Artificial leather and manufacturing method thereof

By using a modified thermoplastic polyolefin layer and corona treatment technology in artificial leather, the problems of high carbon emissions and limited processability in the existing technology are solved, and more efficient material processing and multi-variable surface treatments are achieved.

CN118721874AActive Publication Date: 2024-10-01SAN FANG CHEM IND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310661153.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-06-06
Publication Date
2024-10-01
Estimated Expiration
2043-06-06

AI Technical Summary

Technical Problem

The existing artificial leather manufacturing process has high carbon emissions and large energy losses, and the material structure cannot impart much variability to the surface, resulting in limited processability.

Method used

It uses artificial leather containing a modified thermoplastic polyolefin layer, forms a laminated structure on the base fabric layer, and uses corona treatment and co-extrusion film technology to improve adhesion and surface treatment, and reduce carbon emissions and energy consumption.

Benefits of technology

It achieves better adhesion and processability, reduces carbon emissions and energy consumption, and meets the changing needs of shoemaking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721874A_ABST
    Figure CN118721874A_ABST
Patent Text Reader

Abstract

The invention provides artificial leather and a manufacturing method thereof. The artificial leather comprises a base cloth layer, a thermoplastic polyolefin layer, a modified thermoplastic polyolefin layer, paste and a polyurethane surface layer. The thermoplastic polyolefin layer is arranged on the base cloth layer. The modified thermoplastic polyolefin layer is arranged on the thermoplastic polyolefin layer. And the polyurethane surface layer is adhered to the modified thermoplastic polyolefin layer through the paste. According to the artificial leather disclosed by the invention, the modified thermoplastic polyolefin layer is used for lamination, so that better adhesiveness can be provided. In addition, by using the thermoplastic polyolefin layer and the modified thermoplastic polyolefin layer, the carbon emission in the process can be reduced, and the energy loss can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an artificial leather and a manufacturing method thereof, in particular to an artificial leather comprising a modified thermoplastic polyolefin layer and a manufacturing method thereof. Background Art

[0002] As the requirements of environmental protection in various countries around the world are increasing year by year, the emission standards (e.g., carbon emission, volatile organic compounds, etc.) of many products in the manufacturing process are becoming increasingly strict to reduce the pollution caused to the environment. However, the carbon emission of materials used in the manufacture of artificial leather is relatively high and will cause high energy loss. In addition, the structure of the known artificial leather cannot give its surface variability, and in order to maintain the adhesion between the layers, materials of the same nature must be used for processing, so the processability is greatly limited. Summary of the invention

[0003] In some embodiments, an artificial leather comprises a base fabric layer, a thermoplastic polyolefin layer, a modified thermoplastic polyolefin layer, a paste, and a polyurethane surface layer. The thermoplastic polyolefin layer is disposed on the base fabric layer. The modified thermoplastic polyolefin layer is disposed on the thermoplastic polyolefin layer. The polyurethane surface layer is adhered to the modified thermoplastic polyolefin layer through the paste.

[0004] In some embodiments, an artificial leather comprises a base fabric layer, a modified thermoplastic polyolefin layer, a thermoplastic polyurethane layer, a paste, and a polyurethane surface layer. The modified thermoplastic polyolefin layer is disposed on the base fabric layer. The thermoplastic polyurethane layer is disposed on the modified thermoplastic polyolefin layer. The polyurethane surface layer is adhered to the thermoplastic polyurethane layer through the paste.

[0005] In some embodiments, a method for manufacturing artificial leather includes: providing a base fabric layer; forming a laminated structure on the base fabric layer, wherein the laminated structure includes a modified thermoplastic polyolefin layer; and bonding a polyurethane surface layer to the laminated structure by means of a paste. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] When read in conjunction with the accompanying drawings, the following is a detailed description of some embodiments of the present invention that is easy to understand. It should be noted that various structures may not be drawn to scale, and the size of various structures may be arbitrarily increased or reduced for clarity of discussion.

[0007] Figure 1 A schematic cross-sectional view of artificial leather according to some embodiments of the present disclosure is shown.

[0008] Figure 2 A schematic cross-sectional view of artificial leather according to some embodiments of the present disclosure is shown.

[0009] Figure 3A schematic cross-sectional view of artificial leather according to some embodiments of the present disclosure is shown.

[0010] Figure 4 Schematic diagram showing one or more stages of some embodiments of the method for manufacturing artificial leather according to the present disclosure.

[0011] Figure 5 Schematic diagram showing one or more stages of some embodiments of the method for manufacturing artificial leather according to the present disclosure.

[0012] Figure 6 Schematic diagram showing one or more stages of some embodiments of the method for manufacturing artificial leather according to the present disclosure.

