A multicolor tunable phosphate fluorescent glass-ceramic and its preparation method

By employing a multicolor tunable phosphate fluorescent glass-ceramic material doped with Dy3+ and Tm3+ in a P2O5-BaO-ZnO-B2O3 glass matrix in LED lighting technology, the problems of insufficient thermal and chemical stability of epoxy resin encapsulation materials are solved, enabling the adjustment of luminous color and color temperature, improving luminous efficiency and extending device life.

CN118666495BActive Publication Date: 2026-11-17XINJIANG TECH INST OF PHYSICS & CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310241968.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-14
Publication Date
2026-11-17
Estimated Expiration
2043-03-14

AI Technical Summary

Technical Problem

In existing LED lighting technologies, epoxy resin or silicone composite phosphor encapsulation materials suffer from insufficient thermal stability, chemical stability, and luminous stability under high power, leading to shortened device lifespan and color drift.

Method used

A multicolor tunable phosphate fluorescent glass-ceramic material doped with Dy3+ and Tm3+ using a P2O5-BaO-ZnO-B2O3 glass matrix was prepared by a suitable heat treatment process to form BaZn2(PO4)2 nanocrystals, which provide good thermal stability and luminescence performance.

Benefits of technology

It achieves adjustable emission color and color temperature, improves luminous efficiency and stability, extends the lifespan of LED devices, simplifies the production process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118666495B_ABST
    Figure CN118666495B_ABST
Patent Text Reader

Abstract

This invention provides a multicolor tunable phosphate fluorescent glass-ceramic and its preparation method. The chemical composition of the glass matrix of this glass-ceramic includes P2O5, BaO, ZnO, and B2O3, and the glass matrix is ​​doped with Dy. 3+ and Tm 3+ The glass matrix, after undergoing crystallization heat treatment, precipitates BaZn2(PO4)2 nanocrystals. This glass-ceramic material possesses high crystallinity and transparency. The excitation spectrum of the phosphor is in the ultraviolet region, and this can be achieved by changing Tm. 3+ The doping amount can achieve spectral shift and thus change the emission color. The sample of this invention has good thermal stability and rich luminescent properties, and can be used as a novel fluorescent material in the field of luminescence.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of phosphate glass-ceramic composite materials technology, specifically to an adjustable multicolor phosphate fluorescent glass-ceramic and its preparation method. Background Technology

[0002] While LED lighting, as a next-generation solid-state lighting technology, boasts numerous advantages such as energy saving, environmental friendliness, and long lifespan, its application in high-power lighting suffers from "efficiency decline." Using existing LED lighting encapsulation technologies, such as epoxy resin or silicone composite phosphors, presents challenges in meeting the required thermal, chemical, and luminous stability standards. Firstly, commercially available materials typically use organic resins to encapsulate phosphors, resulting in poor performance at high power levels. This encapsulation method, due to the mismatch in refractive indices between the organic material and the phosphor, hinders light absorption and emission. Secondly, organic materials have low thermal conductivity, while high-power LEDs operate at temperatures between 150 and 200°C. At these temperatures, organic materials soften or yellow, leading to color drift or shortened lifespan. An effective solution is to use inorganic fluorescent materials with high thermal and chemical stability, such as phosphor-in-glass (PiG), fluorescent ceramics, or fluorescent glass-ceramics, to replace traditional organic materials. Research has shown that this approach effectively improves the color coordinate stability of fluorescent materials and extends the lifespan of LED devices. Among them, the fluorescent glass-ceramic prepared by solid-state sintering is obtained by uniformly mixing, pressing, and crystallizing heat treatment of rare earth-doped glass powder. Compared with organic resin encapsulation materials, the resulting glass-ceramic exhibits better thermal stability, avoids problems such as softening and color drift, and also possesses a good color rendering index and rich luminescent properties. Therefore, the development of this type of rare earth-doped glass-ceramic material is of great significance for obtaining LED lighting sources with excellent luminescent performance. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide a multi-color tunable phosphate fluorescent glass-ceramic material and its preparation method, which are in view of the shortcomings of the prior art. The glass-ceramic material has good thermal stability and achieves tunable emission color and color temperature. The preparation method of the glass-ceramic material is simple and efficient.

