An air-stable sulfide all-solid electrolyte membrane material and preparation method thereof
By incorporating nano-polydopamine into the sulfide electrolyte membrane and immersing it in a bisaminosilane coupling agent to form a hydrophobic layer, the problem of air instability in the electrolyte membrane in all-solid-state batteries is solved, and the safety and performance stability of the battery are improved. Provides an effective path for industrialization.
Patent Information
- Application Number
- CN202411207676.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing all-solid-state sulfide electrolyte membrane is unstable in the air, which affects the safety and performance stability of the battery and hinders the industrialization of sulfide all-solid-state batteries.
By immersing the composite in bisaminosilane coupling agent KH-792 or aminopropyl bis-terminated polydimethylsiloxane and incorporating nanopolydopamine into the polymer binder, a hydrophobic layer is formed to enhance the electrolyte Membrane air stability.
It significantly improves the air stability of the electrolyte membrane, reduces water absorption, and forms a hydrophobic layer, which improves the safety and performance stability of the battery and provides an effective solution for the industrialization of all-solid-state batteries.
Smart Images

Figure CN118712471B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to an air-stable sulfide all-solid-state electrolyte membrane material and a preparation method thereof. Background Art
[0002] The development of solid-state lithium-ion secondary batteries that use solid electrolytes instead of liquid electrolytes is being actively carried out. By using solid electrolytes, excellent features such as thinning of the battery and no leakage of the electrolyte can be obtained. As such solid electrolytes, there are mainly oxide solid electrolytes, polymer solid electrolytes, and sulfide electrolytes. Among them, sulfide solid electrolytes have the advantages of the highest ionic conductivity and good ductility and processability. They are an important research and development direction of solid electrolytes. All-solid-state lithium batteries using sulfide electrolytes are regarded as the most effective solution to solve the safety problems of traditional liquid lithium batteries and improve energy density.
[0003] The room temperature ionic conductivity of the currently reported sulfide solid electrolytes such as Li5.5PS4.5Cl1.5, Li10GeP2S12 and Li9.54Si1.74P1.44S11.7Cl0.3 is no less than that of the electrolyte. However, the following issues currently hinder the industrialization of sulfide all-solid-state batteries:
[0004] The existing all-solid-state sulfide electrolyte membrane has insufficient air stability when used as an electrolyte material, which seriously affects the safety and performance stability of all-solid-state batteries. Summary of the invention
[0005] The purpose of an embodiment of the present invention is to provide an air-stable sulfide all-solid-state electrolyte membrane material and a preparation method thereof, which makes the membrane surface hydrophobic by immersing the composite material into a bisaminosilane coupling agent KH-792 or an aminopropyl dicapped polydimethylsiloxane, thereby enhancing the air stability of the electrolyte membrane, thereby solving at least one technical problem involved in the background technology.
[0006] In order to solve the above-mentioned technical problems, the present invention is achieved as follows:
[0007] The embodiment of the present invention provides a method for preparing an air-stable sulfide all-solid-state electrolyte membrane material, comprising the following steps:
[0008] Step 1, adding nano-polydopamine accounting for 10% of the weight of the polymer binder into the polymer binder and mixing them uniformly by grinding or low-speed ball milling, wherein the polymer binder is thermoplastic polyamide;
[0009] Step 2, mixing the sulfide electrolyte and the polymer binder doped with nano-polydopamine evenly by ball milling, and then heating to 130-140 degrees Celsius for pre-pressing to obtain a thin film prefabricated composite material, wherein the sulfide electrolyte is one or a combination of LiPSCl and LiSiPSCl; the mass ratio of the sulfide electrolyte to the polymer binder is 100:(5-0.1); the ball milling rate is 50-250rpm, and the time is 20-60min;
[0010] Step three, immersing the prefabricated composite material into bisaminosilane coupling agent KH-792 or aminopropyl dicapped polydimethylsiloxane to obtain an air-stable sulfide all-solid-state electrolyte membrane material, wherein the immersion temperature is 60-120 degrees Celsius; the reaction time is 10-30 minutes.
[0011] The present invention also provides an air-stable sulfide all-solid electrolyte membrane material, which is prepared by adopting the preparation method.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] 1. By immersing the composite material in bisaminosilane coupling agent KH-792 or aminopropyl dicapped polydimethylsiloxane, the membrane surface is made hydrophobic, thereby enhancing the air stability of the electrolyte membrane, providing an effective idea for the industrialization of all-solid-state batteries;
[0014] 2. By adding nano-polydopamine, the amorphous area of the polymer binder can be filled to reduce its water absorption; it can also help the hydrophobic silane coupling agent to be grafted to the membrane surface to form a hydrophobic layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0016] Figure 1 The present invention provides a flow chart of a method for preparing an air-stable sulfide all-solid-state electrolyte membrane material. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] See also Figure 1 As shown, an embodiment of the present invention provides a method for preparing an air-stable sulfide all-solid-state electrolyte membrane material, comprising the following steps:
[0019] Step S1, adding nano-polydopamine accounting for 10% of the weight of the polymer binder into the polymer binder and mixing uniformly by grinding or low-speed ball milling;
[0020] It should be noted that the speed of the low-speed ball mill is 200 rpm.
[0021] Step S2, mixing the sulfide electrolyte and the polymer binder doped with nano-polydopamine uniformly by ball milling, and then heating to 130-140 degrees Celsius for pre-pressing to obtain a thin film prefabricated composite material, wherein the sulfide electrolyte is one or a combination of LiPSCl and LiSiPSCl; the mass ratio of the sulfide electrolyte to the polymer binder is 100:(5-0.1); the ball milling rate is 50-250rpm, and the time is 20-60min;
[0022] Step S3, immersing the prefabricated composite material into bisaminosilane coupling agent KH-792 or aminopropyl dicapped polydimethylsiloxane to obtain an air-stable sulfide all-solid-state electrolyte membrane material, wherein the immersion temperature is 60-120 degrees Celsius; and the reaction time is 10-30 minutes.
