Electric spark and electrolysis combined machining process for machining net-shaped titanium-based composite material
Through the combined EDM and electrolysis machining process, combined with EDM roughing and finishing and electrolytic machining, the problem of poor mechanical properties and surface quality during the processing of titanium-based composite materials is solved, and a high-quality machined surface is achieved to meet the microstructural requirements. Suitable for aerospace and micro robotics and other fields.
Patent Information
- Application Number
- CN202411046501.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-01
AI Technical Summary
During the processing of titanium-based composite materials, there are problems such as poor mechanical properties, serious room temperature brittleness, high surface roughness, micro-cracks and micro-voids caused by traditional electric discharge machining, and stray corrosion and passive film formation caused by electrolytic machining.
Adopting the combined EDM and electrolytic machining process, through the combination of EDM rough machining and finishing, combined with electrolytic machining, real-time monitoring and adjustment of processing parameters to ensure surface quality, including the steps of EDM rough machining, finishing and electrolytic machining, and control of recasting layer thickness and removal rate, achieving surface roughness as low as 0.1μm, free of defects and stray corrosion.
A high-quality machined surface is obtained, which meets the microstructural requirements, improves the mechanical properties and wear resistance of the material, reduces tool wear and cutting temperature, and is suitable for fields such as aerospace and micro-robots.
Smart Images

Figure CN118720299A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electric spark machining and electrolytic machining, and more specifically to an electric spark electrolytic combined machining process for machining a mesh titanium-based composite material. Background Art
[0002] With the continuous development of metal matrix composites, titanium matrix composites stand out as a material with broad application prospects. It has high strength, excellent ductility, significant wear resistance and superior high temperature durability. These excellent properties make it widely used in aerospace and advanced military fields.
[0003] However, studies have shown that the reinforcement phase in most titanium-based composites is evenly distributed in the matrix material, which leads to poor mechanical properties and severe room temperature brittleness. On the other hand, titanium-based composites are difficult to process. Due to the high hardness and brittleness of the reinforcement phase, composites face major challenges during processing. When using traditional mechanical processing, problems such as severe tool wear, cutting force fluctuations, increased cutting temperature, and difficulty in chip removal often occur.
[0004] In order to improve the above defects, the existing technology also has electric spark machining and electrolytic machining. However, after traditional electric spark machining, a recast layer will be formed on the surface of the material, which will cause the following problems: 1. The surface roughness can be machined to a minimum of 0.5μm, which does not meet the use requirements for many microstructure fields. 2. There are defects such as microcracks and micropores on the surface. 3. After the base material is melted at high temperature, it re-solidifies to form a recast layer. The crystal structure of the material changes, and it differs from the base material in hardness, strength, wear resistance, high-temperature durability, etc. Electrolytic machining will also cause a series of problems: 1. Due to the different corrosion rates of the material matrix and the reinforcing phase, stray corrosion is serious and the surface machining quality is poor. 2. Electrolytic machining of titanium-based materials will form a passivation film on the surface of the workpiece, which hinders material removal. Summary of the invention
[0005] The invention provides an electric spark electrolysis combined machining process for machining a mesh titanium-based composite material, which can obtain a high-quality machined surface that can meet microstructure requirements.
[0006] The above purpose is achieved through the following technical solutions:
[0007] A combined electric spark and electrolytic machining process for machining a mesh titanium-based composite material comprises the following steps:
[0008] Step 1: Performing electrospark machining on the surface of the mesh titanium-based composite material;
[0009] Step 2: detecting the surface of the mesh titanium-based composite material after electrospark machining to obtain the thickness of the recast layer of the mesh titanium-based composite material after electrospark finishing machining;
[0010] Step 3: electrolytically machining another mesh titanium-based composite material;
[0011] Step 4: measuring the removal rate of the electrolytic machining of the mesh titanium-based composite material and the residual degree of the recast layer;
[0012] Step 5: Calculate the electrolytic processing time according to the thickness of the recast layer after EDM;
[0013] Step 6: Electrolytic machining is performed on the EDM surface of the mesh titanium-based composite material according to the electrolytic machining time and the removal rate in the electrolytic machining;
[0014] Step 7: Detect the surface of the mesh titanium-based composite material electrolytically processed in step 6 to obtain the following data: electrolytically processed surface morphology, surface roughness, and residual degree of the recast layer;
[0015] Step 8: If the data meets the requirements, the processing is terminated; if the data does not meet the requirements, the electrolytic processing is repeated until the requirements are met.