[0013] Explanation of symbols:

[0014] 1: Artificial leather

[0015] 1a: Artificial leather

[0016] 1b: Artificial leather

[0017] 10: Base fabric layer

[0018] 20: Thermoplastic polyolefin

[0019] 30: Modified thermoplastic polyolefin layer

[0020] 31: First surface

[0021] 32: Second surface

[0022] 40: Paste

[0023] 50: Polyurethane surface

[0024] 60: Thermoplastic polyurethane layer

[0025] 61: First surface

[0026] 62: Second surface

[0027] 80: Modified blending layer

[0028] 81: First surface

[0029] 82: Second surface

[0030] 90:Laminated structure

[0031] 30a: modified thermoplastic polyolefin layer

[0032] 90a: Laminated structure DETAILED DESCRIPTION

[0033] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0034] See also Figure 1 , which is a schematic cross-sectional view of an artificial leather 1 according to some embodiments of the present disclosure. The artificial leather 1 of the present invention comprises a base fabric layer 10, a thermoplastic polyolefin (TPO) layer 20, a modified thermoplastic polyolefin (m-TPO) layer 30, a paste 40, and a polyurethane (PU) surface layer 50. In some embodiments, the base fabric layer 10 may include but is not limited to non-woven fabric.

[0035] The thermoplastic polyolefin layer 20 is disposed on the base fabric layer 10. In some embodiments, the thickness of the thermoplastic polyolefin layer 20 may be less than or equal to the thickness of the base fabric layer 10.

[0036] The modified thermoplastic polyolefin layer 30 is disposed on the thermoplastic polyolefin layer 20, so the modified thermoplastic polyolefin layer 30 and the thermoplastic polyolefin layer 20 can form a laminated structure 90. In some embodiments, the modified thermoplastic polyolefin layer 30 can be a blend of thermoplastic polyolefin and maleic acid, and its purpose is to modify the thermoplastic polyolefin by the maleic acid so that the adhesion of the modified thermoplastic polyolefin layer 30 can be greater than the adhesion of the thermoplastic polyolefin layer 20. In some embodiments, based on the total weight of the modified thermoplastic polyolefin layer 30 being 100wt%, the content of the maleic acid can be 3wt% to 50wt%. When the content of maleic acid is lower than 3wt%, the polyurethane surface layer 50 will not adhere properly, and the peeling strength between the modified thermoplastic polyolefin layer 30 and the polyurethane surface layer 50 will be lower than 1kg / cm and cannot be used for shoemaking. When the content of maleic acid is higher than 50wt%, the film-forming property of the modified thermoplastic polyolefin layer 30 is poor and the processability is poor. In some embodiments, the content of maleic acid may be 20wt% to 40wt%, 22wt% to 38wt%, 24wt% to 36wt%, 26wt% to 34wt% or 28wt% to 32wt%. In addition, in some embodiments, the thickness of the modified thermoplastic polyolefin layer 30 may be less than or equal to the thickness of the thermoplastic polyolefin layer 20.

[0037] In some embodiments, Figure 1As shown, the modified thermoplastic polyolefin layer 30 has a first surface (e.g., lower surface) 31 and a second surface (e.g., upper surface) 32. The first surface 31 contacts the thermoplastic polyolefin layer 20. The second surface 32 is opposite to the first surface 31. In some embodiments, the second surface 32 may be a corona discharge processed surface.

[0038] The paste 40 may be a non-solvent paste or a solvent paste (the solvent content may be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%). In some embodiments, the paste 40 may include but is not limited to one of the following: solvent-based polyurethane resin, water-based polyurethane resin, thermoplastic polyurethane resin, ethylene-vinyl acetate copolymer adhesive, polyvinyl chloride adhesive, polyolefin adhesive and epoxy resin adhesive. In some embodiments, the thickness of the paste 40 may be less than or equal to the thickness of the modified thermoplastic polyolefin layer 30.

[0039] The polyurethane surface layer 50 is attached to the modified thermoplastic polyolefin layer 30 (eg, the second surface (corona treated surface) 32) through the paste 40. Figure 1 As shown, the paste 40 is disposed between the polyurethane surface layer 50 and the modified thermoplastic polyolefin layer 30 (e.g., the second surface (corona treated surface) 32). In some embodiments, the polyurethane surface layer 50 may be a water-based polyurethane surface layer. In addition, in some embodiments, the polyurethane surface layer 50 may be coated with a release paper (Release Paper, RP) (not shown) to transfer the texture. In some embodiments, the thickness of the polyurethane surface layer 50 may be less than or equal to the thickness of the paste 40.