[0023] The present invention also provides an air-stable sulfide all-solid electrolyte membrane material, which is prepared by adopting the preparation method.
[0024] The preparation method of the air-stable sulfide all-solid-state electrolyte membrane material provided by the present invention is described in detail below with reference to specific examples 1-3.
[0025] Embodiment 1 provides a method for preparing an air-stable sulfide all-solid-state electrolyte membrane material, comprising the following steps:
[0026] Step S1, weigh 99wt% Li 5.5 PS 4.5 C 1.5 Solid electrolyte 9.9g, nano-polydopamine 0.01g, 1wt% thermoplastic polyamide 0.1g;
[0027] Step S2, adding nano-polydopamine into the polymer binder and mixing them evenly;
[0028] Step S3, the sulfide electrolyte and the polymer binder doped with nano-polydopamine are mixed by medium-speed ball milling in a planetary ball mill at a ball milling rate of 250 rpm for 20 min, and then heated to 130 degrees Celsius and rolled multiple times to form a dense film with a thickness of 50 μm;
[0029] Step S4, dissolving the bisaminosilane coupling agent KH-792 in cyclohexane solvent to prepare a 10% solution and heating it to 60 degrees Celsius, then immersing the film obtained in step S2 into the solution to react for 20 minutes, and drying at low temperature to obtain an air-stable sulfide all-solid-state electrolyte membrane material.
[0030] Embodiment 2 provides a method for preparing an air-stable sulfide all-solid-state electrolyte membrane material, comprising the following steps:
[0031] Step S1, weigh 99.5wt% Li 5.5 PS 4.5 C 1.5 Solid electrolyte 9.95g, nano-polydopamine 0.005g, 1wt% thermoplastic polyamide 0.05g;
[0032] Step S2, adding nano-polydopamine into the polymer binder and mixing them evenly;
[0033] Step S3, the sulfide electrolyte and the polymer binder doped with nano-polydopamine are mixed by medium-speed ball milling in a planetary ball mill at a ball milling rate of 250 rpm for 20 min, then heated to 140 degrees Celsius, and rolled multiple times to form a dense film of 50 μm;
[0034] Step S4, dissolving aminopropyl dicapped polydimethylsiloxane in cyclohexane solvent to prepare a 15% solution and heating it to 60 degrees Celsius, then immersing the film obtained in step S2 into the solution to react for 15 minutes, and drying at low temperature to obtain an air-stable sulfide all-solid-state electrolyte membrane material.
[0035] Embodiment 3 provides a method for preparing an air-stable sulfide all-solid-state electrolyte membrane material, comprising the following steps:
[0036] Step S1, weighing 9.8 g of 98 wt% LiSiPSCl solid electrolyte, 0.02 g of nano-polydopamine, and 0.2 g of 1 wt% thermoplastic polyamide;
[0037] Step S2, adding nano-polydopamine into the polymer binder and mixing them evenly;
[0038] Step S3, the sulfide electrolyte and the polymer binder doped with nano-polydopamine are mixed by medium-speed ball milling in a planetary ball mill at a ball milling rate of 200 rpm for 25 min, then heated to 140 degrees Celsius, and rolled multiple times to form a 40 μm dense film;
[0039] Step S4, dissolving the bisaminosilane coupling agent KH-792 in cyclohexane solvent to prepare a 10% solution and heating it to 60 degrees Celsius, then immersing the film obtained in step S2 into the solution to react for 30 minutes, and drying at low temperature to obtain an air-stable sulfide all-solid-state electrolyte membrane material.
[0040] The air-stable sulfide all-solid-state electrolyte membrane material prepared by the preparation method provided in Examples 1-3 was tested, and the experimental results are shown in Table 1.
[0041] Table 1 Experimental results
[0042]
[0043] The experimental results in Table 1 show that after the unmodified sulfide electrolyte is exposed to a low dew point environment, the ionic conductivity decreases rapidly and the air stability is poor; after modification, a hydrophobic layer is formed on the sulfide surface, the air stability is improved, and the ionic conductivity remains at a high level in a low dew point environment for a long time.
[0044] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0045] In addition, it should be noted that the scope of the methods and systems in the embodiments of the present invention is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved. For example, the described methods may be performed in an order different from that described, and various steps may be added, omitted, or combined. In addition, features described with reference to certain examples may be combined in other examples.
[0046] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A method for preparing an air-stable sulfide all-solid electrolyte membrane material, characterized in that: The steps include: Step 1, adding nano-polydopamine accounting for 10% of the weight of the polymer binder into the polymer binder and mixing them uniformly by grinding or low-speed ball milling, wherein the polymer binder is thermoplastic polyamide; Step 2, the sulfide electrolyte and the polymer binder doped with nano-polydopamine are mixed evenly by ball milling, and then heated to 130-140 degrees Celsius for pre-pressing to obtain a thin film prefabricated composite material, wherein the sulfide electrolyte is one or a combination of LiPSCl and LiSiPSCl; the mass ratio of the sulfide electrolyte to the polymer binder is 100: (5-0.1); the ball milling rate is 50-250rpm, and the time is 20-60min; Step three, immersing the prefabricated composite material into bisaminosilane coupling agent KH-792 or aminopropyl dicapped polydimethylsiloxane to obtain an air-stable sulfide all-solid-state electrolyte membrane material, wherein the immersion temperature is 60-120 degrees Celsius; the reaction time is 10-30 minutes.
2. An air-stable sulfide all-solid electrolyte membrane material, characterized in that: The preparation method according to claim 1 is used for preparation.