[0016] The beneficial effects of the electric spark electrolysis combined machining process for machining a mesh titanium-based composite material of the present invention are:
[0017] like Figure 2 As shown in the figure, the composite material uses a network of TiB whiskers (TiBw) as the reinforcement phase and TC4 as the matrix material. Its unique capsule structure allows the hard phase to encapsulate the soft phase, so that the composite material exhibits excellent strength, stiffness and elastic modulus, while also showing enhanced ductility, wear resistance and high-temperature durability. Compared with TC4, its operating temperature is increased by 200°C, and compared with commonly used nickel-based superalloys, its specific gravity is lower, thus meeting the industry's demand for lightweight materials.
[0018] In view of the difficult processing characteristics of mesh titanium matrix composite materials, the poor surface quality of EDM, and the problems of stray corrosion in electrolytic processing, the two processing technologies can be combined to inhibit the formation of passivation film when processing the recast layer on the surface of the parts due to its uneven discharge pits. A high-quality processing surface with a surface roughness as low as 0.1μm, no surface defects, no stray corrosion, and no recast layer can be obtained. It has broad application prospects in the fields of aerospace, micro-robots, precision parts, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is the process flow chart of EDM combined machining;
[0020] Figure 2 These are optical microscope and electron microscope images of the mesh titanium matrix composite material;
[0021] Figure 3 It is the laser confocal surface topography of EDM rough machining;
[0022] Figure 4 It is the electron microscope image of the recast layer during EDM rough machining;
[0023] Figure 5 It is the electron microscope image of surface microcracks during EDM rough machining;
[0024] Figure 6 It is the laser confocal surface topography of EDM finishing;
[0025] Figure 7 It is the electron microscope image of the recast layer of EDM finishing;
[0026] Figure 8 It is the electron microscope surface micro-crack image of EDM finishing;
[0027] Fig. 9 This is the XRD analysis diagram of electrolytic processing byproducts in NaCl electrolyte;
[0028] Fig.10 This is the laser confocal surface topography image of electrochemical machining in NaCl electrolyte;
[0029] Fig.11 This is the electron microscope surface morphology of electrolytic machining in NaCl electrolyte;
[0030] Fig.12 It is an electron microscope surface morphology image of EDM combined machining. DETAILED DESCRIPTION
[0031] A combined electrospark and electrolytic machining process for machining mesh titanium-based composite materials, reference Figure 1 , including the following steps:
[0032] Step 1: According to the part contour, leave a machining allowance for the part, for example, by writing G code during CNC programming. On the other hand, considering the problem of electrode loss, real-time online compensation can be performed to ensure the machining accuracy and stability of the part's machining quality. Subsequently, the mesh titanium-based composite material (abbreviated as the part) is rough-machined using electric sparks, using a tungsten electrode with a diameter of 0.3 mm to control the roughness of the part below 3.0 μm and improve the material removal rate. Electric spark rough machining can use large machining energy, with each discharge energy of 1.000-2.000 J, which further improves the material removal rate.
[0033] Step 2: If Figure 3As shown in the figure, the laser confocal surface morphology of the parts after EDM rough machining was observed and the roughness was measured. Under high machining energy, the roughness of the part surface was 1.8-2.0μm. In order to better observe the recast layer, a corrosion reagent, such as Kroll's reagent (5% HF and 15% HNO3), was used to etch the surface of the part to expose its crystal structure. Figure 4 As shown, the different crystal structures of the recast layer and the reticular titanium-based composite material were observed under an electron microscope.
[0034] Due to the randomness and non-uniformity of discharge, the thickness of the recast layer is different under the same processing parameters. Therefore, the average thickness is used to represent the thickness of the recast layer, as shown in Formula 1:
[0035] (1)
[0036] Where: h is the average thickness of the recast layer;
[0037] n——number of sampling times;
[0038] ——The maximum thickness of the recast layer in the nth electron micrograph;
[0039] ——the minimum thickness of the recast layer in the nth electron microscope image;
[0040] Considering the non-uniformity of the recast layer, multiple samplings were performed to obtain the maximum and minimum thickness of the recast layer in all electron microscope photos, and the range was calculated to measure the uniformity of the recast layer, as shown in Formula 2:
[0041] (2) R = h max -h min
[0042] Where: R——the range of the thickness of the recast layer obtained by sampling;
[0043] h max ——Sampling to obtain the maximum thickness of the recast layer in all photos;
[0044] h min ——Sampling to obtain the minimum thickness of the recast layer in all photos;
[0045] The thickness mentioned above is in μm.