[0040] The artificial leather 1 of the present invention uses the modified thermoplastic polyolefin layer 30 for lamination, which can provide better adhesion, and the corona-treated surface of the modified thermoplastic polyolefin layer 30 (i.e., the second surface 32) can further improve the surface adhesion and enhance the processability of the overall material, and can make the artificial leather 1 easier to shape, thereby meeting the relevant physical property requirements of shoemaking and meeting the variability requirements of shoemaking. In addition, the artificial leather 1 of the present invention uses the thermoplastic polyolefin layer 20 and the modified thermoplastic polyolefin layer 30 to reduce carbon emissions and energy loss in the process.

[0041] See also Figure 2 , which is a schematic cross-sectional view showing an artificial leather 1a according to some embodiments of the present disclosure. Figure 2 The artificial leather 1a has and Figure 1The structure is similar to that of artificial leather 1, the difference being that: Figure 2 In some embodiments, the laminated structure 90a of the artificial leather 1a is Figure 2 As shown, the laminate structure 90 a may include a modified thermoplastic polyolefin layer 30 a and a thermoplastic polyurethane layer 60 .

[0042] The modified thermoplastic polyolefin layer 30a is disposed on the base fabric layer 10. In some embodiments, Figure 2 The base fabric layer 10 may be the same as Figure 1 The base fabric layer 10, Figure 2 The modified thermoplastic polyolefin layer 30a may be the same as Figure 1 In some embodiments, the modified thermoplastic polyolefin layer 30a may have a thickness less than or equal to that of the base fabric layer 10.

[0043] The thermoplastic polyurethane layer 60 is disposed on the modified thermoplastic polyolefin layer 30a. In some embodiments, the thickness of the thermoplastic polyurethane layer 60 may be less than or equal to the thickness of the modified thermoplastic polyolefin layer 30a.

[0044] In some embodiments, Figure 2 As shown, the thermoplastic polyurethane layer 60 has a first surface (e.g., lower surface) 61 and a second surface (e.g., upper surface) 62. The first surface 61 contacts the modified thermoplastic polyolefin layer 30a. The second surface 62 is opposite to the first surface 61. In some embodiments, the second surface 62 may be a corona-treated surface.

[0045] Based on the above configuration, the polyurethane surface layer 50 can be attached to the thermoplastic polyurethane layer 60 (eg, the second surface (corona treated surface) 62) through the paste 40. Figure 2 As shown, the paste 40 is disposed between the polyurethane surface layer 50 and the thermoplastic polyurethane layer 60 (eg, the second surface (corona treated surface) 62). In some embodiments, Figure 2 The paste 40 may be the same as Figure 1 Paste 40, Figure 2 The polyurethane surface layer 50 may be the same as Figure 1 In some embodiments, the thickness of the paste 40 may be less than or equal to the thickness of the thermoplastic polyurethane layer 60.

[0046] See also Figure 3 , which is a schematic cross-sectional view showing an artificial leather 1b according to some embodiments of the present disclosure. Figure 3 The artificial leather 1b has and Figure 2 The structure is similar to that of artificial leather 1a, the difference being that: Figure 3 The modified blend layer 80 of artificial leather 1b. In some embodiments, Figure 3 The modified blending layer 80 may be Figure 2 The modified thermoplastic polyolefin layer 30a and the thermoplastic polyurethane layer 60 are mixed layers. That is, Figure 3 The modified blend layer 80 may be a blend of thermoplastic polyolefin, maleic acid and thermoplastic polyurethane. Figure 3 The modified blending layer 80 is a single-layer structure, which is different from Figure 2 The stacked structure 90a.

[0047] In some embodiments, Figure 3 As shown, the modified blending layer 80 has a first surface (e.g., lower surface) 81 and a second surface (e.g., upper surface) 82. The first surface 81 contacts the base fabric layer 10. The second surface 82 is opposite to the first surface 81. In some embodiments, the second surface 82 may be a corona-treated surface. In addition, in some embodiments, Figure 3 The base fabric layer 10 may be the same as Figure 2 The base fabric layer 10 is provided, and the thickness of the modified blended layer 80 may be less than or equal to the thickness of the base fabric layer 10.

[0048] Based on the above configuration, the polyurethane surface layer 50 can be attached to the modified blend layer 80 (eg, the second surface (corona treated surface) 82) through the paste 40. Figure 3 As shown, the paste 40 is disposed between the polyurethane surface layer 50 and the modified blend layer 80 (eg, the second surface (corona treated surface) 82). In some embodiments, Figure 3 The paste 40 may be the same as Figure 2 Paste 40, Figure 3 The polyurethane surface layer 50 may be the same as Figure 2 In some embodiments, the thickness of the paste 40 may be less than or equal to the thickness of the modified blend layer 80.

