Low molecular weight powder salt resistant drag reducer
Through the preparation of low molecular weight powder drag reducer, the polymerization of methacryldopamine and diphenyl-1,3-butadiene is used to combine auxiliary components to form a dry powder drag reducer, which solves the problem of high viscosity oil and the problem of poor resistance reduction effect in fast-flowing water has achieved efficient industrial applications such as resistance reduction and environmental protection.
Patent Information
- Application Number
- CN202411196738.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-29
AI Technical Summary
In the prior art, high molecular weight drag reducing agents have poor resistance reduction effects in exploiting high viscosity oil and fast flowing water systems. The use of too much polymer materials will contaminate the formation, affect storage permeability, and it is difficult to achieve efficient development of unconventional oil and gas. resource.
Using low molecular weight powder drag reducing agent, it is prepared by polymerization of methacryldopamine and diphenyl-1,3-butadiene under heating conditions. The average molecular weight of the polymer is between 30,000 and 60,000, combined with auxiliary components. , a drag reducing agent in a dry powder state, suitable for the resistance reduction of high-speed flowing water and high-viscosity oil.
It achieves excellent resistance reduction effect in high flow rate water environment and high viscosity oil fields, reduces the amount of drag reducing agent used, is suitable for on-site construction and large-scale industrial applications, and has good salt resistance characteristics.
Smart Images

Figure CN118684820B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an additive in a process of extracting oil from a well and a manufacturing process thereof, and to a general organic chemical synthesis method. More specifically, the present invention relates to a drag reducer in an oil extraction process, and to a low molecular weight powder (salt-resistant) drag reducer and a manufacturing process thereof. Background Art
[0002] With the continuous upgrading of industrial automation production and the acceleration of global industrialization, the demand for energy and resources is increasing. In the field of oil and gas extraction, in addition to conventional oil and gas fields, unconventional oil and gas resources need to be deeply developed and utilized. Efficient development and utilization of unconventional oil and gas resources, while ensuring the coordination of environmental protection and green development, has become a potential development goal and an important component of the energy industry.
[0003] The use of pressurized water to implement fracturing has become an important method for the exploitation of unconventional oil and gas fields, such as the development of shale gas, coalbed methane, and high-density sandstone oil and gas reservoirs. Based on relevant technologies, the slick water fracturing process was developed at the end of the last century to successfully improve the process of tight gas wells. Since then, the slick water fracturing system has begun to become the mainstream development process and gradually become the main improvement technology for the exploitation of tight gas reservoirs. According to the principle of this process, slick water is mainly composed of water, drag reducers and additives. The drag reducer component can reduce the flow resistance of the fluid, increase production capacity and save costs.
[0004] At present, many research teams are conducting research on water fracturing systems and drag reduction processes. For example, patent publication CN102516975A discloses a kind of fast-dissolving and recyclable slippery water in shale gas reservoirs, which claims to be able to effectively develop high-density oil shale fields. However, in this type of patent, the drag agent used is polyacrylamide or polyacrylamide derivatives with a molecular weight of nearly 1 million. When used, the amount of polymer material used is large and the drag reduction effect on high-viscosity oil and fast-flowing water systems is not ideal. On the other hand, when too much polymer material is used in pursuit of a high drag reduction rate, it will pollute the formation and reduce the storage permeability, which is not conducive to the simultaneous development of industrial development and environmental protection. Summary of the invention
[0005] The purpose of the present invention is to solve one or more deficiencies in the above-mentioned prior art and to provide an improved low molecular weight powder drag reducer having high-speed flowing water drag reduction effect and high viscosity oil drag reduction and viscosity reduction effect and a preparation method thereof. At the same time, the drag reducer in powder state is conducive to on-site construction and large-scale industrial application, and may have other auxiliary properties, such as good salt resistance when using an on-site preparation process.
[0006] The first aspect of the present invention provides a low molecular weight powder drag reducer, for example, a low molecular weight powder salt-resistant drag reducer, wherein the low molecular weight powder drag reducer comprises a low molecular weight polymer with an average molecular weight within 3 million, preferably between 30,000 and 60,000, wherein the low molecular weight polymer is polymerized by methacryloyl dopamine and diphenyl-1,3-butadiene in the presence of a polymerization initiating component and under heating conditions.
[0007] According to an optional technical solution of the present invention, in the low molecular weight powder drag reducer of the present invention, the diphenyl-1,3-butadiene is 1,4-diphenyl-1,3-butadiene, and the low molecular weight polymer is expressed by the following molecular formula:
[0008] .
[0009] In a typical scheme, the average molecular weight of the polymer of the present invention may refer to the viscosity average molecular weight. In the measurement and characterization of the viscosity average molecular weight, it is usually difficult to accurately control the n value to a certain value. As long as the average molecular weight of the prepared low molecular weight polymer is less than 100,000 by adjusting the raw material ratio or process parameters in the scheme of the present invention, in an optional scheme, the average molecular weight of the polymer is between 30,000 and 60,000. Correspondingly, the n value may be between 70 and 130, preferably between about 80 and 95.
