterial activity and antibacterial durability. At the same time, based on the process settings of the specific glaze and printing effect pattern, the texture of the product and the marble simulation texture on the surface are good, and the scores of the texture and texture can reach more than 9 points. Figure 1 As shown. According to Example 1, Examples 3 to 5, Comparative Examples 1 to 2 and Comparative Example 6, it can be seen that the amount of silver-loaded nano-titanium dioxide as a raw material for preparing the surface glaze layer not only directly affects the antibacterial effect of the product, but also affects the texture and appearance of the product. Figure 2 As shown, the surface glaze layer of the product described in Comparative Example 6 does not introduce silver-loaded nano-titanium dioxide, and the other raw material formulas and proportions are also different from those of the products in each embodiment. It belongs to the conventional marble tile surface glaze formula, which not only has poor antibacterial effect, poor marble texture effect, but also has a slippery glaze surface and an undulating orange peel morphology, and the texture is naturally poor. Figure 3 and Figure 4 Based on Example 1, the material formula of other glaze layers is not changed. Only the amount of silver-loaded nano-titanium dioxide added is adjusted. From the pictures of the products of Comparative Examples 1 and 2, it can be seen that excessive introduction of silver-loaded nano-titanium dioxide will have a significant impact on the clarity of the product's grain, and the grain will be blurred and yellow. From the results, since the introduction of too much silver-loaded nano-titanium dioxide will cause the grain of the glaze layer to be distorted and the texture to deteriorate, it is necessary to maintain the addition amount of 0.3 to 0.8 parts by weight, and it is further preferred to add 0.5 to 0.6 parts; on the other hand, 0.3 to 0.8 parts of silver-loaded nano-titanium dioxide are introduced into Example 1, Example 2, and Comparative Examples 5 and 7, but only Examples 1 and 2 meet expectations among the prepared products. The reason is that in the glaze layer, in addition to silver-loaded nano-titanium dioxide, the oxide components formed by other preparation raw materials will also affect the performance of the product. If the combination is not appropriate, the glaze composition will not be able to take into account both the antibacterial effect and the marble simulation effect.

[0157] According to Examples 1 and 8-10, it can be seen that the silver loading amount of silver-loaded nano-titanium dioxide will be different by adjusting the formula during preparation. Since the antibacterial mechanisms of silver and titanium dioxide are different, the difference in the ratio of the two will affect the antibacterial property of the product. In order to achieve the best balance between the antibacterial activity of silver and the photocatalytic antibacterial effect of titanium dioxide, a moderate silver loading amount is appropriate.

[0158] In addition to the glaze layer, the wax film layer of the product of the present invention is also the key to the antibacterial and simulation effects. It can be seen from Example 1, Examples 6-7 and Comparative Examples 3-4 that the introduction of silver-loaded nano-titanium dioxide in the wax film layer is also a necessary factor for whether the product can achieve antibacterial properties and antibacterial durability, but this component cannot be introduced too much, otherwise it will not only lead to a decrease in the texture and grain simulation effect of the product, but also cause the glaze surface to be uneven. According to Example 1 and Comparative Example 8, it can be seen that the product of the present invention is based on the special design of the glaze. If the traditional process is still used to print the marble effect pattern on the glaze layer, the apparent marble grain simulation degree of the product will be greatly reduced, and the grain will be distorted. Therefore, it is necessary to print the marble effect pattern directly on the body layer in advance.

[0159] It can be seen from Comparative Example 9 that if silver and nano-titanium dioxide, two well-known antibacterial active ingredients, are used as raw materials to construct the surface glaze layer, although the raw materials cannot be distinguished from each other in terms of chemical composition, the antibacterial activity and antibacterial durability of the prepared product are not ideal. The main reason is that both will suffer from loss and crystal transformation during the firing process, and the stability is poor. The surface glaze layer of the products prepared in Example 1 and Comparative Example 9 was tested for chemical composition after firing, and the results are shown in Table 3 (ignition loss and trace impurities are not listed in the table) and Figures 5 and 6 As shown, it can be seen that at the same addition amount, the chemical composition of the two is not the same, especially the titanium dioxide and silver with antibacterial active ingredients are less in the product prepared in Comparative Example 9, which fully demonstrates that only when the surface glaze layer is constructed in the form of silver-loaded nano-titanium dioxide as the preparation raw material, the obtained product can achieve sufficient antibacterial activity and antibacterial durability.