[0004] The technical solution adopted by this invention to solve the above-mentioned technical problems is as follows: a multicolor tunable phosphate fluorescent glass-ceramic material, wherein the glass matrix of the glass-ceramic material comprises, by mass percentage: P2O5 30-45%, BaO 10-15%, ZnO 25-40%, and B2O3 15-30%, with the total mass of the above components being 100%, and the glass matrix being doped with Dy.3+ Tm 3+ The material is doped in the form of compounds, with the doped dysprosium-containing compounds and thulium-containing compounds accounting for 0.2-0.3% and 0.1-1% of the total mass of other raw materials, respectively, and BaZn2(PO4)2 nanocrystals are precipitated in the glass matrix.

[0005] Preferably, the dysprosium compound is Dy2O3 and the thulium compound is Tm2O3.

[0006] The glass-ceramic material of this invention uses a P2O5-BaO-ZnO-B2O3 glass matrix, in which P2O5 and B2O3 provide a rigid structure, giving the glass-ceramic material advantages such as high hardness and good mechanical properties, while creating nucleation and boundary conditions for the glass crystallization process; the role of introducing ZnO and BaO is to provide the necessary constituent elements for the precipitation of nanocrystalline BaZn2(PO4)2.

[0007] The matrix glass of this invention possesses good forming ability and thermal stability, as well as low phonon energy and good transparency. It is an excellent matrix for rare earth ions, has a low forming temperature, and low raw material cost. The nanocrystalline BaZn2(PO4)2 precipitated in the glass matrix contains Ba... 2+ The radius and the doped Dy 3+ Tm 3+ Since their radii are similar, the incorporated Dy can be made more efficient. 3 + Tm 3+ It is relatively easy to embed into nanocrystalline BaZn2(PO4)2. A large number of rare earth luminescent ions are embedded in a low phonon energy environment, which helps to reduce the probability of non-radiative transitions and improve luminescence efficiency.

[0008] This invention provides a method for preparing a multicolor tunable phosphate fluorescent glass-ceramic material, comprising the following steps:

[0009] 1) Raw material preparation: Weigh the raw materials according to the percentage of their mass, mix them evenly, and obtain a uniformly mixed powder;

[0010] 2) Melting and quenching: The powder obtained in step 1) is calcined, melted, quenched, and then dried to obtain solid glass;

[0011] 3) Annealing: The solid glass obtained in step 2) is annealed and cooled to room temperature to obtain precursor glass. The precursor glass is then ground to obtain glass powder.

[0012] 4) Pressing: Pour the glass powder obtained in step 3) into a mold and press it into a round green sheet;

[0013] 5) Heat treatment: The circular green blank obtained in step 4) is heat treated and cooled to room temperature to obtain rare earth Dy. 3+ / Tm 3+ BaZn2(PO4)2 fluorescent glass-ceramic material.

[0014] Preferably, in step 2), the calcination temperature is 1200-1300℃ and the calcination time is 2-4 hours.

[0015] The molten material is poured into a beaker filled with deionized water for quenching.

[0016] Preferably, in step 3), the annealing temperature is 350-450℃, the annealing time is 2-5 hours, and the grinding time is 3-6 hours.

[0017] Preferably, in step 4), a hydraulic press is used for pressing, with the hydraulic press using 20-40MPa and a holding time of 50-70 seconds.

[0018] Preferably, in step 5), the heat treatment temperature is 530℃-560℃ and the heat treatment time is 3-6 hours.

[0019] Specifically, the aforementioned rare earth Dy 3+ Tm 3+ The preparation method of ion-doped BaZn2(PO4)2 glass-ceramic material is carried out according to the following steps:

[0020] 1) Raw material preparation: Weigh the raw materials according to the following mass percentages: P2O5 30-45%, BaO 10-15%, ZnO 25-40%, B2O3 15-30%, Dy2O3 0.25%, Tm2O3 0.1-1%. The total mass of the above components is 100%. Mix and grind them evenly in an agate mortar to obtain a uniformly mixed powder. Transfer the powder to a high-purity corundum crucible.

[0021] 2) Melting and quenching: The powder obtained in step 1 is placed in a muffle furnace at a temperature of 1200-1300℃ and calcined for 2-4 hours. The molten material in the high-purity corundum crucible is quickly poured into a beaker filled with deionized water to complete the quenching process. Then it is transferred to an oven to dry and obtain solid glass.

[0022] 3) Annealing: The solid glass obtained in step 2 is annealed at a temperature of 400℃ for 3 hours. Finally, it is allowed to cool naturally to room temperature to obtain the precursor glass. The precursor glass is then ground in an agate mortar for 4 hours to obtain glass powder.

