A fully biodegradable agricultural mulch film

By using marinate and cross-linking treatment of materials such as maleic acid, wood chips, cotton fibers and sodium carboxymethylcellulose in agricultural mulch, a fully biodegradable agricultural mulch with high mechanical properties and water resistance was prepared, and the solution was solved The problem of difficulty in degrading traditional mulch reduces the risk of pollution and improves the safety of the agricultural ecological environment.

CN118684944BActive Publication Date: 2024-12-03FUJIAN MANSHANHONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172703.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing agricultural mulching materials are difficult to degrade, resulting in soil and water pollution, and lack of effective recycling and treatment methods, which affects the agricultural ecological environment.

Method used

By using the preparation method of fully biodegradable agricultural mulch, by beating and crosslinking materials such as maleic acid, wood chips, cotton fibers and sodium carboxymethylcellulose, it forms a composite material with high mechanical properties and water resistance. And use glutaraldehyde and borax to enhance their biodegradability.

Benefits of technology

It achieves rapid biodegradation of mulch film, reduces the risk of pollution, and improves the mechanical properties and water resistance of the materials, solving the problem that traditional mulch films are difficult to degrade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a fully biodegradable agricultural mulch film, and relates to the technical field of agricultural mulch films. The invention utilizes sawdust and cotton fibers for pulping treatment, the sawdust swells and brooms, and the hydrogen bonds exposed on the surface of the cotton fibers increase with the degree of beating, so that the binding force between the two is enhanced, thereby enhancing the mechanical properties of the matrix, and then, as a reinforcement, it is cross-linked with sodium carboxymethyl cellulose, and through glutaraldehyde and borax, the chance of cross-linking of sodium carboxymethyl cellulose molecules is increased, so that the molecular weight of the system is increased, and a small amount of lignin in the sawdust can be filled into the gaps in the cellulose film, thereby improving the rigidity of the matrix, thereby being closely connected with the reinforcement fibers, reducing the number of hydroxyl groups in the matrix, improving water resistance and enhancing mechanical properties, and achieving full biodegradability of the mulch film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of agricultural mulch films, in particular to a fully biodegradable agricultural mulch film. Background Art

[0002] As a type of plastic material, mulch plays an important role in modern agriculture, such as preventing weed growth, preventing water evaporation and soil erosion, and maintaining soil temperature. Mulch cultivation technology can keep the soil warm and moist, effectively increasing crop yields. It is currently widely used in early seedling cultivation and growth of crops, and is known as the "white revolution in agriculture." In addition, plastic mulch covering crops also provides physical protection for crops against adverse growth conditions such as bad weather, birds, and pests, reducing the use of pesticides and promoting crop growth.

[0003] The annual increase in plastic film production and the expansion of coverage area have brought increased income and production to agriculture, but have also brought serious white pollution to agriculture.

[0004] The earliest agricultural film used in my country's agriculture was polyvinyl chloride film, and then gradually developed into linear low-density polyethylene and low-density polyethylene film. The molecular weight of these materials is about 25,000-30,000 and the molecular structure is stable. It is extremely difficult to degrade and can exist in the soil for 200 to 400 years. Once this type of film material decomposes in the soil, it will produce toxic substances that pollute the soil and water bodies. In addition, the remaining film fragments are extremely difficult to clean. The long-term residue of film in the soil will cause soil compaction, block the root system's absorption of water, and thus lead to reduced crop yields and livestock death by accidental ingestion. Most parts of my country have a low degree of agricultural mechanization. In some areas, the labor force is tight, and the residual film cannot be collected in time after the crop harvest, resulting in more and more serious pollution from residual film, affecting the rural ecological environment. If the recycled residual film cannot be effectively treated in time or is disposed of improperly, it will pollute the environment again. At present, my country mainly treats the recycled residual film by incineration and landfill. Incineration of residual film will cause air pollution, and landfill cannot effectively solve the problem of residual film being difficult to degrade. my country has not yet established complete regulations on pollution caused by agricultural film and standards for soil residual film rates. In summary, it can be seen that the development of new degradable film materials is particularly important for solving my country's agricultural film pollution problem. Summary of the invention

[0005] The purpose of the present invention is to provide a fully biodegradable agricultural mulch film to solve the problems existing in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a fully biodegradable agricultural mulch film, comprising the following preparation steps:

