High-sintering-density stainless steel powder for injection molding and preparation process thereof
By mixing ultra-fine iron-nickel-copper-niobium-molybdenum alloy powder with a stainless steel powder matrix in the MIM injection molding process, the problem of insufficient sintering density of stainless steel powder is solved, and high-efficiency, low-cost stainless steel powder with high sintering density and low energy consumption is achieved. preparation, improving product performance and process efficiency.
Patent Information
- Application Number
- CN202410680552.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-01
AI Technical Summary
The sintering density of stainless steel powder in the existing MIM injection molding process is insufficient, which affects product performance and process efficiency, and the production cost is high.
Stainless steel powder including a stainless steel powder matrix and ultra-fine iron-nickel-copper-niobium-molybdenum alloy powder is used. It is prepared through smelting, atomization, vacuum drying and screening processes. The alloy powder has fine particle size and reasonable content. The tap density of the mixed stainless steel powder reaches 4.8~5.0g/cm3, reducing sintering temperature and energy consumption.
Achieving high sintering density of stainless steel powder reduces sintering temperature and energy consumption, improves product density and performance, complies with national composition standards, reduces inclusions and oxygen content, and promotes the activity and efficiency of the sintering process.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal powders, and in particular to a stainless steel powder with high sintering density for injection molding and a preparation process thereof. Background Art
[0002] Metal injection molding (MIM) is a new technology that combines traditional powder metallurgy process with existing plastic injection molding technology. It not only has the characteristics of high material utilization rate of powder cold metallurgy products, but also has the advantages of high production efficiency of injection molding, uniform product structure, close to net shape, and high dimensional accuracy. This process meets the development trend of current technology miniaturization, integration, functionalization, and thinness, and has therefore been widely studied and developed rapidly in recent years. It is now widely used in a variety of material systems such as high specific gravity, cemented carbide, stainless steel, low alloy steel, and magnetic materials. Its products have also been widely used in many industries such as computers, mechanical automation, automobiles and ships, and medical devices.
[0003] The MIM injection molding process mainly consists of powder and binder mixing, granulation, injection molding, degreasing and sintering. Each process will affect the final performance of the product. Among them, the characteristics of the powder are particularly important. Improper selection of powder not only affects the performance of the final product, but also affects the smooth progress of the entire process.
[0004] Stainless steel, as a special type of steel with high alloy content, has many excellent properties such as good corrosion resistance, oxidation resistance, high strength, and good toughness, and is widely used. With the development of powder metallurgy related processes, higher and higher requirements are also put forward for stainless steel products, among which the sintering density of MIM injection molded products is particularly concerned. Therefore, based on the development needs of the industry, in order to solve the above problems, it is necessary to develop a stainless steel powder product with high sintering density suitable for MIM injection molding, which is efficient, feasible, and has appropriate production costs. Summary of the invention
[0005] In view of the above-mentioned shortcomings, the present invention provides a stainless steel powder for injection molding with high sintering density and a preparation process thereof.
[0006] The present invention achieves the above-mentioned purpose through the following technical scheme: a stainless steel powder for injection molding with high sintering density, characterized in that: the stainless steel powder comprises a stainless steel powder matrix and ultrafine iron-nickel-copper-niobium-molybdenum alloy powder, the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder comprises, by mass percentage: iron Fe: 50-60%; nickel Ni: 15-30%; copper Cu: 14-30%; niobium Nb: 0.20-0.30%; molybdenum Mo: 0.20-0.30%; oxygen O: ≤0.80%; carbon C: 0.50-0.80%, and the ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 2-4% of the mass of the stainless steel powder.
[0007] Preferably, the powder particle size D50 of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder is 3-4 μm.
[0008] Preferably, the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder has a powder particle size D100 of 10 to 15 μm.
[0009] Preferably, the tap density of the stainless steel powder is 4.8 to 5.0 g / cm 3 .
[0010] Preferably, the stainless steel powder matrix is 17-4PH stainless steel powder, and the powder particle size of the 17-4PH stainless steel powder is D50: 9-10 μm; D100: 74-88 μm; and the bulk density is 2.8-3.2 g / cm 3 ; Tap density: 4.6~4.9g / cm 3 .