[0046] The results show that under high-energy EDM, the average thickness of the recast layer on the machined surface of the part is 13μm. At the same time, the thickness of the recast layer varies to 20μm. Figure 5As shown, the microcrack defects on the surface of the EDM rough machining were observed using an electron microscope. In summary, after EDM rough machining, the surface roughness and average thickness of the recast layer of the obtained parts are large, the recast layer is extremely uneven, and there are many microcracks on the surface of the parts, which seriously affects the surface quality of the parts.
[0047] Step 3: Perform EDM finishing on the parts after EDM rough machining, use a tungsten electrode with a diameter of 0.1mm for machining, control the roughness of the parts below 1.0μm, improve the manufacturing accuracy of the parts, and select small energy machining for EDM finishing, with a discharge energy of 0.005-0.010J each time. According to the actual situation, select appropriate process parameters such as pulse width, pulse interval and current, and compensate for the loss of electrode in real time online.
[0048] Step 4: Check the surface of the parts after EDM finishing. Figure 6 As shown in the figure, it is a confocal laser surface morphology image of EDM finishing. It can be clearly observed that the diameter of the discharge pit on the surface of the part becomes smaller, and its surface roughness drops to about 0.8μm. Kroll's reagent (5% HF and 15% HNO3) is used to etch the surface of the part. Figure 7 The results are obtained by electron microscope observation.
[0049] The results show that under low-energy EDM finishing, the average thickness of the recast layer on the surface of the parts is about 6μm. At the same time, the thickness of the recast layer is as low as 4μm. Figure 8 As shown in the figure, the micro cracks on the surface of the EDM finishing machined parts are significantly reduced. In summary, after EDM finishing, the surface roughness and average thickness of the recast layer of the parts are reduced, the recast layer is relatively uniform, the micro cracks on the surface of the parts are reduced, and the surface quality has been improved to a certain extent, but it is not enough to achieve the requirements of 0.1μm surface roughness, no recast layer, and no surface damage for the microstructure surface quality.
[0050] Step 5: Electrochemical machining of the second part, and the byproducts of electrochemical machining of the part in NaCl electrolyte are collected. At the beginning of electrochemical machining, a large number of bubbles are observed on the anode workpiece in the electrolyte. This indicates that oxygen bubbles are generated by the hydrolysis of water on the surface of the anode workpiece, and its electrochemical reaction formula is shown in Equation 1:
[0051] (1) 4OH - →2H2O+O2↑+4e -
[0052] As the electrolytic machining proceeds, a large number of dense bubbles are precipitated at the cathode, which indicates that the cathode reduces the hydrogen ions in the electrolyte to hydrogen gas. The electrochemical reaction formula is shown in Formula 2:
[0053] (2)2H + +2e- →H2↑
[0054] XRD analysis was performed on the byproducts of electrolytic processing of the reticular titanium-based composite material in NaCl electrolyte. Fig. 9 As shown in Figure 2, the byproducts of electrolytic processing of the mesh titanium-based composite material in NaCl electrolyte are TiO2 and TiB. This is because Cl- ions have an activation effect on titanium-based alloys, and the dissolution of the Ti element is controlled by forming a halide complex, and its electrochemical dissolution behavior is shown in Equations 3 and 4:
[0055] (3) Ti-4e - +4Cl - →TiCl4
[0056] (4) TiCl4+2H2→TiO2+4Cl - +4H +
[0057] Step 6: Observe the surface of the parts electrochemically processed by NaCl electrolyte through laser confocal microscopy. Fig.10 As shown in the figure, it can be found that when electrolytic machining parts, the stray corrosion on the surface of the parts is more serious, and the surface roughness reaches 3.2μm, which is much higher than the surface obtained by EDM. Fig.11 As shown in the figure, by observing the surface morphology under an electron microscope, it can be found that the stray corrosion is caused by the inconsistent corrosion rate of the reinforcement phase and the base material. The titanium-based matrix is first oxidized to titanium ions. As the electrolytic processing proceeds, the reinforcement phase slowly protrudes until the surrounding titanium-based matrix material is completely oxidized to titanium ions and the reinforcement phase falls off. As a result, the reinforcement phase protrudes during the electrolysis process, causing stray corrosion, which seriously affects the quality of the machined surface of the part. The surface quality obtained by electrolytic processing in the area without the reinforcement phase is higher.