[0007] (1) Maleic acid and deionized water are mixed and dissolved at 50-65°C until the solution becomes transparent, pretreated sawdust and cotton fiber are added, the temperature is raised to 90-110°C, and the mixture is stirred at 350-500 rpm for 30-70 min for pulping, and then polyamide polyoxychloropropane resin is added, and the mixture is stirred at 100-200 rpm for 15-50 min under an ultrasonic frequency of 21 kHz to obtain a composite reinforcement;

[0008] (2) Sodium carboxymethyl cellulose and deionized water are mixed, stirred at 100-200 rpm for 20-40 min, heated to 70-90 °C, the composite reinforcement is added, stirring is continued for 1-2 h, borax is added, and a 3 wt % glutaraldehyde aqueous solution is added dropwise, stirred at 50-70 °C and 200-350 rpm for 1-2 h, then ultrasonically degassed, and allowed to stand for 3-5 h, cast in a template, and dried at room temperature for 3-6 h to obtain a fully biodegradable agricultural mulch film.

[0009] Furthermore, the preparation method of the pretreated sawdust in step (1) is as follows: the poplar wood sawdust is crushed to pass through a 10-20 mesh sieve, immersed in a 4 wt % sodium hydroxide aqueous solution, heated to 85° C., alkalized for 1-2 h, then immersed in a 1.7 wt % hydrogen peroxide aqueous solution, reacted for 1-2 h, and finally rinsed with deionized water for 5-8 times, and dried at 60-80° C. for 4-8 h.

[0010] Furthermore, the cotton fiber in step (1) has a length of 0.1 to 0.5 cm.

[0011] Furthermore, the beating in step (1) is performed to a beating degree of 40-50° SR.

[0012] Furthermore, the power of the ultrasound in step (1) is 400-500W.

[0013] Furthermore, in step (1), the mass ratio of maleic acid, deionized water, pretreated wood chips, cotton fiber, and polyamide polyoxychloropropane resin is 50:50:5:1-3:0.1.

[0014] Furthermore, the dripping rate of the 3 wt % glutaraldehyde aqueous solution in step (2) is 10-40 mL / min.

[0015] Furthermore, the frequency of the ultrasonic degassing in step (2) is 21-25 kHz and the time is 20-60 min.

[0016] Furthermore, the thickness of the fully biodegradable agricultural mulch film in step (2) is 0.01-0.1 mm.

[0017] Furthermore, in step (2), the mass ratio of sodium carboxymethyl cellulose, deionized water, composite reinforcement, borax, and 3 wt% glutaraldehyde aqueous solution is 1-2:100:20-70:3:1.5.

[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0019] The present invention utilizes sawdust and cotton fiber for pulping treatment. With the increase of temperature, the sawdust swells and brooms, so that the number of single fibers increases, and the separated lignin undergoes esterification reaction with a carboxyl group in maleic acid, while the hydrogen ion of the other carboxyl group in maleic acid will not be ionized due to the intramolecular hydrogen bonding, and the carboxyl group can be free in the fluid, thereby improving the dispersion performance of the matrix material. At the same time, the hydrogen bonds exposed on the surface of the cotton fiber also increase with the beating degree, so that the bonding force between the two fibers is enhanced, and the cationic charge provided by the wet strength agent is strongly adsorbed with the anionic charge of the fiber, thereby enhancing the mechanical properties of the matrix. Then, as a reinforcement, it is cross-linked with sodium carboxymethyl cellulose, wherein the cross-linking agent is glutaraldehyde and borax, and the glutaraldehyde and carboxymethyl cellulose The hydroxyl groups of sodium cellulose molecules undergo etherification reaction to form a cross-linked spatial network structure, which increases the molecular weight of the system and enhances its density. A small amount of lignin in the wood chips can be filled into the voids of the cellulose film, which helps to transfer stress and thus improve the rigidity of the matrix. When the content of borax molecules increases, the chances of cross-linking of sodium carboxymethyl cellulose molecules also increase, so that they can be tightly connected with the reinforcement fibers, reducing the number of hydroxyl groups in the matrix, improving water resistance and enhancing mechanical properties. Borax hydrolyzes to produce hydroxyl groups of tetrahydroxyborate ions, which connect the sodium carboxymethyl cellulose molecules, thereby forming more cross-linked chemical bonds, enhancing the intramolecular interaction between the filler and the matrix, and achieving the full biodegradability of the mulch film. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0021] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the fully biodegradable agricultural mulch films prepared in the following examples are as follows:

[0022] Biodegradability: The same size of the examples and comparative examples were taken according to ISO 16929 to test the biodegradability of the samples on the 100th day.