[0011] Preferably, the method for preparing the stainless steel powder for injection molding with high sintering density comprises the following steps:
[0012] A: Preparation of ultrafine iron-nickel-copper-niobium-molybdenum alloy powder: Step 1, smelting process: the raw materials of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder are prepared according to the component ratio, and then smelted and deoxidized to obtain molten steel; Step 2, atomization process: the molten steel obtained in step 1 is atomized by water and gas to form alloy powder; Step 3, vacuum drying process: the alloy powder obtained in step 2 is dried; Step 4, screening process: airflow classification is used to control the powder particle size and distribution of the dried alloy powder, and the powder particle size D50 is controlled to 3-4 μm and D100 to 10-15 μm to obtain ultrafine iron-nickel-copper-niobium-molybdenum alloy powder;
[0013] B: Preparation of stainless steel powder: The prepared ultrafine iron-nickel-copper-niobium-molybdenum alloy powder is mixed with a stainless steel powder matrix to obtain stainless steel powder. The mass of the ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 2-4% of the mass of the stainless steel powder. The tap density of the stainless steel powder is 4.8-5.0 g / cm 3 .
[0014] Preferably, in step one: the raw materials are fed into a medium frequency induction furnace in the order of nickel, iron, ferromolybdenum, copper, ferroniobium and high carbon iron for smelting in an air atmosphere, the smelting power is controlled to be 100-400KW, the smelting time is 40-55min, and alloying treatment is carried out after the molten steel temperature reaches 1620-1650°C, and the alloying time is 10-20min.
[0015] Preferably, in step one: after alloying treatment, the power of the medium frequency induction furnace is reduced to 80-150KW, silicon calcium and lime are used to slag and deoxidize the molten steel, and the slag is cleaned, and the pump is started to pour steel, and the tapping temperature is 1580-1620°C.
[0016] Preferably, in step 2: nitrogen is used as the process protective atmosphere, and the nitrogen flow rate is: 5.0-10.0m 3 / h; the molten steel flows into the tundish and flows out from the leak at the bottom of the tundish, the leak size is 4.0mm; the atomization process adopts 35° / 25° main and auxiliary spray discs and double V-shaped nozzles; the atomizing water pressure is 120-130MPa, and the atomizing water flow rate is 200L / min.
[0017] Preferably, in step three: a double-cone vacuum dryer is used for drying, the drying temperature is 130° C., and the vacuum degree is 1000 Pa.
[0018] The beneficial effects of the present invention are:
[0019] 1. The ultrafine iron-nickel-copper-niobium-molybdenum alloy powder added has the characteristic of lower sintering temperature than conventional powder. Among the three elements of iron, nickel and copper, copper has the lowest melting point, followed by nickel, and iron has the highest melting point. Therefore, copper and nickel are selected as the main elements to reduce the sintering temperature of the alloy. There is a large amount of iron in the alloy. With the addition of carbon, iron Fe-carbon C eutectic can be formed in the alloy, forming a two-phase structure of austenite-carbide, thereby reducing the melting point during the alloy sintering process. The formation of a micro-melting pool can further improve the sintering activity of the alloy; secondly, the powder particle size is fine, and after sintering, There are few surface inclusions. Due to the use of water-gas combined atomization powder making method, the alloy steel liquid is in contact with the atmosphere during the open smelting process. During the atomization process, the alloy melt reacts with the atomized water medium at high temperature to form oxide inclusions. Since the iron and copper content in the alloy design components is relatively high, the powder fine surface area is large, and the powder oxygen content is relatively high, so a higher carbon content is designed, which can not only reduce the sintering temperature, but also in the sintering stage of the powder product, the carbon can remove oxygen at high temperature to form carbon monoxide. The characteristic can reduce the oxygen content in the sintered product, reduce the proportion of inclusions, and promote sintering.