[0049] Figures 4 to 5 A schematic diagram showing one or more stages of some embodiments of the method for making artificial leather according to the present disclosure. In some embodiments, the method is for making Figure 1 The artificial leather 1 is shown.

[0050] See also Figure 4 , providing a base fabric layer 10. Figure 4 The base fabric layer 10 may be the same as Figure 1 The base fabric layer 10.

[0051] See also Figure 5, forming a laminated structure 90 on the base fabric layer 10 . Figure 5 The laminated structure 90 may be the same as Figure 1 The laminated structure 90. Therefore, Figure 5 The laminated structure 90 may include Figure 1 Thermoplastic polyolefin layer 20 and Figure 1 The modified thermoplastic polyolefin layer 30 is formed by a T-shaped coextrusion film head (not shown) to co-extrude the modified thermoplastic polyolefin layer 30 and the thermoplastic polyolefin layer 20 to form the laminated structure 90. In some embodiments, the modified thermoplastic polyolefin layer 30 may be a blend of thermoplastic polyolefin and maleic acid. In some embodiments, the content of maleic acid may be 3wt% to 50wt% based on the total weight of the modified thermoplastic polyolefin layer 30 as 100wt%. In some embodiments, the moisture content of the maleic acid may be 250PPM to 50PPM. When the moisture content of the maleic acid is higher than 250 PPM, the film forming property of the film co-extruded by the T-type co-extrusion film head is likely to be poor, and during heat processing of the finished product, holes may be sunken due to water evaporation; when the moisture content of the maleic acid is lower than 50 PPM, the required drying time is too long, which is contrary to the purpose of the present invention to reduce carbon emissions and energy consumption.

[0052] In some embodiments, Figure 5 As shown, after forming the laminated structure 90 (including, for example, the modified thermoplastic polyolefin layer 30 and the thermoplastic polyolefin layer 20), it may further include: performing corona treatment on the surface of the modified thermoplastic polyolefin layer 30 (for example, the second surface 32) to improve the surface polarity of the modified thermoplastic polyolefin layer 30. In some embodiments, the processing current of the corona treatment may be 3KW to 4.5KW, and the processing rate of the corona treatment may be 2.5m / min to 5m / min. When the processing current is lower than 3KW and the processing rate is higher than 5m / min, it is easy to cause the dyne to fail to meet the standard (need to be higher than 42); when the processing current is higher than 4.5KW and the processing rate is lower than 2.5m / min, it is easy to cause the material surface to be unable to bear the load, resulting in the material being broken down by the arc.

[0053] See also Figure 1 The polyurethane surface layer 50 is adhered to the laminated structure 90 (for example, the modified thermoplastic polyolefin layer 30) through the paste 40 to obtain Figure 1 The artificial leather 1 is shown.

[0054] The present invention performs corona treatment on the modified thermoplastic polyolefin layer 30 before laminating the polyurethane surface layer 50, which can improve the surface adhesion of the modified thermoplastic polyolefin layer 30, so that it can be well laminated with the polyurethane surface layer 50 through the paste 40, thereby achieving surface texture and color changes to meet the variability required for shoemaking.

[0055] In addition, the current processing temperature requirement for artificial leather embossing is about 220-240°C, while the constituent materials of the artificial leather 1 of the present invention can be embossed at 170-190°C, which can reduce the overall processing temperature requirement and achieve energy saving and carbon reduction effects.

[0056] Figure 6 A schematic diagram showing one or more stages of some embodiments of the method for making artificial leather according to the present disclosure. In some embodiments, the method is for making Figure 2 The artificial leather 1b shown. The initial stage of the process described is similar to Figure 4 Depicted for manufacturing Figure 1 The artificial leather 1 is the same or similar to the stage. Figure 6 Depiction Figure 4 The stage following the stage depicted.

[0057] See also Figure 6 , forming a laminated structure 90 a on the base fabric layer 10 . Figure 6 The laminated structure 90a may be the same as Figure 2 Therefore, Figure 6 The laminated structure 90a may include Figure 2 Thermoplastic polyurethane layer 60 and Figure 2 The modified thermoplastic polyolefin layer 30a is formed by coextruding the modified thermoplastic polyolefin layer 30a and the thermoplastic polyurethane layer 60 through a T-type coextrusion die head (not shown) to form the laminated structure 90a. In some embodiments, the modified thermoplastic polyolefin layer 30a may be a blend of thermoplastic polyolefin and maleic acid. In some embodiments, the content of maleic acid may be 3wt% to 50wt% based on the total weight of the modified thermoplastic polyolefin layer 30a as 100wt%. In some embodiments, the moisture content of the maleic acid may be 250PPM to 50PPM.