[0160] Table 3

[0161]

[0162] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An antibacterial ceramic marble brick, characterized in that: It comprises a body layer, a glaze layer, a dry particle layer and a wax film layer which are adjacent to each other in sequence, wherein the raw material for preparing the glaze layer comprises silver-loaded nano-titanium dioxide; The glaze layer includes the following chemical components in percentage by weight: SiO250~60%, Al2O317~23%, ZrO24~7%, K2O 2.5~4%, Na2O 2~5%, MgO0.3~2%, CaO2~6%, ZnO2~6%, BaO0.5~1.5%, TiO20.42~0.83% and Ag0.04~0.12%; the Ag is Ag + Mass content meter; The raw materials for preparing the surface glaze layer include the following components in parts by weight: 5-12 parts of air knife soil, 15-25 parts of potassium feldspar, 20-30 parts of sodium feldspar, 8-15 parts of nepheline, 3-5 parts of wollastonite, 3-6 parts of calcined zinc oxide, 8-15 parts of zirconium silicate, 5-10 parts of calcined aluminum oxide, 5-10 parts of frit, 10-15 parts of quartz powder and 0.3-0.8 parts of silver-loaded nano-titanium dioxide; The frit comprises the following components in parts by weight: 10-15 parts of kaolin, 15-20 parts of potassium feldspar, 20-30 parts of sodium feldspar, 10-15 parts of barium carbonate, 5-10 parts of dolomite, 5-10 parts of calcite, 1-3 parts of zinc oxide, 6-10 parts of aluminum oxide and 10-15 parts of quartz; The wax film layer comprises silver-loaded nano-titanium dioxide, and the mass percentage of the silver-loaded nano-titanium dioxide in the wax film layer is 2-5%.

2. The antibacterial ceramic marble tile according to claim 1, characterized in that: The particle size of the silver-loaded nano-titanium dioxide is 10-100 nm; the mass percentage of nano-titanium dioxide in the silver-loaded nano-titanium dioxide is 96-99%.

3. The antibacterial ceramic marble tile according to claim 2, characterized in that: The preparation method of the silver-loaded nano-titanium dioxide is as follows: (1) adding 0.03-0.05 mol of tetrabutyl titanate into water and stirring, then adding alkali solution and mixing until the pH value of the resulting mixed solution reaches 10, thereby obtaining a titanium dioxide solution, wherein the titanium element concentration in the titanium dioxide solution is 0.4-0.6 mol / L, then performing a hydrolysis precipitation reaction at 120-130° C., filtering the precipitate, and washing to obtain hydrated titanium dioxide; (2) Adding hydrated titanium dioxide to the silver nitrate solution, impregnating and stirring the mixture, drying the obtained solid, and then keeping the mixture at 450-500° C. for 0.5-1.5 h, and crushing the solid to obtain the silver-loaded nano-titanium dioxide.

4. The antibacterial ceramic marble tile according to claim 1, characterized in that: The dry particle layer includes dry particle particles, and the dry particle particles include the following chemical components in percentage by weight: SiO2 45~55%, Al2O3 17~20%, SrO4~7%, K2O2~5%, Na2O2~5%, MgO1~3%, CaO3~6%, ZnO3~6% and BaO8~11%.

5. The antibacterial ceramic marble tile according to claim 1, characterized in that: The wax film layer comprises the following components in percentage by weight: Carrier wax 95~98% and silver-loaded nano-titanium dioxide 2~5%.

6. The method for preparing the antibacterial ceramic marble brick according to any one of claims 1 to 5, characterized in that: The following steps are involved: The green body layer is pressed and dried to a moisture content of ≤0.3%; Printing a marble effect pattern on the body layer; Arranging a glaze layer on the body layer; Printing patterns and digital glaze ink on the surface glaze layer; A dry particle layer is provided on the pattern and digital glaze ink to prepare a blank to be fired; The blank to be fired is fired, and then a wax film layer is provided through polishing and edge grinding to obtain the antibacterial ceramic marble tile.

7. The method for preparing the antibacterial ceramic marble brick according to claim 6, characterized in that: The surface glaze layer is provided by spraying the surface glaze slurry on the body layer.

8. The method for preparing the antibacterial ceramic marble brick according to claim 6, characterized in that: The glaze amount of the surface glaze layer is 250-300 g / m 2 The dry particle amount of the dry particle layer is 200-300 g / m 2 .

9. The method for preparing the antibacterial ceramic marble brick according to claim 6, characterized in that: The dry particle layer is provided by spraying dry particle slurry on the pattern and the digital glaze ink.

Citation Information

Patent Citations

  • High-strength antibacterial domestic ceramic product and preparation method thereof

    CN111499362A

  • Antibacterial glaze, antibacterial brick and preparation method of antibacterial brick

    CN112239372A