[0010] The low molecular weight powder drag reducer of the present invention refers to a polymer having an average molecular weight (such as viscosity average molecular weight) of less than 100,000, preferably less than or equal to 80,000, preferably between 10,000 and 80,000, or between 30,000 and 60,000. This is relative to the high molecular weight polymers with an average molecular weight of hundreds of thousands or even millions used in the related art. Those skilled in the art can clearly understand the meaning of "low molecular weight" based on the contents and explanations disclosed in this specification and the common knowledge of the related art in this field.
[0011] In a further optional scheme of the present invention, the low molecular weight powder drag reducer also includes an auxiliary agent component, which is formed by polymerizing sodium 2-acrylamido-2-methylpropane sulfonate and sodium acrylate in the presence of an initiator at 40°C to 50°C, the average molecular weight of the auxiliary agent component is 50,000 to 80,000, and the mass ratio of the low molecular weight polymer to the auxiliary agent component is 5:1 to 10:1.
[0012] In a further preferred technical solution, the auxiliary agent component is described by the following chemical structure:
[0013] .
[0014] Similarly, the average molecular weight of the auxiliary agent component can also be expressed as a viscosity average molecular weight, wherein the value of m can be between 170 and 280, preferably, the value range of m can be approximately between 220 and 250.
[0015] In an optional technical solution, the low molecular weight powder drag reducer is in a dry powder state. In the present invention, the low molecular weight powder drag reducer in a dry powder (powder) state has a significantly excellent effect for industrial applications, such as on-site construction of oil wells, which will be further described in subsequent specific embodiments.
[0016] In a further optional technical solution, the low molecular weight polymer is obtained by the following preparation process:
[0017] 1) Prepare 3-methacryloyl dopamine, and then determine the amounts of 3-methacryloyl dopamine, 1, 4-diphenyl-1,3-butadiene, n-propanol, and purified water according to a molar ratio of 1: (0.90-1.1): (1-1.2): (10-30);
[0018] 2) mixing the 1,4-diphenyl-1,3-butadiene and n-propanol and stirring them thoroughly to obtain a 1,4-diphenyl-1,3-butadiene mixed liquid;
[0019] 3) Mix 3-methacryloyl dopamine with purified water, and add it into the above 1,4-diphenyl-1,3-butadiene mixture under stirring;
[0020] 4) adding a polymerization initiator in an amount of 0.1 mol% to 1 mol% of the total molar amount of the raw materials, and introducing an inert gas for 0.5 to 2 hours;
[0021] 5) heating the reaction at 60 to 80° C. for 10 to 20 hours to obtain the low molecular weight polymer component.
[0022] In another optional technical solution, the auxiliary agent component is obtained by the following preparation process:
[0023] Sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate are dissolved in deionized water at a mass ratio of 10:(1-5), and the mixture is stirred thoroughly. The pH value is adjusted to be in the range of 6 to 7, and an inert gas is introduced for 0.5 to 2 hours. An initiator is added at 40° C. to 50° C., and the amount of the initiator added is 0.5% of the total mass of sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate. The reaction is continued for 1 to 3 hours to obtain the auxiliary agent component.
[0024] In an optional technical solution, the low molecular weight powder drag reducer is obtained by treating the low molecular weight polymer and the auxiliary agent component using a post-mixing treatment step, and the post-mixing treatment step includes:
[0025] The low molecular weight polymer and the auxiliary agent component are mixed in a mass ratio of 5:1 to 10:1, and deionized water of 1 to 3 times the total mass of the two is added for stirring. After stirring, the composition is filtered and dried. In the drying step, the mixture is sent to a rotary dryer for 0.5 to 3 hours, and the dried solid matter is then sent to a vibrating fluidized bed for further drying. After vibration drying, it is sieved to obtain the low molecular weight powder drag reducer.