[0058] See also Figure 2 The polyurethane surface layer 50 is adhered to the laminated structure 90a (for example, the thermoplastic polyurethane layer 60) through the paste 40 to obtain Figure 2 The artificial leather 1a is shown.

[0059] The present invention is described in detail with the following examples, but it does not mean that the present invention is limited to the contents disclosed in the following examples.

[0060] [Example 1]

[0061] (1) Extruder setting parameters

[0062] Thermoplastic polyolefin (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0063] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0064] The T-Die die head temperature is set at 180°C.

[0065] (2) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (component B) is 1:3.

[0066] (3) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0067] (4) Use water-based polyurethane (PU) fabric to coat release paper (RP) to transfer the texture, and then use a non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After maturation, remove the RP to obtain the environmentally friendly artificial leather finished product.

[0068] [Example 2]

[0069] (1) Drying conditions

[0070] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0071] (2) Extruder setting parameters

[0072] A blend of thermoplastic polyolefin (70 wt%) of component A and maleic acid (30 wt%) of component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0073] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0074] The temperature of the T-type co-extrusion film head is set at 180℃.

[0075] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0076] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0077] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0078] [Example 3]

[0079] (1) Drying conditions

[0080] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0081] (2) Extruder setting parameters

[0082] A blend of thermoplastic polyolefin (50 wt%) as component A and maleic acid (50 wt%) as component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0083] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0084] The temperature of the T-type co-extrusion film head is set at 180℃.

[0085] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0086] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0087] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0088] [Example 4]

[0089] (1) Extruder setting parameters

[0090] Thermoplastic polyolefin (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0091] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0092] The temperature of the T-type co-extrusion film head is set at 180℃.

[0093] (2) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (component B) is 1:3.

[0094] (3) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0095] (4) Use water-based PU fabric to apply RP transfer pattern, and then use solvent-based paste (solvent content 65%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0096] [Example 5]

[0097] (1) Drying conditions

[0098] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0099] (2) Extruder setting parameters

[0100] A blend of thermoplastic polyolefin (70 wt%) of component A and maleic acid (30 wt%) of component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0101] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0102] The temperature of the T-type co-extrusion film head is set at 180℃.

[0103] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0104] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0105] (5) Use water-based PU fabric to apply RP transfer pattern, and then use solvent-based paste (solvent content 65%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0106] [Example 6]

[0107] (1) Drying conditions

[0108] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0109] (2) Extruder setting parameters

[0110] A blend of thermoplastic polyolefin (50 wt%) as component A and maleic acid (50 wt%) as component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0111] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0112] The temperature of the T-type co-extrusion film head is set at 180℃.

[0113] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0114] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0115] (5) Use water-based PU fabric to apply RP transfer pattern, and then use solvent-based paste (solvent content 65%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0116] [Example 7]

[0117] (1) Extruder setting parameters

[0118] Thermoplastic polyolefin (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0119] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0120] The temperature of the T-type co-extrusion film head is set at 180℃.

[0121] (2) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (component B) is 1:3.

[0122] (3) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0123] (4) Use water-based PU fabric to coat the RP transfer pattern, and then use a solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After maturation, remove the RP to obtain the environmentally friendly artificial leather finished product.

[0124] [Example 8]

[0125] (1) Drying conditions

[0126] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0127] (2) Extruder setting parameters

[0128] A blend of thermoplastic polyolefin (70 wt%) of component A and maleic acid (30 wt%) of component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0129] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0130] The temperature of the T-type co-extrusion film head is set at 180℃.

[0131] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0132] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0133] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0134] [Example 9]

[0135] (1) Drying conditions

[0136] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0137] (2) Extruder setting parameters

[0138] A blend of thermoplastic polyolefin (50 wt%) as component A and maleic acid (50 wt%) as component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0139] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0140] The temperature of the T-type co-extrusion film head is set at 180℃.

[0141] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0142] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0143] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0144] [Example 10]

[0145] (1) Extruder setting parameters

[0146] Thermoplastic polyolefin (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0147] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0148] The temperature of the T-type co-extrusion film head is set at 180℃.

[0149] (2) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (component B) is 1:3.

[0150] (3) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0151] (4) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a non-solvent paste. After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0152] [Example 11]

[0153] (1) Drying conditions

[0154] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0155] (2) Extruder setting parameters

[0156] A blend of thermoplastic polyolefin (70 wt%) of component A and maleic acid (30 wt%) of component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0157] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0158] The temperature of the T-type co-extrusion film head is set at 180℃.

[0159] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0160] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0161] (5) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a non-solvent paste. After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0162] [Example 12]

[0163] (1) Drying conditions

[0164] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0165] (2) Extruder setting parameters

[0166] A blend of thermoplastic polyolefin (50 wt%) as component A and maleic acid (50 wt%) as component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0167] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0168] The temperature of the T-type co-extrusion film head is set at 180℃.