[0020] 2. The stainless steel powder includes a stainless steel powder matrix and an ultrafine iron-nickel-copper-niobium-molybdenum alloy powder. The ultrafine iron-nickel-copper-niobium-molybdenum powder is mixed with a conventional stainless steel powder matrix, and the mass of the ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 2-4% of the total weight to obtain a stainless steel powder with a high tap density of 4.8-5.0 g / cm 3 The composition of the mixed stainless steel powder meets the national standard for stainless steel powder composition. The ultrafine iron, nickel, copper, niobium and molybdenum powders have fine and uniform particle size dispersion, low melting point, few inclusions and low sintering temperature. The sintering of the conventional stainless steel powder matrix is promoted, thereby achieving the high sintering density of the mixed stainless steel powder. It can also achieve the function of lowering the sintering temperature of the mixed stainless steel powder products, thereby reducing energy consumption, saving energy and reducing emissions. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0022] Example 1
[0023] A stainless steel powder for injection molding with high sintering density, comprising a stainless steel powder matrix and ultrafine iron-nickel-copper-niobium-molybdenum alloy powder, wherein the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder comprises, by mass percentage, 50% iron Fe, 20% nickel Ni, 29.5% copper Cu, 0.25% niobium Nb, 0.25% molybdenum Mo, 0.70% oxygen O, and 0.50% carbon C, wherein the ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 2% of the mass of the mixed stainless steel powder; the stainless steel powder matrix is conventional 17-4PH stainless steel powder, and the conventional 17-4PH stainless steel powder accounts for 98% of the mass of the mixed stainless steel powder.
[0024] A method for preparing stainless steel powder for injection molding with high sintering density comprises the following steps:
[0025] A: Preparation of ultrafine iron-nickel-copper-niobium-molybdenum alloy powder: Step 1, smelting process: The raw materials of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder are prepared according to the above-mentioned component ratio, and the raw materials are sequentially charged into a medium frequency induction furnace in the order of nickel, iron, ferromolybdenum, copper, ferroniobium and high carbon iron for smelting in air atmosphere, and the smelting power is controlled to be 100KW, and the smelting time is 40min. After the temperature of the molten steel reaches 1620°C, alloying treatment is performed, and the alloying time is 10min. After the alloying treatment, the power of the medium frequency induction furnace is reduced to 80KW, and silicon calcium and lime are used to slag and deoxidize the molten steel, and the slag is cleaned, and the pump is started to cast steel, and the tapping temperature is 1580°C;
[0026] Step 2, atomization process: The molten steel obtained in step 1 is atomized by water and gas to form alloy powder, and the nitrogen flow rate is: 5.0m 3 / h; the molten steel flows into the tundish and flows out from the leak at the bottom of the tundish, the leak size is 4.0mm; the atomization process adopts 35° / 25° main and auxiliary spray plates and double V-shaped nozzles; the atomization water pressure is 120MPa, and the atomization water flow rate is 200L / min;
[0027] Step 3, vacuum drying process: drying the alloy powder obtained in step 2, using a double cone vacuum dryer for drying, the drying temperature is 130° C., and the vacuum degree is 1000 Pa;
[0028] Step 4, screening process: airflow classification is used to control the powder particle size and distribution of the dried alloy powder, and the powder particle size D50: 3.54 μm, D100: 13.86 μm are obtained to obtain ultrafine iron-nickel-copper-niobium-molybdenum alloy powder;
[0029] B: Preparation of stainless steel powder: The prepared ultrafine iron-nickel-copper-niobium-molybdenum alloy powder and the stainless steel powder matrix are mixed and mixed by a double planetary mixer for 2 hours per 100 kg to obtain stainless steel powder. The tap density of the stainless steel powder is 4.95 g / cm 3 .
[0030] Example 2
[0031] A stainless steel powder for injection molding with high sintering density. The stainless steel powder comprises a stainless steel powder matrix and ultrafine iron-nickel-copper-niobium-molybdenum alloy powder. The ultrafine iron-nickel-copper-niobium-molybdenum alloy powder comprises, by mass percentage, 50% iron Fe, 29.5% nickel Ni, 20% copper Cu, 0.25% niobium Nb, 0.25% molybdenum Mo, 0.60% oxygen O, and 0.80% carbon C. The ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 4% of the mass of the stainless steel powder. The stainless steel powder matrix is conventional 17-4PH stainless steel powder, and the conventional 17-4PH stainless steel powder accounts for 96% of the mass of the mixed stainless steel powder.