[0023] 4) Tableting: Weigh 0.2g of the powder obtained in step 3 and pour it into a mold with a diameter of 10mm. Press it into a round green sheet by using a hydraulic press with a pressure of 20-40MPa for 60 seconds.

[0024] 5) Heat treatment: The round green blanks obtained in step 4 are placed in a muffle furnace for heat treatment at a temperature of 530℃-560℃ for 4 hours. Finally, they are allowed to cool naturally to room temperature to obtain rare earth Dy. 3+ / Tm 3+ BaZn2(PO4)2 fluorescent glass-ceramic material.

[0025] The preparation process of this invention simplifies the heat treatment process for inducing precursor glass nucleation and crystallization. By using appropriate heat treatment temperature and time, the precursor glass obtains sufficient energy for nucleation and growth, resulting in a glass-ceramic material with high crystallinity and good light transmittance. Replacing the two-step crystallization heat treatment with a one-step method simplifies the process flow, reduces production costs, and improves production efficiency.

[0026] Compared with the prior art, the present invention has the following technical effects:

[0027] 1. This invention first obtains a precursor glass through a melt-quenching method, and then partially crystallizes it through heat treatment to obtain a glass-ceramic material rich in BaZn2(PO4)2 nanocrystals, which provides a low phonon energy environment for rare earth luminescent ions, resulting in a large amount of rare earth luminescent ions Dy 3+ Tm 3+ It can be embedded in low phonon energy environments, which is beneficial to improve its luminescence intensity, reduce the probability of non-radiative transitions, and improve luminescence efficiency.

[0028] 2. The glass-ceramic material of the present invention possesses high crystallinity and transparency. The excitation spectrum of the phosphor is in the ultraviolet region. By changing Tm... 3+ The doping level can shift the spectrum and thus change the emission color. This fluorescent glass-ceramic, by changing the doping Tm... 3+ The value can be adjusted for BaZn2(PO4)2:Dy 3+ / Tm 3+ Glass ceramics have a warm and pleasant color temperature of light emission, as well as good thermal and luminescent stability, making them a novel fluorescent material that can be applied in the field of light emission. Attached Figure Description

[0029] Figure 1 The XRD spectrum of the fluorescent glass-ceramic in Example 1 of this invention;

[0030] Figure 2 The temperature-dependent emission spectral coordinates of the fluorescent glass ceramic in Embodiment 3 of the present invention;

[0031] Figure 3 The emission spectra of the fluorescent glass ceramics in Examples 1, 2, 3, and 4 of this invention are shown.

[0032] Figure 4 These are the emission spectral color coordinates of the fluorescent glass ceramics in Examples 1, 2, 3, and 4 of this invention. Detailed Implementation

[0033] The technical solution of the present invention will be described in detail below with reference to the accompanying drawings and embodiments.

[0034] Example 1:

[0035] (1) Weigh the raw materials according to the mass percentage of P2O5 32%, BaO 10%, ZnO 32%, B2O3 26%, Dy2O3 0.25%, Tm2O3 0.1%, place them in an agate mortar and grind them to obtain a uniformly mixed powder, and transfer them to a high-purity corundum crucible.

[0036] (2) Place the powder obtained in step (1) in a muffle furnace at 1200℃ for 2 hours, quickly pour the melt in the high-purity corundum crucible into a beaker filled with deionized water to complete the quenching process, and then transfer it to an oven to dry to obtain solid glass.

[0037] (3) Anneal the solid glass obtained in step (2) at a temperature of 400°C for 3 hours, and then let it cool naturally to room temperature to obtain the precursor glass. Grind the precursor glass in an agate mortar for 4 hours to obtain glass powder.

[0038] (4) Weigh 0.2g of the powder obtained in step (3) and pour it into a mold with a diameter of 10mm. Press it into a round blank by using a hydraulic press with a pressure of 20MPa for 60 seconds.

[0039] (5) The circular green blank obtained in step (4) is placed in a muffle furnace for heat treatment at a temperature of 530°C for 4 hours. Finally, it is allowed to cool naturally to room temperature to obtain rare earth Dy. 3+ / Tm 3+ BaZn2(PO4)2 fluorescent glass-ceramic material.