[0169] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0170] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0171] (5) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the environmentally friendly artificial leather semi-finished product after the corona treatment through a non-solvent paste. After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0172] [Example 13]

[0173] (1) Extruder setting parameters

[0174] Thermoplastic polyolefin (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0175] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0176] The temperature of the T-type co-extrusion film head is set at 180℃.

[0177] (2) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (component B) is 1:3.

[0178] (3) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0179] (4) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a solvent-based paste (solvent content 65%). After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0180] [Example 14]

[0181] (1) Drying conditions

[0182] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0183] (2) Extruder setting parameters

[0184] A blend of thermoplastic polyolefin (70 wt%) of component A and maleic acid (30 wt%) of component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0185] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0186] The temperature of the T-type co-extrusion film head is set at 180℃.

[0187] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0188] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0189] (5) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a solvent-based paste (solvent content 65%). After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0190] [Example 15]

[0191] (1) Drying conditions

[0192] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0193] (2) Extruder setting parameters

[0194] A blend of thermoplastic polyolefin (50 wt%) as component A and maleic acid (50 wt%) as component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0195] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0196] The temperature of the T-type co-extrusion film head is set at 180℃.

[0197] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0198] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0199] (5) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a solvent-based paste (solvent content 65%). After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0200] [Example 16]

[0201] (1) Extruder setting parameters

[0202] Thermoplastic polyolefin (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0203] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0204] The temperature of the T-type co-extrusion film head is set at 180℃.

[0205] (2) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (component B) is 1:3.

[0206] (3) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0207] (4) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a solvent-based paste (solvent content 35%). After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0208] [Example 17]

[0209] (1) Drying conditions

[0210] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0211] (2) Extruder setting parameters

[0212] A blend of thermoplastic polyolefin (70 wt%) of component A and maleic acid (30 wt%) of component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0213] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0214] The temperature of the T-type co-extrusion film head is set at 180℃.

[0215] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0216] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0217] (5) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a solvent-based paste (solvent content 35%). After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0218] [Example 18]

[0219] (1) Drying conditions

[0220] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0221] (2) Extruder setting parameters

[0222] A blend of thermoplastic polyolefin (50 wt%) as component A and maleic acid (50 wt%) as component C was fed into the A axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0223] Thermoplastic polyolefin (100 wt %) of component B was fed into the B axis, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0224] The temperature of the T-type co-extrusion film head is set at 180℃.

[0225] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (the blend of components A and C) to the lower layer (component B) is 1:3.

[0226] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0227] (5) After the surface of the environmentally friendly artificial leather semi-finished product is corona treated, the RP transfer pattern is coated on a water-based PU fabric, and then the water-based PU fabric is adhered to the corona-treated environmentally friendly artificial leather semi-finished product through a solvent-based paste (solvent content 35%). After ripening, the RP is removed to obtain the environmentally friendly artificial leather finished product.

[0228] [Example 19]

[0229] (1) Drying conditions

[0230] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0231] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0232] (2) Extruder setting parameters

[0233] Thermoplastic polyurethane (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0234] The blend of thermoplastic polyolefin (90 wt %) of component B and maleic acid (10 wt %) of component C was fed into the B axis, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0235] The temperature of the T-type co-extrusion film head is set at 180℃.

[0236] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (the blend of components B and C) is 1:3.

[0237] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0238] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0239] [Example 20]

[0240] (1) Drying conditions

[0241] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0242] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0243] (2) Extruder setting parameters

[0244] Thermoplastic polyurethane (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0245] The blend of thermoplastic polyolefin (B component) (80 wt%) and maleic acid (C component) (20 wt%) was fed into the B axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0246] The temperature of the T-type co-extrusion film head is set at 180℃.

[0247] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (the blend of components B and C) is 1:3.

[0248] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0249] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0250] [Example 21]

[0251] (1) Drying conditions

[0252] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0253] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0254] (2) Extruder setting parameters

[0255] Thermoplastic polyurethane (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0256] The blend of thermoplastic polyolefin (70 wt%) of component B and maleic acid (30 wt%) of component C was fed into the B axis, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0257] The temperature of the T-type co-extrusion film head is set at 180℃.

[0258] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (the blend of components B and C) is 1:3.

[0259] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0260] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0261] [Example 22]

[0262] (1) Drying conditions

[0263] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0264] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0265] (2) Extruder setting parameters

[0266] Thermoplastic polyurethane (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0267] The blend of thermoplastic polyolefin (90 wt %) of component B and maleic acid (10 wt %) of component C was fed into the B axis, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0268] The temperature of the T-type co-extrusion film head is set at 180℃.