[0032] A method for preparing stainless steel powder for injection molding with high sintering density comprises the following steps:
[0033] A: Preparation of ultrafine iron-nickel-copper-niobium-molybdenum alloy powder: Step 1, smelting process: The raw materials of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder are prepared according to the above-mentioned component ratio, and the raw materials are sequentially charged into a medium frequency induction furnace in the order of nickel, iron, ferromolybdenum, copper, ferroniobium and high carbon iron for smelting in air atmosphere, and the smelting power is controlled to be 400KW, and the smelting time is 55min. When the temperature of the molten steel reaches 1650°C, alloying treatment is carried out for 20min. After the alloying treatment, the power of the medium frequency induction furnace is reduced to 150KW, and silicon calcium and lime are used to slag and deoxidize the molten steel, and the slag is cleaned, and the pump is started to cast steel, and the tapping temperature is 1620°C;
[0034] Step 2, atomization process: The molten steel obtained in step 1 is atomized by water and gas to form alloy powder, and the nitrogen flow rate is: 10.0m 3 / h; the molten steel flows into the tundish and flows out from the leak at the bottom of the tundish, the leak size is 4.0mm; the atomization process adopts 35° / 25° main and auxiliary spray plates and double V-shaped nozzles; the atomization water pressure is 130MPa, and the atomization water flow rate is 200L / min;
[0035] Step 3, vacuum drying process: drying the alloy powder obtained in step 2, using a double cone vacuum dryer for drying, the drying temperature is 130° C., and the vacuum degree is 1000 Pa;
[0036] Step 4, screening process: airflow classification is used to control the powder particle size and distribution of the dried alloy powder, and the powder particle size D50: 3.42 μm, D100: 12.89 μm are obtained to obtain ultrafine iron-nickel-copper-niobium-molybdenum alloy powder;
[0037] B: Preparation of stainless steel powder: The prepared ultrafine iron-nickel-copper-niobium-molybdenum alloy powder and the stainless steel powder matrix are mixed and mixed by a double planetary mixer for 2 hours per 100 kg to obtain stainless steel powder. The tap density of the stainless steel powder is 4.95 g / cm 3 .
[0038] Example 3
[0039] A stainless steel powder for injection molding with high sintering density. The stainless steel powder comprises a stainless steel powder matrix and ultrafine iron-nickel-copper-niobium-molybdenum alloy powder. The ultrafine iron-nickel-copper-niobium-molybdenum alloy powder comprises, by mass percentage, 60% iron Fe, 15% nickel Ni, 24.5% copper Cu, 0.25% niobium Nb, 0.25% molybdenum Mo, 0.80% oxygen O, and 0.50% carbon C. The ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 2% of the mass of the stainless steel powder. The stainless steel powder matrix is conventional 17-4PH stainless steel powder, and the conventional 17-4PH stainless steel powder accounts for 98% of the mass of the mixed stainless steel powder.
[0040] A method for preparing stainless steel powder for injection molding with high sintering density comprises the following steps:
[0041] A: Preparation of ultrafine iron-nickel-copper-niobium-molybdenum alloy powder: Step 1, smelting process: The raw materials of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder are prepared according to the above-mentioned composition ratio, and the raw materials are sequentially charged into a medium frequency induction furnace in the order of nickel, iron, ferromolybdenum, copper, ferroniobium and high carbon iron for smelting in air atmosphere, and the smelting power is controlled to be 100KW, and the smelting time is 40min. When the temperature of the molten steel reaches 1620°C, alloying treatment is carried out for 10min. After the alloying treatment, the power of the medium frequency induction furnace is reduced to 80KW, and silicon calcium and lime are used to slag and deoxidize the molten steel, and the slag is cleaned, and the pump is started to cast steel, and the tapping temperature is 1580°C;
[0042] Step 2, atomization process: The molten steel obtained in step 1 is atomized by water and gas to form alloy powder, and the nitrogen flow rate is: 5.0m 3 / h; the molten steel flows into the tundish and flows out from the leak at the bottom of the tundish, the leak size is 4.0mm; the atomization process adopts 35° / 25° main and auxiliary spray plates and double V-shaped nozzles; the atomization water pressure is 120MPa, and the atomization water flow rate is 200L / min;
[0043] Step 3, vacuum drying process: drying the alloy powder obtained in step 2, using a double cone vacuum dryer for drying, the drying temperature is 130° C., and the vacuum degree is 1000 Pa;
[0044] Step 4, screening process: airflow classification is used to control the powder particle size and distribution of the dried alloy powder, and the powder particle size D50: 3.62 μm, D100: 13.99 μm are obtained to obtain ultrafine iron-nickel-copper-niobium-molybdenum alloy powder;
[0045] B: Preparation of stainless steel powder: The prepared ultrafine iron-nickel-copper-niobium-molybdenum alloy powder and the stainless steel powder matrix are mixed and mixed by a double planetary mixer for 2 hours per 100 kg to obtain stainless steel powder. The tap density of the stainless steel powder is 4.80 g / cm 3 .