[0023] Water resistance: Take the same size of the embodiment and the comparative example, immerse the sample in deionized water at 25°C according to GB / T1034, take it out after 24 hours, and test its water absorption rate.

[0024] Mechanical properties: The yield stress and Elmendorf tear strength of the examples and comparative examples of the same size were tested according to JIS K7127 and ISO 6383-2, respectively.

[0025] Example 1; (1) Poplar wood chips were crushed until they passed through a 10-mesh sieve, immersed in a 4 wt % sodium hydroxide aqueous solution, heated to 85° C., alkalized for 1 h, then immersed in a 1.7 wt % hydrogen peroxide aqueous solution, reacted for 1 h, and finally rinsed with deionized water 5 times, and dried at 60° C. for 4 h to obtain pretreated wood chips; maleic acid and deionized water were mixed, dissolved at 50° C. until the solution was transparent, pretreated wood chips and cotton fibers with a length of 0.1 cm were added, heated to 90° C., stirred at 350 rpm for 30 min, and beaten to a beating degree of 40° SR, then polyamide polychlorohydrin resin was added, and stirred at 100 rpm for 15 min under the conditions of an ultrasonic frequency of 21 kHz and a power of 400 W to obtain a composite reinforcement; the mass ratio of maleic acid, deionized water, pretreated wood chips, cotton fibers with a length of 0.1 cm, and polyamide polychlorohydrin resin was 50:50:5:1:0.1;

[0026] (2) Sodium carboxymethyl cellulose and deionized water were mixed, stirred at 100 rpm for 20 min, heated to 70°C, a composite reinforcement was added, the stirring was continued for 1 h, borax was added, and a 3 wt % glutaraldehyde aqueous solution was added dropwise at 10 mL / min, stirred at 50°C and 200 rpm for 1 h, and then ultrasonic degassing was performed at a frequency of 21 kHz and a time of 20 min. Then, the mixture was allowed to stand for 3 h, cast in a template, and dried at room temperature for 3 h to obtain a fully biodegradable agricultural mulch film with a thickness of 0.01 mm; the mass ratio of the sodium carboxymethyl cellulose, deionized water, composite reinforcement, borax, and 3 wt % glutaraldehyde aqueous solution was 1:100:20:3:1.5.

[0027] Example 2: (1) Poplar wood chips were crushed until they passed through a 15-mesh sieve, immersed in a 4 wt% sodium hydroxide aqueous solution, heated to 85°C, alkalized for 1.5 h, then immersed in a 1.7 wt% hydrogen peroxide aqueous solution, reacted for 1.5 h, and finally rinsed with deionized water 7 times and dried at 70°C for 6 h to obtain pretreated wood chips; maleic acid and deionized water were mixed and dissolved at 58°C until the solution was transparent, pretreated wood chips and cotton fibers with a length of 0.2 cm were added, and the temperature was raised to 100°C. ℃, 430rpm stirring for 50min, beating treatment to a beating degree of 45°SR, then adding polyamide polychlorohydrin resin, stirring at 150rpm for 30min under the conditions of ultrasonic frequency of 21kHz and power of 450W, to obtain a composite reinforcement; the mass ratio of maleic acid, deionized water, pretreated sawdust, cotton fiber with a length of 0.2cm, and polyamide polychlorohydrin resin is 50:50:5:2:0.1;

[0028] (2) Sodium carboxymethyl cellulose and deionized water were mixed, stirred at 150 rpm for 30 min, heated to 80° C., a composite reinforcement was added, and stirring was continued for 1.5 h. Borax was added, and a 3 wt % glutaraldehyde aqueous solution was added dropwise at 30 mL / min. The mixture was stirred at 60° C. and 270 rpm for 1.5 h. Ultrasonic degassing was then performed at a frequency of 22 kHz for 40 min. The mixture was allowed to stand for 4 h, cast in a template, and dried at room temperature for 5 h to obtain a fully biodegradable agricultural mulch film with a thickness of 0.05 mm. The mass ratio of the sodium carboxymethyl cellulose, deionized water, composite reinforcement, borax, and 3 wt % glutaraldehyde aqueous solution was 1.5:100:50:3:1.5.