[0269] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (the blend of components B and C) is 1:3.

[0270] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0271] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0272] [Example 23]

[0273] (1) Drying conditions

[0274] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0275] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0276] (2) Extruder setting parameters

[0277] Thermoplastic polyurethane (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0278] The blend of thermoplastic polyolefin (B component) (80 wt%) and maleic acid (C component) (20 wt%) was fed into the B axis, and the extruder temperature was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0279] The temperature of the T-type co-extrusion film head is set at 180℃.

[0280] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (the blend of components B and C) is 1:3.

[0281] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0282] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0283] [Example 24]

[0284] (1) Drying conditions

[0285] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0286] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0287] (2) Extruder setting parameters

[0288] Thermoplastic polyurethane (100 wt%) of component A was fed into axis A, and the temperature of the extruder was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0289] The blend of thermoplastic polyolefin (70 wt%) of component B and maleic acid (30 wt%) of component C was fed into the B axis, and the temperature of the extruder was set to 170° C., 190° C., 185° C., and 180° C. in sequence.

[0290] The temperature of the T-type co-extrusion film head is set at 180℃.

[0291] (3) Adjust the speed of the metering pumps of the A and B axes so that the thickness ratio of the upper layer (component A) to the lower layer (the blend of components B and C) is 1:3.

[0292] (4) The plastics of the A and B axes are co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0293] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0294] [Example 25]

[0295] (1) Drying conditions

[0296] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0297] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0298] (2) Extruder setting parameters

[0299] A blend of thermoplastic polyurethane (48 wt%), thermoplastic polyolefin (48 wt%) and maleic acid (4 wt%) was fed into the A axis, and the extruder temperature was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0300] The temperature of the T-type co-extrusion film head is set at 180℃.

[0301] (3) Adjust the speed of the metering pump of the A-axis.

[0302] (4) The plastic of the A-axis is co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0303] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0304] [Example 26]

[0305] (1) Drying conditions

[0306] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0307] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0308] (2) Extruder setting parameters

[0309] A blend of thermoplastic polyurethane (32 wt %), thermoplastic polyolefin (64 wt %) and maleic acid (4 wt %) was fed into the A axis, and the extruder temperature was set to 180° C., 200° C., 190° C. and 180° C. in sequence.

[0310] The temperature of the T-type co-extrusion film head is set at 180℃.

[0311] (3) Adjust the speed of the metering pump of the A-axis.

[0312] (4) The plastic of the A-axis is co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0313] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0314] [Example 27]

[0315] (1) Drying conditions

[0316] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0317] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0318] (2) Extruder setting parameters

[0319] A blend of thermoplastic polyurethane (64 wt%), thermoplastic polyolefin (32 wt%) and maleic acid (4 wt%) was fed into the A axis, and the extruder temperature was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0320] The temperature of the T-type co-extrusion film head is set at 180℃.

[0321] (3) Adjust the speed of the metering pump of the A-axis.

[0322] (4) The plastic of the A-axis is co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0323] (5) Use water-based PU fabric to apply RP transfer pattern, and then use non-solvent paste to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0324] [Example 28]

[0325] (1) Drying conditions

[0326] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0327] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0328] (2) Extruder setting parameters

[0329] A blend of thermoplastic polyurethane (48 wt%), thermoplastic polyolefin (48 wt%) and maleic acid (4 wt%) was fed into the A axis, and the extruder temperature was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0330] The temperature of the T-type co-extrusion film head is set at 180℃.

[0331] (3) Adjust the speed of the metering pump of the A-axis.

[0332] (4) The plastic of the A-axis is co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0333] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0334] [Example 29]

[0335] (1) Drying conditions

[0336] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0337] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0338] (2) Extruder setting parameters

[0339] A blend of thermoplastic polyurethane (32 wt %), thermoplastic polyolefin (64 wt %) and maleic acid (4 wt %) was fed into the A axis, and the extruder temperature was set to 180° C., 200° C., 190° C. and 180° C. in sequence.

[0340] The temperature of the T-type co-extrusion film head is set at 180℃.

[0341] (3) Adjust the speed of the metering pump of the A-axis.

[0342] (4) The plastic of the A-axis is co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0343] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0344] [Example 30]

[0345] (1) Drying conditions

[0346] The moisture content of the thermoplastic polyurethane of component A is controlled within a range of 250 PPM to 50 PPM.

[0347] The moisture content of maleic acid in component C is controlled within a range of 250 PPM to 50 PPM.

[0348] (2) Extruder setting parameters

[0349] A blend of thermoplastic polyurethane (64 wt%), thermoplastic polyolefin (32 wt%) and maleic acid (4 wt%) was fed into the A axis, and the extruder temperature was set to 180° C., 200° C., 190° C., and 180° C. in sequence.