[0046] Example 4
[0047] A stainless steel powder for injection molding with high sintering density. The stainless steel powder comprises a stainless steel powder matrix and ultrafine iron-nickel-copper-niobium-molybdenum alloy powder. The ultrafine iron-nickel-copper-niobium-molybdenum alloy powder comprises, by mass percentage, 60% iron Fe, 25% nickel Ni, 14.5% copper Cu, 0.25% niobium Nb, 0.25% molybdenum Mo, 0.70% oxygen O, and 0.80% carbon C. The ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 4% of the mass of the stainless steel powder. The stainless steel powder matrix is conventional 17-4PH stainless steel powder, and the conventional 17-4PH stainless steel powder accounts for 96% of the mass of the mixed stainless steel powder.
[0048] A method for preparing stainless steel powder for injection molding with high sintering density comprises the following steps:
[0049] A: Preparation of ultrafine iron-nickel-copper-niobium-molybdenum alloy powder: Step 1, smelting process: The raw materials of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder are prepared according to the above-mentioned component ratio, and the raw materials are sequentially charged into a medium frequency induction furnace in the order of nickel, iron, ferromolybdenum, copper, ferroniobium and high carbon iron for smelting in air atmosphere, and the smelting power is controlled to be 400KW, and the smelting time is 55min. When the temperature of the molten steel reaches 1650°C, alloying treatment is carried out for 20min. After the alloying treatment, the power of the medium frequency induction furnace is reduced to 150KW, and silicon calcium and lime are used to slag and deoxidize the molten steel, and the slag is cleaned, and the pump is started to cast steel, and the tapping temperature is 1620°C;
[0050] Step 2, atomization process: The molten steel obtained in step 1 is atomized by water and gas to form alloy powder, and the nitrogen flow rate is: 10.0m 3 / h; the molten steel flows into the tundish and flows out from the leak at the bottom of the tundish, the leak size is 4.0mm; the atomization process adopts 35° / 25° main and auxiliary spray plates and double V-shaped nozzles; the atomization water pressure is 130MPa, and the atomization water flow rate is 200L / min;
[0051] Step 3, vacuum drying process: drying the alloy powder obtained in step 2, using a double cone vacuum dryer for drying, the drying temperature is 130° C., and the vacuum degree is 1000 Pa;
[0052] Step 4, screening process: airflow classification is used to control the powder particle size and distribution of the dried alloy powder, and the powder particle size D50: 3.27 μm, D100: 10.52 μm is obtained to obtain ultrafine iron-nickel-copper-niobium-molybdenum alloy powder;
[0053] B: Preparation of stainless steel powder: The prepared ultrafine iron-nickel-copper-niobium-molybdenum alloy powder and the stainless steel powder matrix are mixed and mixed by a double planetary mixer for 2 hours per 100 kg to obtain stainless steel powder. The tap density of the stainless steel powder is 4.80 g / cm 3 .
[0054] The following is a sintering experiment on the mixed stainless steel powder obtained in Examples 1 to 4 of the present invention. The stainless steel powder matrix used in Examples 1 to 4 is the same batch of conventional 17-4PH stainless steel powder. The powder particle size of the conventional 17-4PH stainless steel powder is D50: 9.54μm, D100: 87.52μm. The mixed stainless steel powders of Examples 1 to 4 are processed in batches into samples of the same type according to the same processing technology, and the density of the sintered products is tested and the sintering density change data is compared. The planned sintering temperature is 1280℃, partial pressure sintering, and sintering is carried out in the same furnace. At the same time, the same batch of conventional 17-4PH stainless steel powder is selected to be sintered in the same furnace for comparison.
[0055] The test results are shown in Table 1:
[0056] Table 1:
[0057]
[0058] The test results show that the sintering density of conventional 17-4PH stainless steel powder MIM injection molded products can only reach 7.60-7.70 g / cm 3 The stainless steel powder obtained by mixing the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder and the stainless steel powder matrix of the present invention can achieve a sintering density of 7.72-7.80 g / cm2 of the MIM injection molded product. 3 sintering density.