[0026] The second aspect of the present invention provides a method for preparing a low molecular weight powder drag reducer, the method comprising the following first step, second step and third step:
[0027] First step: Preparation of low molecular weight polymer
[0028] Weigh 3-methacryloyl dopamine, and then determine the amount of 3-methacryloyl dopamine, 1, 4-diphenyl-1,3-butadiene, n-propanol, and purified water according to the molar ratio of 1: (0.90-1.1): (1-1.2): (10-30);
[0029] The 1,4-diphenyl-1,3-butadiene and n-propanol are mixed and stirred sufficiently to obtain a 1,4-diphenyl-1,3-butadiene mixed liquid;
[0030] After mixing 3-methacryloyl dopamine with purified water, add the mixture into the above 1,4-diphenyl-1,3-butadiene solution under stirring;
[0031] Add a polymerization initiator in an amount of 0.1 mol% to 1 mol% of the total molar amount of the raw materials, and introduce an inert gas for 0.5 to 2 hours;
[0032] heating the reaction at 60 to 80° C. for 10 to 20 hours, and measuring the average molecular weight to obtain the low molecular weight polymer;
[0033] Second step: preparation of auxiliary components
[0034] Dissolve sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate in deionized water at a mass ratio of 10:(1-5), stir thoroughly, adjust the pH value to a range of 6 to 7, introduce an inert gas for 0.5 to 2 hours, add an initiator at 40° C. to 50° C., the amount of the initiator added is 0.5% of the total mass of sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate, continue the reaction for 1 to 3 hours, and then measure the average molecular weight to obtain the auxiliary agent component;
[0035] Step 3: Post-mixing process
[0036] The low molecular weight polymer and the auxiliary agent component are mixed in a mass ratio of 5:1 to 10:1 to obtain a mixture, and deionized water of 1 to 3 times the total mass of the two is added for stirring. After stirring, the composition is filtered and dried. In the drying step, the mixture is sent to a rotary dryer for 0.5 to 3 hours. The dried solid matter is sent to a vibrating fluidized bed for further drying, and sieved after vibration drying to obtain the low molecular weight powder drag reducer.
[0037] In the technical solution provided by the present invention, any crushing and drying technology can be added to ensure that a low molecular weight drag reducer in the form of a powder is finally obtained.
[0038] In an optional technical solution, the method prepares a low molecular weight powder drag reducer as described in any one of the technical solutions in the first aspect. The preparation method of the present invention can be implemented alone as a method for preparing a low molecular weight powder drag reducer, and can also be implemented to prepare a low molecular weight powder drag reducer having the various characteristics described in the first aspect.
[0039] The low molecular weight powder drag reducer and preparation process provided by the technical solution of the present invention are suitable for the drag reduction field of high velocity water environment (such as high pressure water fracturing oil well exploitation environment) and high viscosity oil, and can achieve excellent drag reduction effect in high velocity water environment and high viscosity oil, and can reduce the use amount of drag reducer. In the process of the present invention, a drag reducer product in powder (dry powder) state is also provided, which is particularly suitable for on-site construction and exploitation process on oil wells.
[0040] It should be noted that the product and process of the present invention may include the above steps and other related steps. In an optional or preferred scheme, the scheme of the present invention may only include the above steps or components, no longer include other steps and components, or do not significantly include other main steps or main components. In addition, the steps should be performed in a sequential order in the optional scheme, and the components and steps of the present invention can be implemented independently or arbitrarily superimposed and combined with each other.
[0041] In the following, the technical solutions and advantages of the present invention will be explained and described in more detail in conjunction with specific implementation methods. It should be understood that the contents presented in the specification and specific implementation methods are only for the purpose of more clearly illustrating the technical solutions and advantages of the present invention, and do not limit the protection scope of the present invention. Those skilled in the art can obtain the changed technical solutions based on the disclosure of the specification for various reasonable transformations. As long as they do not deviate from the spirit of the present invention, the various changed technical solutions should be understood to be included in the protection scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The accompanying drawings are used to provide a further understanding of the technical solution of the present disclosure and constitute a part of the specification. Together with the specific embodiments of the present application, they are used to explain the technical solution of the present disclosure and do not constitute a limitation on the technical solution of the present disclosure.
[0043] Figure 1 It is a common drag reduction performance test spectrum of the main embodiment of the present invention. DETAILED DESCRIPTION
[0044] The present invention is described in more detail hereinafter to facilitate understanding of the invention.
[0045] Before describing the specific implementation scheme, it should be noted that those skilled in the art can select appropriate raw materials according to the enlightenment and teaching of the present disclosure, and use relevant testing equipment to perform relevant tests and obtain corresponding results. For raw materials without specific manufacturers or pathways, those skilled in the art can select raw materials that meet corresponding requirements as reaction starting materials according to the disclosure and requirements of this specification. The reaction raw materials of the process part compounds are derived from the initial products synthesized in the preamble step of the present invention, which can also be understood according to the present disclosure.
[0046] First, the main raw materials used in the present invention and the corresponding acquisition channels or raw material origins are listed in Table 1. It should be noted that the raw materials not described in the present invention are raw material varieties that can be obtained by those skilled in the art based on common technical knowledge and existing market products.
[0047] Table 1: Description of the main raw materials used in the present invention
[0048]
[0049] It should be noted that the molecular weight indicated in the technical solution, the embodiments of the specification and the invention content of the present invention generally refers to the viscosity average molecular weight. In the experimental examples of the present invention, a fully automatic viscosity measurement system (product code IVS800) produced by Zhongwang Technology Co., Ltd. was used.