[0029] Example 3; (1) Poplar wood chips were crushed until they passed through a 20-mesh sieve, immersed in a 4 wt % sodium hydroxide aqueous solution, heated to 85° C., alkalized for 2 h, then immersed in a 1.7 wt % hydrogen peroxide aqueous solution, reacted for 2 h, and finally rinsed with deionized water for 8 times, and dried at 80° C. for 8 h to obtain pretreated wood chips; maleic acid and deionized water were mixed, dissolved at 65° C. until the solution became transparent, pretreated wood chips and cotton fibers with a length of 0.5 cm were added, heated to 110° C., stirred at 500 rpm for 70 min, and beaten to a beating degree of 50° SR, then polyamide polychlorohydrin resin was added, and stirred at 200 rpm for 50 min under the conditions of an ultrasonic frequency of 21 kHz and a power of 500 W to obtain a composite reinforcement; the mass ratio of maleic acid, deionized water, pretreated wood chips, cotton fibers with a length of 0.5 cm, and polyamide polychlorohydrin resin was 50:50:5:3:0.1;

[0030] (2) Sodium carboxymethyl cellulose and deionized water were mixed, stirred at 200 rpm for 40 min, heated to 90°C, a composite reinforcement was added, stirred for 2 h, borax was added, and a 3 wt % glutaraldehyde aqueous solution was added dropwise at 40 mL / min, stirred at 70°C and 350 rpm for 2 h, and then ultrasonic degassing was performed at a frequency of 25 kHz and a time of 60 min. Then, the mixture was allowed to stand for 5 h, cast in a template, and dried at room temperature for 6 h to obtain a fully biodegradable agricultural mulch film with a thickness of 0.1 mm; the mass ratio of the sodium carboxymethyl cellulose, deionized water, composite reinforcement, borax, and 3 wt % glutaraldehyde aqueous solution was 2:100:70:3:1.5.

[0031] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: maleic acid and deionized water are mixed and dissolved at 58°C until the solution is transparent, cotton fiber with a length of 0.2 cm is added, the temperature is raised to 100°C, and stirred at 430rpm for 50min, and pulping is performed until the beating degree is 45°SR, and then polyamide polychlorohydrin resin is added, and stirred at 150rpm for 30min under the conditions of ultrasonic frequency of 21kHz and power of 450W to obtain a composite reinforcement; the mass ratio of maleic acid, deionized water, cotton fiber with a length of 0.2 cm, and polyamide polychlorohydrin resin is 50:50:2:0.1; the remaining steps are the same as Example 2.

[0032] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is different, and step (1) is changed to: the poplar wood chips are crushed to pass through a 15-mesh sieve, immersed in a 4wt% sodium hydroxide aqueous solution, heated to 85°C, alkalized for 1.5h, then immersed in a 1.7wt% hydrogen peroxide aqueous solution, reacted for 1.5h, and finally rinsed with deionized water 7 times, dried at 70°C for 6h, to obtain pretreated wood chips; maleic acid and deionized water are mixed, dissolved at 58°C until the solution is transparent, and pretreated The sawdust was processed, the temperature was raised to 100°C, and the mixture was stirred at 430 rpm for 50 min to perform pulping treatment until the pulping degree was 45°SR. Subsequently, polyamide polychlorohydrin resin was added, and the mixture was stirred at 150 rpm for 30 min under the conditions of ultrasonic frequency of 21 kHz and power of 450 W to obtain a composite reinforcement. The mass ratio of the maleic acid, deionized water, pretreated sawdust, and polyamide polychlorohydrin resin was 50:50:5:0.1. The remaining steps were the same as those in Example 2.

[0033] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that step (1) is different, and step (1) is changed to: the poplar wood chips are crushed to pass through a 15-mesh sieve, immersed in a 4wt% sodium hydroxide aqueous solution, heated to 85°C, alkalized for 1.5h, then immersed in a 1.7wt% hydrogen peroxide aqueous solution, reacted for 1.5h, and finally rinsed with deionized water 7 times, dried at 70°C for 6h, to obtain pretreated wood chips; the deionized water, pretreated wood chips and cotton fibers with a length of 0.2cm are heated to 1 00℃, 430rpm stirring for 50min, beating treatment is carried out to the beating degree of 45°SR, then polyamide polychlorohydrin resin is added, and under the conditions of ultrasonic frequency of 21kHz and power of 450W, stirring at 150rpm for 30min to obtain a composite reinforcement; the mass ratio of the deionized water, pretreated wood chips, cotton fiber with a length of 0.2cm, and polyamide polychlorohydrin resin is 50:5:2:0.1; the remaining steps are the same as those in Example 2.