[0058] Step 7: Develop a combined EDM and electrolytic machining process: Based on the surface morphology and surface roughness of the electrolytically machined parts, as well as the calculated electrolytic machining part removal rate, and the electrolytic machining time calculated based on the thickness of the recast layer after EDM machining, electrolytic machining is performed on the surface of the parts obtained by EDM machining.
[0059] Step 8: Inspect the surface of the part obtained by electrolytic processing in step 7. If the part meets the requirements of surface roughness, residual thickness of the recast layer, surface defects and stray corrosion, the processing is terminated; if the surface quality obtained does not meet the requirements, continue processing according to the requirements of surface roughness, residual thickness of the recast layer, surface defects and stray corrosion until the requirements are met. Fig.12The figure shows the effect of EDM combined machining. The surface of the part is even and flat, without obvious defects, and the recast layer is completely removed. According to laser confocal detection, the surface roughness of the mesh titanium-based composite material obtained by EDM combined machining is as low as 0.08μm, which meets the processing requirements of fine parts.
Claims
1. A combined electrospark and electrolytic machining process for machining a mesh titanium-based composite material, characterized in that: The following steps are involved: Step 1: Performing electrospark machining on the surface of the mesh titanium-based composite material; Step 2: detecting the surface of the mesh titanium-based composite material after electrospark machining to obtain the thickness of the recast layer of the mesh titanium-based composite material after electrospark machining; Step 3: electrolytically machining another mesh-shaped titanium-based composite material; Step 4: measuring the removal rate of the electrolytic machining of the mesh titanium-based composite material and the residual degree of the recast layer; Step 5: Calculate the electrolytic processing time according to the thickness of the recast layer after EDM; Step 6: Electrolytic machining is performed on the EDM surface of the mesh titanium-based composite material according to the electrolytic machining time and the removal rate in the electrolytic machining; Step 7: Detect the surface of the mesh titanium-based composite material electrolytically processed in step 6 to obtain the following data: electrolytically processed surface morphology, surface roughness, and residual degree of the recast layer; Step 8: If the data meets the requirements, the processing is terminated; if the data does not meet the requirements, the electrolytic processing is repeated until the requirements are met.
2. The electric spark electrolysis combined machining process for machining a mesh titanium-based composite material according to claim 1, characterized in that: During EDM, real-time online compensation is performed for electrode loss.
3. The electric spark electrolysis combined machining process for machining a mesh titanium-based composite material according to claim 1, characterized in that: During EDM, tungsten electrodes with diameters of 0.3 mm and 0.1 mm were used successively.
4. The electric spark electrolysis combined machining process for machining a mesh titanium-based composite material according to claim 1, characterized in that: When using a 0.3mm tungsten electrode, the discharge energy is 1-2J, and when using a 0.1mm tungsten electrode, the discharge energy is 0.005-0.010J.
5. The electric spark electrolysis combined machining process for machining a mesh titanium-based composite material according to claim 1, characterized in that: After EDM, the roughness of the parts is controlled below 1.0 μm.
6. The combined electrospark and electrolytic machining process for machining a mesh titanium-based composite material according to claim 1 is characterized by: In step 2, a corrosive agent is used to corrode the machined surface of the mesh titanium-based composite material, and a recast layer of the machined surface is obtained by observation under an electron microscope.
7. The electric spark electrolysis combined machining process for machining a mesh titanium-based composite material according to claim 1, characterized in that: In step three, byproducts of electrolytic processing of the mesh titanium-based composite material in a NaCl electrolyte are collected.
8. The combined electric spark electrolysis machining process for machining a mesh titanium-based composite material according to claim 7, characterized in that: The processed surface obtained by electrolytic processing in NaCl electrolyte was observed by laser confocal microscope, and its surface morphology was observed under electron microscope.
9. The electric spark electrolysis combined machining process for machining a mesh titanium-based composite material according to claim 1, characterized in that: The surface roughness of the mesh titanium-based composite material processed by electric spark electrolysis is controlled below 0.1 μm.
10. A mesh titanium-based composite material, characterized in that: The TiB whiskers distributed in a network are used as the reinforcement phase, and TC4 is used as the matrix material.
Citation Information
Patent Citations
Electric spark induction controllable erosion and electrolysis compound efficient machining method
CN102151924A
Electric spark and electrolytic continuous machining method and tool for efficient plane milling
CN110756926A
Additive manufacturing metal rough surface electrolysis electric spark composite leveling tool and method
CN110893493A
Aluminum alloy electrolytic chemical milling method
CN114669813A
Method for electrolytic polishing of member made of stainless steel
JP1995185941A