[0050] It should also be noted that the "low molecular weight" in the "low molecular weight powder drag reducer" mentioned in the technical solution and embodiments of the present invention is relative to the molecular weight of the polymer used in the related art, which is in the hundreds of thousands, millions or even tens of millions. In the technical solution of the present invention, preferably, "low molecular weight" can refer to polymer molecules with a viscosity average molecular weight of less than 100,000. More typically, the viscosity average molecular weight of the polymer molecules (low molecular weight polymers) contained in the low molecular weight powder drag reducer of the present invention is between 10,000 and 100,000, more typically between 20,000 and 80,000, or between 30,000 and 60,000. In the following description, unless otherwise specified, the molecular weight of the "polymer" generally refers to the "viscosity average molecular weight".
[0051] The term "powder" appearing in the present invention means a powder or granular state that is basically free of water and other solvents. The term "powder" can also be basically interchangeable with "dry powder", which is used for the state in which the drag reducer is basically free of water or other solvents, and is also the preferred product state of the embodiments and technical solutions of the present invention.
[0052] In addition, the present invention may adopt an open-ended component definition method such as "including" or "comprising" to indicate that the embodiment of the present invention may include the main components used and may also include other auxiliary components. However, in a preferred embodiment of the present invention, it may only consist of the components defined in the present invention without including any other components, for example, it may no longer include other inorganic salts as demulsification or viscosity reduction auxiliary enhancers.
[0053] The low molecular weight drag reducer of the present invention may be a low molecular weight powdery salt-resistant drag reducer.
[0054] Test experiment of the present invention
[0055] Before beginning to describe the preparation experimental examples, the test process, standards, and characterization methods used in typical experiments of the present invention are briefly described.
[0056] 1. Test on drag reduction performance of low molecular weight powder drag reducer in high flow water system
[0057] In a typical test experiment, the drag reduction test process of this experiment is roughly described as follows:
[0058] The powder drag reducer is quantitatively dissolved in clean water to prepare a drag reducer solution of a specified concentration; the power device uses a screw pump to properly control the shear effect on the chain segment molecules. The test pipeline uses a circular tubular conveying device to simulate the pipeline state of actual oil field transportation. Pressure sensors and the flow state of the screw pump are installed on both sides of the test pipe section. The index of the pressure sensors at both ends of the test pipe section at different flow rates is recorded, and the pressure drop ΔP generated by the clean water and drag reducer solution flowing through the test pipe section at different flow rates is calculated;
[0059] In a typical test process, the drag reduction rate can be calculated by the following formula.
[0060]
[0061] Where K is the drag reduction rate, expressed in %; ΔP 水 It indicates the pressure drop when clean water flows through the test pipe section, expressed in MPa; ΔP 减阻 It indicates the pressure drop generated when a solution containing a specific drag reducer flows through the test pipe section, expressed in MPa.
[0062] In a typical experiment, 100g of the drag reducer prepared in the embodiment is weighed and added to a container containing 100L of water under stirring to prepare an aqueous solution of a powder drag reducer with a concentration of 0.1% by mass. After stirring, the drag reducer is completely dissolved within 1.5 minutes, meeting the mixing requirements of shale gas fracturing. The prepared drag reducer aqueous solution is added to the resistance test system, and the drag reduction rate of the corresponding drag reducer solution at a flow rate of 30L / min is measured. In the experiment, a 6.5mm round tube is used as the test pipe section, and the pressure drop caused by clean water and 0.1% by mass drag reducer aqueous solution flowing through the test pipe section is recorded, and the drag reduction rate is calculated according to the above formula.
[0063] 2. Viscosity and drag reduction effects of high viscosity heavy oil
[0064] In addition to the drag reducing effect on high-speed flowing water systems, the inventors have found in experiments that the low molecular weight powder drag reducer of the present invention also has a good and surprising viscosity reducing effect on high-viscosity heavy oil.
[0065] In a typical experiment, 50g of heavy oil with a viscosity of 1200000mPa.s is selected, 20g of 0.2wt% low molecular weight powder drag reducer solution prepared on site is added, and it is placed in a constant temperature water bath at 45°C, stirred at a rate of about 60rpm for 30 seconds, and then kept still for 15 minutes. Then the test tube is poured out, keeping the angle between the test tube and the table at 45°, and the oil in the test tube is poured out. By comparing the mass of crude oil in the test tube before and after pouring, the static viscosity reduction rate (d) is calculated. Typically, the static viscosity reduction rate can be calculated by the following formula:
[0066]
[0067] In the above formula, d represents the static viscosity reduction rate of heavy oil; m0 represents the mass of the test tube, in grams; m1 represents the mass of the heavy oil in the test tube, in grams; and m2 represents the mass of the test tube after the viscosity reduction effect occurs and the oil is poured out, in grams.
[0068] From the test results, we can see that if the viscosity reduction effect is better, there will be less oil remaining on the test tube wall after the oil product is discharged, resulting in the d value being closer to 1 (100%). Such a ratio value is used to representatively show the drag reduction effect of the tested heavy oil.
[0069] Example 1
[0070] This example describes the preparation process of a low molecular weight powder drag reducer.