[0040] The XRD pattern of the BaZn2(PO4)2 glass-ceramic obtained in step (5) is as follows: Figure 1 As shown, both crystalline and amorphous peaks are present, and the peak positions and intensities of the crystalline peaks correspond to those of the BaZn2(PO4)2 PDF card, indicating the presence of the corresponding crystalline phase. The emission spectrum measured under 362nm excitation is shown below. Figure 3 Display Dy 3+ / Tm 3+ Characteristic emission peak positions of BaZn2(PO4)2 phosphate glass-ceramics. Color coordinates are (0.3184, 0.3515), see [reference needed]. Figure 4 The position indicated by "a" has a color temperature of 6104K and emits cool white light.

[0041] Example 2:

[0042] (1) Weigh the raw materials according to the mass percentages of P2O5 35%, BaO 12%, ZnO 37%, B2O3 16%, Dy2O3 0.25%, and Tm2O3 0.25%, place them in an agate mortar and grind them to obtain a uniformly mixed powder, and then transfer them to a high-purity corundum crucible.

[0043] (2) Place the powder obtained in step (1) in a muffle furnace at 1250°C for 3 hours, quickly pour the melt in the high-purity corundum crucible into a beaker filled with deionized water to complete the quenching process, and then transfer it to an oven to dry to obtain solid glass.

[0044] (3) Anneal the solid glass obtained in step (2) at a temperature of 400°C for 3 hours, and then let it cool naturally to room temperature to obtain the precursor glass. Grind the precursor glass in an agate mortar for 4 hours to obtain glass powder.

[0045] (4) Weigh 0.2g of the powder obtained in step (3) and pour it into a mold with a diameter of 10mm. Press it into a round blank by using a hydraulic press with a pressure of 30MPa for 60 seconds.

[0046] (5) The circular green blank obtained in step (4) is placed in a muffle furnace for heat treatment at a temperature of 540°C for 4 hours. Finally, it is allowed to cool naturally to room temperature to obtain rare earth Dy. 3+ / Tm 3+ BaZn2(PO4)2 fluorescent glass-ceramic material.

[0047] The emission spectrum of the BaZn2(PO4)2 glass ceramic obtained in step (5) under 362nm light source excitation is shown in the figure. Figure 3 Display Dy 3+ / Tm 3+ Characteristic emission peak positions of BaZn2(PO4)2 phosphate glass-ceramics. Color coordinates are (0.2951, 0.3092), see [reference needed]. Figure 4 The position indicated by "b" has a color temperature of 7887K and emits cool white light.

[0048] Example 3:

[0049] (1) Weigh the raw materials according to the mass percentages of P2O5 40%, BaO 11%, ZnO 29%, B2O3 20%, Dy2O3 0.25%, and Tm2O3 0.5%, place them in an agate mortar and grind them to obtain a uniformly mixed powder, and then transfer them to a high-purity corundum crucible.

[0050] (2) Place the powder obtained in step (1) in a muffle furnace at 1300℃ for 4 hours, quickly pour the melt in the high-purity corundum crucible into a beaker filled with deionized water to complete the quenching process, and then transfer it to an oven to dry to obtain solid glass.

[0051] (3) Anneal the solid glass obtained in step (2) at a temperature of 400°C for 3 hours, and then let it cool naturally to room temperature to obtain the precursor glass. Grind the precursor glass in an agate mortar for 4 hours to obtain glass powder.

[0052] (4) Weigh 0.2g of the powder obtained in step (3) and pour it into a mold with a diameter of 10mm. Press it into a round blank by using a hydraulic press with a pressure of 40MPa for 60 seconds.

[0053] (5) The circular green blank obtained in step (4) is placed in a muffle furnace for heat treatment at a temperature of 550°C for 4 hours. Finally, it is allowed to cool naturally to room temperature to obtain rare earth Dy. 3+ / Tm 3+ BaZn2(PO4)2 fluorescent glass-ceramic material.

[0054] The temperature-dependent emission chromaticity coordinates of the BaZn2(PO4)2 glass ceramic obtained in step (5) are as follows: Figure 2 As shown, the emission spectrum color coordinates show almost no shift with increasing temperature, indicating that the material possesses good thermal stability. The emission spectrum measured under 362 nm light source excitation is shown below. Figure 3 Display Dy 3+ / Tm 3+ Characteristic emission peak positions of BaZn2(PO4)2 phosphate glass-ceramics. Color coordinates are (0.2904, 0.2911), see [reference needed]. Figure 4 The position indicated by "c" has a color temperature of 8793K and emits cool white light.