[0059] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A stainless steel powder for injection molding with high sintering density, characterized in that: The stainless steel powder comprises a stainless steel powder matrix and ultrafine iron-nickel-copper-niobium-molybdenum alloy powder. The ultrafine iron-nickel-copper-niobium-molybdenum alloy powder is calculated by mass percentage. The invention comprises: iron Fe: 50-60%, nickel Ni: 15-30%, copper Cu: 14-30%, niobium Nb: 0.20-0.30%, molybdenum Mo: 0.20-0.30%, oxygen O: ≤0.80%, carbon C: 0.50-0.80%, and the ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 2-4% of the mass of the stainless steel powder.
2. The stainless steel powder for injection molding with high sintering density according to claim 1, characterized in that: The powder particle size D50 of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder is 3-4 μm.
3. The stainless steel powder for injection molding with high sintering density according to claim 2, characterized in that: The powder particle size D100 of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder is 10-15 μm.
4. The stainless steel powder for injection molding with high sintering density according to claim 1, characterized in that: The tap density of the stainless steel powder is 4.8-5.0 g / cm 3 .
5. The stainless steel powder for injection molding with high sintering density according to claim 1, characterized in that The stainless steel powder matrix is 17-4PH stainless steel powder, the powder particle size of the 17-4PH stainless steel powder is D50: 9-10 μm; D100: 74-88 μm; loose density: 2.8-3.2 g / cm 3 ; Tap density: 4.6~4.9g / cm 3 .
6. The method for preparing a stainless steel powder for injection molding with high sintering density according to any one of claims 1 to 5, characterized in that: The following steps are involved: A: Preparation of ultrafine iron-nickel-copper-niobium-molybdenum alloy powder: Step 1, smelting process: the raw materials of the ultrafine iron-nickel-copper-niobium-molybdenum alloy powder are prepared according to the component ratio, and then smelted and deoxidized to obtain molten steel; Step 2, atomization process: the molten steel obtained in step 1 is atomized by water and gas to form alloy powder; Step 3, vacuum drying process: the alloy powder obtained in step 2 is dried; Step 4, screening process: airflow classification is used to control the powder particle size and distribution of the dried alloy powder, and the powder particle size D50 is controlled to 3-4 μm and D100 to 10-15 μm to obtain ultrafine iron-nickel-copper-niobium-molybdenum alloy powder; B: Preparation of stainless steel powder: The prepared ultrafine iron-nickel-copper-niobium-molybdenum alloy powder is mixed with a stainless steel powder matrix to obtain stainless steel powder. The mass of the ultrafine iron-nickel-copper-niobium-molybdenum powder accounts for 2-4% of the mass of the stainless steel powder. The tap density of the stainless steel powder is 4.8-5.0 g / cm 3 .
7. The method for preparing a stainless steel powder for injection molding with high sintering density according to claim 6, characterized in that: In step 1: the raw materials are fed into a medium frequency induction furnace in the order of nickel, iron, ferromolybdenum, copper, ferroniobium and high carbon iron for smelting in an air atmosphere, the smelting power is controlled to be 100-400KW, the smelting time is 40-55min, and alloying treatment is carried out after the molten steel temperature reaches 1620-1650°C, and the alloying time is 10-20min.
8. The method for preparing a stainless steel powder for injection molding with high sintering density according to claim 7, characterized in that: In step 1: after alloying treatment, the power of the medium frequency induction furnace is reduced to 80-150KW, silicon calcium and lime are used to slag and deoxidize the molten steel, and the slag is cleaned, and the pump is started to pour steel, and the tapping temperature is 1580-1620℃.
9. The method for preparing a stainless steel powder for injection molding with high sintering density according to claim 6, characterized in that: In step 2: nitrogen is used as the process protective atmosphere, and the nitrogen flow rate is: 5.0~10.0m 3 / h; the molten steel flows into the tundish and flows out from the leak at the bottom of the tundish, the leak size is 4.0mm; the atomization process adopts 35° / 25° main and auxiliary spray discs and double V-shaped nozzles; the atomizing water pressure is 120-130MPa, and the atomizing water flow rate is 200L / min.
10. The method for preparing a stainless steel powder for injection molding with high sintering density according to claim 6, characterized in that: In step three: a double cone vacuum dryer is used for drying, the drying temperature is 130° C., and the vacuum degree is 1000 Pa.