[0071] Step 1) Preparation of low molecular weight polymer
[0072] Weigh 0.5 mol of 3-methacryloyl dopamine (component A1), and then determine the amounts of 3-methacryloyl dopamine, 1,4-diphenyl-1,3-butadiene (component A2), n-propanol, and purified water according to a molar ratio of 1:0.95:1.15:20;
[0073] Mixing 1,4-diphenyl-1,3-butadiene and n-propanol and stirring them thoroughly to obtain a 1,4-diphenyl-1,3-butadiene mixed liquid;
[0074] After mixing 3-methacryloyl dopamine with purified water, add the mixture into the above 1,4-diphenyl-1,3-butadiene solution under stirring;
[0075] Azobisisobutyronitrile was added in an amount of 0.5 mol% of the total molar amount of the raw materials as a polymerization initiator, and an inert gas was introduced for 1 hour to remove oxygen components;
[0076] The reaction was heated at 65° C. for 16 hours to obtain a viscous liquid with a molecular weight of 36,500 (viscosity average molecular weight). The low molecular weight polymer drag reducing component of this embodiment can be represented by the following molecular formula.
[0077]
[0078] Due to the process parameter interval of the present invention and the characteristics of the polymer, the viscosity average molecular weight is unlikely to accurately determine the degree of polymerization of each individual molecule, so the value of n that meets the above molecular weight range is approximately between 80 and 95.
[0079] Step 2) Preparation of auxiliary components
[0080] Sodium 2-acrylamido-2-methylpropanesulfonate (e.g., 100 g in the test, component B1) and sodium acrylate (component B2) are dissolved in deionized water at a mass ratio of 10:3, stirred thoroughly, sodium bicarbonate (or sodium hydroxide solution with a molar concentration of 0.1 mol / L) is added to adjust the pH value to 6.5, inert gas (N2) is introduced for 1 hour to remove oxygen components, azobisisobutylimidazoline hydrochloride is added at 45°C as an initiator (inorganic compound potassium persulfate plus sodium bisulfite can also be used as an initiator), the amount of initiator added is 0.5% of the total monomer mass, and the reaction is continued for 2 hours to obtain a viscous auxiliary component; its viscosity average molecular weight is measured to be 68500. The obtained auxiliary component can be described by the following chemical structure:
[0081]
[0082] The value range of m that satisfies the above molecular weight is approximately between 220 and 250.
[0083] Step 3) Post-mixing treatment steps
[0084] The low molecular weight polymer drag reducing component obtained in step 1) and the auxiliary agent component obtained in step 2) are mixed in a mass ratio of 8:1 (component ratio C), and deionized water of 1.5 times the total mass of the two is added and stirred. After stirring, the composition is filtered, dried, and granulated. The low molecular weight powder drag reducing agent is sent to a rotary dryer, the temperature is controlled at 90°C, and the required drying time is 1 to 1.5 hours. The dried solid matter is sent to a vibrating fluidized bed for further drying (the vibrating fluidized bed controls the temperature at 85°C), and is sieved after vibration drying. A 70-mesh sieve is used for sieving, and the low molecular weight powder drag reducing agent of this embodiment is obtained after sieving. The low molecular weight powder drag reducing agent is marked as E 10 .
[0085] Example 2
[0086] In Example 2, the same process and raw materials as in Example 1 are used, except that the proportions of the raw material components in the preparation of the low molecular weight polymer and the auxiliary component are adjusted, so as to appropriately adjust the average molecular weight of the corresponding product obtained. As shown in the following table:
[0087] Table 2: Main experimental parameters of Example 2
[0088]
[0089] The inventors have found in experiments that when the components of A1 and A2, and the components of B1 and B2 are closer, the molecular weight of the corresponding synthesis will decrease accordingly. In the experiment of the present invention, adjusting the ratio of each component is not the only way to adjust the molecular weight of the synthesized polymer. For example, the molecular weight of the low molecular weight polymer and the auxiliary component polymer can also be adjusted by adjusting the synthesis temperature, the ratio of the initiator used, and the duration of the core reaction.
[0090] It can be seen from the experimental examples of the present invention and the subsequent comparative tests that the embodiments of the present invention preferably adjust the molecular weight of the low molecular weight polymer to greater than 30,000 and up to 60,000, for example, between 32,000 and 50,000, preferably, the molecular weight of the low molecular weight polymer component is adjusted to between 32,000 and 40,000. For the auxiliary component, its molecular weight is adjusted to between 50,000 and 80,000, preferably, the molecular weight is adjusted to between 55,000 and 70,000.
[0091] Embodiment 3:
[0092] Example 3 uses the same process and similar raw materials as Example 1, except that 1,1-diphenyl-1,3-butadiene is used instead of 1,4-diphenyl-1,3-butadiene. From the perspective of molecular structure, 1,1-diphenyl-1,3-butadiene is different from 1,4-diphenyl-1,3-butadiene in that the two phenyl groups are located on the same carbon atom. After polymerization, the density and distribution of the benzene rings in the polymer will be more concentrated. The low molecular weight powder drag reducer obtained in Example 3 is marked as sample E. 30 .