[0034] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that there is no step (1), and step (2) is changed to: sodium carboxymethyl cellulose and deionized water are mixed, stirred at 150rpm for 30min, heated to 80°C, borax is added, and 3wt% glutaraldehyde aqueous solution is added dropwise at 30mL / min, stirred at 60°C and 270rpm for 1.5h, followed by ultrasonic degassing at a frequency of 22kHz and a time of 40min, then allowed to stand for 4h, cast in a template, and dried at room temperature for 5h to obtain a fully biodegradable agricultural mulch film with a thickness of 0.05mm; the mass ratio of the sodium carboxymethyl cellulose, deionized water, borax, and 3wt% glutaraldehyde aqueous solution is 1.5:100:3:1.5; the remaining steps are the same as Example 2.

[0035] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that step (2) is different. Step (2) is changed to: mix sodium carboxymethyl cellulose and deionized water, stir at 150 rpm for 30 min, heat to 80°C, add the composite reinforcement, continue stirring for 1.5 h, add borax, and add 3 wt% glutaraldehyde aqueous solution dropwise at 30 mL / min, stir at 60°C and 270 rpm for 1.5 h, then perform ultrasonic degassing at a frequency of 22 kHz and a time of 40 min, then let it stand for 4 h, cast it in a template, and dry it at room temperature for 5 h to obtain a fully biodegradable agricultural mulch film with a thickness of 0.05 mm; the mass ratio of the sodium carboxymethyl cellulose, deionized water, composite reinforcement, borax, and 3 wt% glutaraldehyde aqueous solution is 1.5:100:50:1:1.5; the remaining steps are the same as Example 2.

[0036] Comparative Example 6: The difference between Comparative Example 6 and Example 2 is that step (2) is different. Step (2) is changed to: mix sodium carboxymethyl cellulose and deionized water, stir at 150 rpm for 30 min, heat to 80°C, add the composite reinforcement, continue stirring for 1.5 h, add 3 wt% glutaraldehyde aqueous solution at 30 mL / min, stir at 60°C and 270 rpm for 1.5 h, then perform ultrasonic degassing at a frequency of 22 kHz and a time of 40 min, then let it stand for 4 h, cast it in a template, and dry it at room temperature for 5 h to obtain a fully biodegradable agricultural mulch film with a thickness of 0.05 mm; the mass ratio of the sodium carboxymethyl cellulose, deionized water, composite reinforcement, and 3 wt% glutaraldehyde aqueous solution is 1.5:100:50:1.5; the remaining steps are the same as Example 2.

[0037] Comparative Example 7: The difference between Comparative Example 7 and Example 2 is that step (2) is different. Step (2) is changed to: mix sodium carboxymethyl cellulose and deionized water, stir at 150 rpm for 30 min, heat to 80°C, add the composite reinforcement, continue stirring for 1.5 h, add borax, stir at 60°C and 270 rpm for 1.5 h, then perform ultrasonic degassing at a frequency of 22 kHz and a time of 40 min, then let it stand for 4 h, cast it in a template, and dry it at room temperature for 5 h to obtain a fully biodegradable agricultural mulch film with a thickness of 0.05 mm; the mass ratio of sodium carboxymethyl cellulose, deionized water, composite reinforcement, borax, is 1.5:100:50:3; the remaining steps are the same as Example 2.

[0038] Effect example

[0039] Table 1 below shows the performance analysis results of the fully biodegradable agricultural mulch films of Examples 1 to 3 of the present invention and Comparative Examples 1 to 7.