[0350] The temperature of the T-type co-extrusion film head is set at 180℃.

[0351] (3) Adjust the speed of the metering pump of the A-axis.

[0352] (4) The plastic of the A-axis is co-extruded through a T-type co-extrusion film extrusion head to form a film, which is then pressed together by a molding wheel and a silicone wheel and then poured onto the non-woven fabric. The molding wheel line speed is set to 3 m / min, and after being cooled and shaped by the molding wheel, an environmentally friendly artificial leather semi-finished product can be obtained.

[0353] (5) Use water-based PU fabric to coat RP transfer pattern, and then use solvent-based paste (solvent content 35%) to stick the water-based PU fabric to the environmentally friendly artificial leather semi-finished product. After ripening, remove RP to obtain the environmentally friendly artificial leather finished product.

[0354] The artificial leathers of Examples 1 to 18 correspond to Figure 1 The artificial leather 1 of Examples 19 to 24 corresponds to Figure 2 The artificial leather 1a of Examples 25 to 30 corresponds to Figure 3 The peel strength test results of Examples 1 to 30 are summarized in Table 1. From the results in Table 1, it can be found that the peel strengths of Examples 11, 12, 14, 15, 20, 21, 23 and 24 can all reach 4.5 kg / 2.54 cm or more, and the peel strengths of Examples 11 and 24 can even reach 7.1 kg / 2.54 cm.

[0355] Table 1. Peel strength test results of Examples 1 to 30

[0356]

[0357]

[0358]

[0359]

[0360] The above embodiments are only for explaining the principle and effect of the present invention, but not for limiting the present invention. After reading the above teachings, those skilled in the art can make appropriate modifications to the contents of the above embodiments, and still achieve the effect claimed by the present invention. The protection scope of the present invention shall be subject to the attached claims.

Claims

1. An artificial leather comprising: Base fabric layer; a thermoplastic polyolefin layer disposed on the base fabric layer; a modified thermoplastic polyolefin layer disposed on the thermoplastic polyolefin layer; as well as The polyurethane surface layer is adhered to the modified thermoplastic polyolefin layer by means of a paste.

2. The artificial leather according to claim 1, wherein the modified thermoplastic polyolefin layer is a blend of thermoplastic polyolefin and maleic acid.

3. The artificial leather according to claim 2, wherein the content of the maleic acid is 3wt% to 50wt%, based on the total weight of the modified thermoplastic polyolefin layer being 100wt%.

4. The artificial leather according to claim 1, wherein the adhesiveness of the modified thermoplastic polyolefin layer is greater than the adhesiveness of the thermoplastic polyolefin layer.

5. The artificial leather as claimed in claim 1, wherein the paste comprises one of the following: solvent-based polyurethane resin, water-based polyurethane resin, thermoplastic polyurethane resin, ethylene-vinyl acetate copolymer adhesive, polyvinyl chloride adhesive, polyolefin adhesive and epoxy resin adhesive.

6. An artificial leather comprising: Base fabric layer; A modified thermoplastic polyolefin layer, which is disposed on the base fabric layer; a thermoplastic polyurethane layer disposed on the modified thermoplastic polyolefin layer; as well as The polyurethane surface layer is adhered to the thermoplastic polyurethane layer by means of a paste.

7. The artificial leather according to claim 6, wherein the modified thermoplastic polyolefin layer is a blend of thermoplastic polyolefin and maleic acid, and the content of maleic acid is 3wt% to 50wt% based on the total weight of the modified thermoplastic polyolefin layer as 100wt%.

8. A method for producing artificial leather, comprising: providing a base fabric layer; forming a laminated structure on the base fabric layer, wherein the laminated structure comprises a modified thermoplastic polyolefin layer; as well as The polyurethane surface layer is adhered to the laminated structure by means of a paste.

9. The manufacturing method according to claim 8, wherein the modified thermoplastic polyolefin layer is a blend of thermoplastic polyolefin and maleic acid, and the moisture content of the maleic acid is 250 PPM to 50 PPM.

10. The manufacturing method according to claim 8, further comprising: The surface of the modified thermoplastic polyolefin layer is subjected to corona treatment, and the processing current of the corona treatment is 3 KW to 4.5 KW.

Citation Information

Patent Citations

  • Thermoplastic elastomer artificial leather and preparation method thereof

    CN108001024A

  • Polypropylene laminated material and manufacturing method thereof

    CN113524828A

  • Method for producing synthetic leather and the resultant synthetic leather

    JP2002339262A

  • Artificial leather and manufacturing method therefor

    WO2023279625A1

  • IT8020469A0