[0093] Comparative Example 1:
[0094] On the basis of the above embodiments, in order to highlight the concept and features of the invention, the inventors also conducted the following experiments for comparison.
[0095] Comparative Example C 10 : In C 10 In the experiment, the same preparation process and parameters as those in the corresponding steps of Example 1 were used, but only low molecular weight polymer was used as the low molecular weight powder drag reducer without adding auxiliary agent components. 10 In the experiment, the preparation of the auxiliary agent component in step 2) of Example 1 was not performed. After the synthesis step in step 1) was completed, the corresponding steps of deionized water stirring, filtering, drying and granulation in step 3) were directly performed.
[0096] Comparative Example C 11: The same preparation process and parameters as those in the corresponding steps of Example 1 were used, but no low molecular weight polymer was used as the low molecular weight powder drag reducer, and only the auxiliary agent component was synthesized. That is, in C 11 In the experiment, the preparation of the auxiliary agent component in step 1) of Example 1 was not performed, and the synthesis step of step 2) was directly performed. After that, the corresponding steps of stirring with deionized water, filtering, drying, and granulation in step 3) were directly performed to obtain the corresponding experimental product.
[0097] Comparative Example 2:
[0098] This test series, based on Example 1, adjusted / changed the molecular weight distribution of each component. As shown in the following table:
[0099] Table 3: Main experimental parameters of comparative example 2
[0100]
[0101] Note: According to the description in Example 1, the component ratio C represents the mass ratio of the low molecular weight polymer drag reducing component synthesized in step 1) and the auxiliary agent component obtained in step 2).
[0102] Test results and analysis
[0103] First, the inventors conducted water system fluidity drag reduction tests on typical experimental examples and comparative examples. The results can be found in Figure 1 As can be seen from the figure, E 10 and E 20 The best test results in the water system drag reduction experiment. Under the high flow rate of 30L / min, the aqueous solution prepared by adding only the powder drag reducer prepared in the example with a concentration of 0.1% by mass achieved a drag reduction efficiency (K) of more than 75% in a short time of 30 to 35 seconds.
[0104] In E 30 The experiment also achieved an effective drag reduction effect, but the curve rise time was slightly slower than that of E 10 and E 20 .
[0105] In C 10 During the experiment, although a certain drag reduction effect was achieved in the flowing water system, using only the low molecular weight powder drag reducer of step 1 could not achieve a drag reduction effect of more than 50% under large flowing water conditions.
[0106] The water flow drag reduction rate (K, 35 seconds) and the viscosity reduction and drag reduction efficiency (d) of high viscosity heavy oil of other corresponding experimental examples are shown in the following table:
[0107] Table 4: Drag reduction rate of water flow (K) and viscosity reduction and drag reduction efficiency of high viscosity heavy oil (d)
[0108]
[0109] With respect to the above test results, the inventors do not expect to be constrained by any theoretical explanation or constraint. However, the raw materials, processes, and various low-molecular polymers prepared by the present invention can be analyzed to obtain the principles and reasons for the different experimental results. In the preferred embodiment of the present invention, a combination of low-molecular polymers and auxiliary components should be used. When only one of the components is used, satisfactory viscosity and drag reduction effects of high-velocity water systems and high-oil systems cannot be achieved. One of the possibilities that the inventors believe is that the evenly distributed benzene ring structure in the molecular structure of the low-molecular polymer of the present invention helps the drag reducer component to form a grid structure to cut off the flowing water and high-viscosity oil components that cause resistance. At the same time, the Na ions attached to the low-molecular-weight polymer grid in the auxiliary component and the hydroxyl groups (OH) on the benzene rings in the low-molecular-weight polymer component form a weakly connected network structure with charged ionic compound characteristics during the preparation process after mixing. This structure helps to quickly destroy the adhesion brought by the heavy oil structure. When only one of the components is used (for example, C 10 and C 11 ), unable to form a benzene ring-hydroxyl-polymer Na ion oil-breaking network, so the oil-breaking effect on heavy viscous oil (for example, viscosity up to 1.2 million) is reduced.
[0110] The inventors also found that when using C 10 During the process, it was found that the crushing progress was significantly slowed down in the solidification and crushing process of step 3), and agglomeration occurred, and the crushing particle size was uneven. This shows that the auxiliary process also assists the solidification and crushing state when the two components are mixed, preventing the individual polymer components from being crushed unfavorably. The advantages of the low molecular weight powder drag reducer in an effective powder (dry powder) state will be described in more detail below.