[0055] Example 4:

[0056] (1) Weigh the raw materials according to the mass percentages of P2O5 45%, BaO 15%, ZnO 25%, B2O3 15%, Dy2O3 0.25%, and Tm2O3 1.0%, place them in an agate mortar and grind them to obtain a uniformly mixed powder, and transfer them to a high-purity corundum crucible.

[0057] (2) Place the powder obtained in step (1) in a muffle furnace at 1250°C for 3 hours, quickly pour the melt in the high-purity corundum crucible into a beaker filled with deionized water to complete the quenching process, and then transfer it to an oven to dry to obtain solid glass.

[0058] (3) Anneal the solid glass obtained in step (2) at a temperature of 400°C for 3 hours, and then let it cool naturally to room temperature to obtain the precursor glass. Grind the precursor glass in an agate mortar for 4 hours to obtain glass powder.

[0059] (4) Weigh 0.2g of the powder obtained in step (3) and pour it into a mold with a diameter of 10mm. Press it into a round blank by using a hydraulic press with a pressure of 30MPa for 60 seconds.

[0060] (5) The circular green blank obtained in step (4) is placed in a muffle furnace for heat treatment at a temperature of 560°C for 4 hours. Finally, it is allowed to cool naturally to room temperature to obtain rare earth Dy. 3+ / Tm 3+ BaZn2(PO4)2 fluorescent glass-ceramic material.

[0061] The emission spectrum of the BaZn2(PO4)2 glass ceramic obtained in step (5) under excitation by a 362nm light source is shown below. Figure 3 Display Dy 3+ / Tm 3+ Characteristic emission peak positions of BaZn2(PO4)2 phosphate glass-ceramics. Color coordinates are (0.2844, 0.2832), see [reference needed]. Figure 4 The position indicated by "d" has a color temperature of 9749K and emits cool white light.

[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to the embodiments, those skilled in the art should understand that modifications or equivalent substitutions to the technical solutions of the present invention do not depart from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A multicolor tunable phosphate fluorescent glass-ceramic, characterized in that, The glass matrix of the multicolor adjustable phosphate fluorescent glass ceramic consists of the following components in mass percentage: P2O5 30-45%, BaO 10-15%, ZnO 25-40% and B2O3 15-30%, and the glass matrix is doped with Dy in the form of compound 3+ and Tm 3+ , and the doped dysprosium compound and thulium compound account for 0.2-0.3% and 0.1-1% of the total mass of other raw materials respectively; and the glass matrix is precipitated with BaZn2(PO4)2 nanocrystals.

2. The multicolor tunable phosphate fluorescent glass-ceramic according to claim 1, characterized in that, The dysprosium-containing compound is Dy2O3, and the thulium-containing compound is Tm2O3.

3. A method for preparing a multicolor tunable phosphate fluorescent glass-ceramic material, used to prepare the multicolor tunable phosphate fluorescent glass-ceramic material as described in claim 1 or 2, comprising the following steps: 1) Raw material preparation: Weigh the raw materials according to the percentage by weight, mix them evenly, and obtain the powder; 2) Melting and quenching: The powder obtained in step 1) is calcined, melted, quenched, and then dried to obtain solid glass; 3) Annealing: The solid glass obtained in step 2) is annealed and cooled to room temperature to obtain precursor glass. The precursor glass is then ground to obtain glass powder. 4) Pressing: Pour the glass powder obtained in step 3) into a mold and press it into a round green sheet; 5) Heat treatment: The circular green blank obtained in step 4) is heat treated and cooled to room temperature to obtain rare earth Dy. 3+ / Tm 3+ BaZn2(PO4)2 fluorescent glass-ceramic material.

4. The preparation method according to claim 3, characterized in that, In step 2), the calcination temperature is 1200-1300℃ and the calcination time is 2-4 hours; The molten material is poured into a beaker filled with deionized water for quenching.

5. The preparation method according to claim 3, characterized in that, In step 3), the annealing temperature is 350-450℃, the annealing time is 2-5 hours, and the grinding time is 3-6 hours.

6. The preparation method according to claim 3, characterized in that, In step 4), a hydraulic press is used for pressing, with the hydraulic press using 20-40MPa and a holding time of 50-70 seconds.

7. The preparation method according to claim 3, characterized in that, In step 5), the heat treatment temperature is 530℃-560℃ and the heat treatment time is 3-6 hours.