[0040] Table 1

[0041]

[0042] From the comparison of the experimental data of the embodiment and the comparative example in Table 1, it can be found that the present invention uses sawdust and cotton fiber for pulping treatment. As the temperature rises, the sawdust swells and brooms, and the separated lignin undergoes esterification reaction with a carboxyl group in maleic acid, while the hydrogen ion of the other carboxyl group in maleic acid will not be ionized due to the intramolecular hydrogen bonding, and the carboxyl group can be free in the fluid, thereby improving the dispersion performance of the matrix material. At the same time, the hydrogen bonds exposed on the surface of the cotton fiber also increase with the beating degree, so that the bonding force between the two fibers is enhanced, thereby enhancing the mechanical properties of the matrix. Then, as a reinforcement, it is cross-linked with sodium carboxymethyl cellulose, wherein the cross-linking agent is glutaraldehyde and borax, and glutaraldehyde and carboxyl methyl cellulose are cross-linked. The hydroxyl groups of the sodium methylcellulose molecules undergo etherification reaction to form a cross-linked spatial network structure, which increases the molecular weight of the system and enhances its density. A small amount of lignin in the wood chips can be filled into the voids of the cellulose film to improve the rigidity of the matrix. When the content of borax molecules increases, the chances of cross-linking of the sodium carboxymethylcellulose molecules also increase, so that they can be tightly connected with the reinforcement fibers, reducing the number of hydroxyl groups in the matrix, improving water resistance and enhancing mechanical properties. Borax is hydrolyzed to produce tetrahydroxyborate ions, which connect the sodium carboxymethylcellulose molecules, enhance the intramolecular interaction between the filler and the matrix, and achieve the full biodegradability of the mulch film.

[0043] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A fully biodegradable agricultural mulch film, characterized in that: The method comprises the following preparation steps: (1) Maleic acid and deionized water are mixed and dissolved at 50-65°C until the solution becomes transparent, pretreated sawdust and cotton fiber are added, the temperature is raised to 90-110°C, and the mixture is stirred at 350-500 rpm for 30-70 min for pulping, and then polyamide polyoxychloropropane resin is added, and the mixture is stirred at 100-200 rpm for 15-50 min under an ultrasonic frequency of 21 kHz to obtain a composite reinforcement; (2) Mix sodium carboxymethyl cellulose and deionized water, stir at 100-200 rpm for 20-40 min, heat to 70-90° C., add a composite reinforcement, continue stirring for 1-2 h, add borax, and dropwise add a 3 wt % glutaraldehyde aqueous solution, stir at 50-70° C. and 200-350 rpm for 1-2 h, then perform ultrasonic degassing, let stand for 3-5 h, cast in a template, and dry at room temperature for 3-6 h to obtain a fully biodegradable agricultural mulch film; the mass ratio of the sodium carboxymethyl cellulose, deionized water, composite reinforcement, borax, and 3 wt % glutaraldehyde aqueous solution is 1:100:20:3:1.5 or 1.5:100:50:3:1.5 or 2:100:70:3:1.

5.

2. A fully biodegradable agricultural mulch film according to claim 1, characterized in that: The preparation method of the pretreated sawdust in step (1) is as follows: the poplar wood sawdust is crushed to pass through a 10-20 mesh sieve, immersed in a 4wt% sodium hydroxide aqueous solution, heated to 85°C, alkalized for 1-2h, then immersed in a 1.7wt% hydrogen peroxide aqueous solution, reacted for 1-2h, and finally rinsed with deionized water for 5-8 times, and dried at 60-80°C for 4-8h.

3. A fully biodegradable agricultural mulch film according to claim 1, characterized in that: The cotton fiber length in step (1) is 0.1-0.5 cm.

4. A fully biodegradable agricultural mulch film according to claim 1, characterized in that: The beating in step (1) is performed until the beating degree is 40-50°SR.

5. A fully biodegradable agricultural mulch film according to claim 1, characterized in that: The power of the ultrasound in step (1) is 400-500W.

6. A fully biodegradable agricultural mulch film according to claim 1, characterized in that: The mass ratio of maleic acid, deionized water, pretreated wood chips, cotton fiber and polyamide polyoxychloropropane resin in step (1) is 50:50:5:1-3:0.

1.

7. The fully biodegradable agricultural mulch film according to claim 1, characterized in that: The dripping rate of the 3 wt % glutaraldehyde aqueous solution in step (2) is 10-40 mL / min.

8. A fully biodegradable agricultural mulch film according to claim 4, characterized in that: The frequency of the ultrasonic degassing in step (2) is 21-25 kHz and the time is 20-60 min.

9. The fully biodegradable agricultural mulch film according to claim 1, characterized in that: The thickness of the fully biodegradable agricultural mulch film in step (2) is 0.01-0.1 mm.