[0111] The low molecular weight polymer of the present invention is beneficial to improve the viscosity reduction and drag reduction effect of high-speed flowing water system and heavy oil system, so it is necessary to control the average molecular weight of each component. The inventor found that when the molecular weight of the low molecular weight polymer component (first component) is relatively large (such as greater than 60,000) or less than 30,000, the viscosity reduction effect of the flowing water system and heavy oil is deteriorated. When the molecular weight of the auxiliary component is too large (such as greater than 100,000), the total viscosity reduction and drag reduction effect is also reduced. Considering various factors, the combination of the appropriate two component molecular weights is easy to effectively form a suitable oil-breaking network. For example, when the molecular weight of a single auxiliary component is too large, it is not conducive to the formation of an effective weak molecular connection network (sulfate group Na and phenyl hydroxyl) in large quantities. Therefore, the heavy oil breaking effect is deteriorated, and it is not suitable as the most preferred implementation scheme for heavy oil viscosity reduction.
[0112] In addition, when 1,1-diphenyl-1,3-butadiene is used to replace the raw material 1,4-diphenyl-1,3-butadiene, a certain drag reduction and viscosity reduction effect can also be achieved. However, it is worth noting that the inventors found that since the two phenyl groups of 1,1-diphenyl-1,3-butadiene are located on the same carbon atom from the perspective of the molecular structure, after polymerization, the density and distribution of the benzene rings in the polymer will be more concentrated, which is not conducive to forming a uniform drag reduction and oil breaking network. Therefore, a more evenly distributed benzene ring and network structure is a further preferred solution in the embodiment of the present invention.
[0113] Example 4: Application of powdered low molecular weight polymer drag reducing composition
[0114] In the embodiments of the present invention, the inventors emphasize the use of a powder (dry powder) system of a low molecular weight polymer drag reducing composition. The inventors believe that it is necessary to emphasize the drag reducing composition in the powder (dry powder) state. In the actual oil well drilling application using a powder as a polymer drag reducing composition, rather than using an emulsion or a formulated drag reducing composition, at least the following advantages are achieved in industrial applications. The advantages are some of the key points summarized by the inventors in large-scale industrial applications. At least the following advantages are included:
[0115] 1) Solid polymers with 100% active ingredients can be delivered to the job site, which can reduce the transportation volume of drag reducers / thickeners by 50-60%; 2) During the construction of oil wells on site, drag reducer dry powder (powder) can be directly transported through pipelines between tank trucks without any auxiliary operations such as lifting, eliminating the potential risks of related lifting operations (such as falling, chemical leakage, personal injury and equipment damage); 3) On-site operation ash tanks (12-20m³) can be transported with the assistance of high-pressure gas, and can be loaded and unloaded in a very short time (such as 20-30 minutes) without any forklift or crane loading and transportation operations; 4) On-site operation equipment occupies a small area. In typical oil well construction, the size of the main mixing truck can be only 6.0m 2.2m 2.0m, ash tank skid size is 6m 2.0m 2.5m; 5) It can also help solve the impact of the stability, shelf life, and harsh environment (extreme cold, heat) of traditional emulsion polymer thickener products on construction efficiency; 6) Salt resistance. The inventors were also surprised to find that the specific low-molecular polymer powder of the present invention, as a polymer drag-reducing composition, has good salt resistance, that is, at the construction site, it can be prepared with backflow liquid, and the salt resistance can reach 200,000 mineralization (0 to 200,000), and calcium and magnesium ions can reach 20,000 (0 to 20,000).
[0116] According to the implementation scheme and technical contents recorded in the specification of the present invention, the present invention can at least provide the following technical solutions: Although the present disclosure includes specific embodiments, it is obvious to those skilled in the art that various formal and detailed replacements or changes can be made to these embodiments without departing from the gist and scope of the invention of the present claims and their equivalent technical solutions. The embodiments described herein should be considered to be illustrative only and not for the purpose of limitation. The description of the features and aspects in each embodiment is considered to be applicable to similar features and aspects in other embodiments. Therefore, the scope of the present disclosure should not be limited by the specific description, but by the technical solutions of the claims, and all changes within the scope of the claims and their equivalents are interpreted as being included in the technical solutions of the present disclosure.
Claims
1. A low molecular weight powder salt-resistant drag reducer, characterized in that: The low molecular weight powder drag reducer comprises a low molecular weight polymer having an average molecular weight between 30,000 and 60,000, wherein the low molecular weight polymer is polymerized by methacryloyl dopamine and diphenyl-1,3-butadiene in the presence of a polymerization initiating component and under heating; and The diphenyl-1,3-butadiene is 1,4-diphenyl-1,3-butadiene, and the low molecular weight polymer is represented by the following molecular formula: ; And wherein the low molecular weight powder salt-resistant drag reducer also includes an auxiliary component, the auxiliary component is polymerized by sodium 2-acrylamido-2-methylpropane sulfonate and sodium acrylate in the presence of an initiator at 40° C. to 50° C., the average molecular weight of the auxiliary component is 50,000 to 80,000, and the mass ratio of the low molecular weight polymer to the auxiliary component is 5:1 to 10:1; And, the low molecular weight polymer is obtained by the following preparation process: 1) Prepare 3-methacryloyl dopamine, and then determine the amount of 3-methacryloyl dopamine, 1, 4-diphenyl-1,3-butadiene, n-propanol, and purified water according to the molar ratio of 1: (0.90-1.1): (1-1.2): (10-30); 2) mixing the 1,4-diphenyl-1,3-butadiene and n-propanol and stirring them thoroughly to obtain a 1,4-diphenyl-1,3-butadiene mixed liquid; 3) Mix 3-methacryloyl dopamine with purified water, and add it into the above 1,4-diphenyl-1,3-butadiene mixture under stirring; 4) adding a polymerization initiator in an amount of 0.1 mol% to 1 mol% of the total molar amount of the raw materials, and introducing an inert gas for 0.5 to 2 hours; 5) heating the reaction at 60 to 80° C. for 10 to 20 hours to obtain the low molecular weight polymer component.
2. The low molecular weight powder salt-resistant drag reducer according to claim 1, characterized in that: The adjuvant component is described by the following chemical structure: 。 3. The low molecular weight powder salt-resistant drag reducer according to claim 1, characterized in that: The low molecular weight powder salt-resistant drag reducer is in a dry powder state.
4. The low molecular weight powder salt-resistant drag reducer according to claim 1, characterized in that: The auxiliary agent component is obtained by the following preparation process: Sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate are dissolved in deionized water at a mass ratio of 10:(1-5), and the mixture is stirred thoroughly. The pH value is adjusted to be in the range of 6 to 7, and an inert gas is introduced for 0.5 to 2 hours. An initiator is added at 40° C. to 50° C., and the amount of the initiator added is 0.5% of the total mass of sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate. The reaction is continued for 1 to 3 hours to obtain the auxiliary agent component.
5. The low molecular weight powder salt-resistant drag reducer according to claim 1, characterized in that: The low molecular weight powder salt-resistant drag reducer is obtained by treating the low molecular weight polymer and the auxiliary agent component by a post-mixing treatment step, wherein the post-mixing treatment step comprises: The low molecular weight polymer and the auxiliary agent component are mixed in a mass ratio of 5:1 to 10:1, and deionized water of 1 to 3 times the total mass of the two is added for stirring. After stirring, the composition is filtered and dried. In the drying step, the mixture is sent to a rotary dryer for 0.5 to 3 hours, and the dried solid matter is then sent to a vibrating fluidized bed for further drying. After vibration drying, it is sieved to obtain the low molecular weight powder salt-resistant drag reducer.
6. A method for preparing a low molecular weight powder salt-resistant drag reducer, characterized in that: The method comprises the following first step, second step and third step: First step: Preparation of low molecular weight polymer Weigh 3-methacryloyl dopamine, and then determine the amount of 3-methacryloyl dopamine, 1, 4-diphenyl-1,3-butadiene, n-propanol, and purified water according to the molar ratio of 1: (0.90-1.1): (1-1.2): (10-30); The 1,4-diphenyl-1,3-butadiene and n-propanol are mixed and stirred sufficiently to obtain a 1,4-diphenyl-1,3-butadiene mixed liquid; After mixing 3-methacryloyl dopamine with purified water, add the mixture into the above 1,4-diphenyl-1,3-butadiene solution under stirring; Add a polymerization initiator in an amount of 0.1 mol% to 1 mol% of the total molar amount of the raw materials, and introduce an inert gas for 0.5 to 2 hours; heating the reaction at 60 to 80° C. for 10 to 20 hours, and measuring the average molecular weight to obtain the low molecular weight polymer; Second step: preparation of auxiliary components Dissolve sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate in deionized water at a mass ratio of 10:(1-5), stir thoroughly, adjust the pH value to a range of 6 to 7, introduce an inert gas for 0.5 to 2 hours, add an initiator at 40° C. to 50° C., the amount of the initiator added is 0.5% of the total mass of sodium 2-acrylamide-2-methylpropane sulfonate and sodium acrylate, continue the reaction for 1 to 3 hours, and then measure the average molecular weight to obtain the auxiliary agent component; Step 3: Post-mixing process The low molecular weight polymer and the auxiliary agent component are mixed in a mass ratio of 5:1 to 10:1 to obtain a mixture, and deionized water of 1 to 3 times the total mass of the two is added for stirring. After stirring, the composition is filtered and dried. In the drying step, the mixture is sent to a rotary dryer for 0.5 to 3 hours. The dried solid matter is sent to a vibrating fluidized bed for further drying, and sieved after vibration drying to obtain the low molecular weight powder salt-resistant drag reducer.
Citation Information
Cited By
Low-molecular salt-resistant thickening agent and preparation method thereof
CN120988216A
Low-molecular salt-resistant thickening agent and preparation method thereof
CN120988216B