Laminated film
By using laser Raman spectroscopy analysis to optimize the orientation parameters of the laminated film in the flexible printed circuit substrate, the problem of insufficient puncture strength of the polyimide-based film in 5G communication applications was solved, and high puncture strength and appropriate dielectric properties were achieved. combination.
Patent Information
- Application Number
- CN202410360730.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-01
AI Technical Summary
In flexible printed circuit boards, it is difficult for polyimide-based films to improve mechanical properties while maintaining an appropriate range of dielectric properties. Especially when facing 5G communication applications for high-frequency bands, the puncture strength is insufficient.
By using a laminated structure of a polyimide-based resin-containing layer and a polyimide-based resin-containing layer in a laminated film, and analyzing the average orientation parameters of each layer using a laser Raman spectroscopy device, it can satisfy specific requirements. relationship to improve puncture strength.
A laminated film that achieves high puncture strength is suitable for high-speed communications applications such as 5G, while maintaining appropriate dielectric characteristics and mechanical properties.
Smart Images

Figure BDA0004762668900000031 
Figure BDA0004762668900000032 
Figure BDA0004762668900000041
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated film including a layer containing a polyimide-based resin, particularly a laminated film that can be used in substrate materials such as printed circuit boards and antenna substrates that can cope with high-frequency bands, a laminated sheet including the laminated film, and a flexible printed circuit board. Background Art
[0002] Flexible printed circuit substrate (hereinafter, sometimes recorded as FPC) is thin and light, flexible, and can realize three-dimensional, high-density installation. It is used in many electronic devices such as mobile phones and hard disks, which contributes to its miniaturization and lightness. In the past, polyimide resins with excellent heat resistance, mechanical properties, and electrical insulation were widely used in FPC. For example, as metal-clad laminates such as copper-clad laminates (hereinafter, sometimes abbreviated as CCL) for FPC, laminates with copper foil layers on one or both sides of polyimide films are known.
[0003] In recent years, the fifth generation mobile communication system called 5G has been widely used (for example, Patent Document 1), and polyimide films suitable for high-speed communication applications after 5G have been studied.
[0004] Patent Document 1: Japanese Patent Application Publication No. 2021-161285 Summary of the invention
[0005] For the polyimide film used in FPC, it is possible to apply an impact along the thickness direction of the film during processing, and a puncture strength that can withstand the impact is required. However, it is difficult to improve the mechanical properties while controlling the dielectric properties within an appropriate range. Therefore, it is considered necessary to develop a polyimide film with high puncture strength and that can be used for high-speed communication purposes after 5G.
[0006] An object of the present invention is to provide a laminate film having high puncture strength, a laminate sheet including the laminate film, and a flexible printed circuit board.
[0007] The inventors of the present application have conducted intensive research to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by making the average orientation parameters of each layer obtained by linear analysis of a cross section along the thickness direction of the laminated film using a laser Raman spectrometer satisfy a specific relationship in a laminated film including a layer (PI-1) containing a polyimide resin and a layer (PI-2) containing a polyimide resin, thereby completing the present invention. That is, the present invention provides the following preferred embodiments.
[0008] [1] A laminated film comprising a layer (PI-1) containing a polyimide resin and a layer (PI-2) containing a polyimide resin,
[0009] The thickness of the layer (PI-1) is 10 μm or more, the thickness of the layer (PI-2) is 2 μm or more,
[0010] The average orientation parameter of each layer obtained by linear analysis of a cross section along the thickness direction of the laminated film using a laser Raman spectrometer satisfies the relationship of formula (I).
[0011] (P1 / P2) / (|P1-P2|)≥0.70(I)
[0012] [wherein, P1 represents the average orientation parameter of the aforementioned layer (PI-1) within the range of 1.5 μm to 6.5 μm in the aforementioned thickness direction calculated from the end of the aforementioned layer (PI-1) on the aforementioned layer (PI-2) side, and P2 represents the average orientation parameter of the aforementioned layer (PI-2) within the range of ±0.5 μm in the aforementioned thickness direction calculated from the center of the aforementioned layer (PI-2), wherein the aforementioned average orientation parameter is obtained by (1615 cm in a polarization configuration consistent with the in-plane direction of the aforementioned laminated film) -1 Peak intensity near 725 cm / 725 cm in a polarization configuration consistent with the in-plane direction of the laminated film -1 Peak intensity near) / (1615cm in the polarization configuration consistent with the thickness direction of the aforementioned laminated film -1 Peak intensity near 725 cm / 725 cm in polarization configuration consistent with the thickness direction of the laminated film -1 The peak intensity near ) represents the average value of the orientation parameter]
[0013] [2] The laminated film according to [1], wherein in the formula (I), P1 is 5.70 or less.
[0014] [3] A laminated film as described in [1] or [2], wherein when the average orientation parameter of the aforementioned layer (PI-1) within the range of ±2.5 μm in the thickness direction of the aforementioned laminated film measured from the center of the aforementioned layer (PI-1) containing a polyimide resin is set to P1c, the relationship of formula (II) is satisfied.
[0015] P1c / P1>0.84(II)
[0016] [4] The laminated film according to any one of [1] to [3], wherein an intermediate region is provided between the polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2),
[0017] The intermediate region is a region where, when the elastic modulus of the cross section in the thickness direction of the laminated film is continuously measured along the thickness direction using a scanning probe microscope, the elastic modulus changes continuously from the average elastic modulus (1) of the layer (PI-1) to the average elastic modulus (2) of the layer (PI-2),
[0018] The thickness of the intermediate region is 50 nm or more.
[0019] [5] The laminated film according to any one of [1] to [4], wherein the thickness of the polyimide resin-containing layer (PI-2) is 0.05 to 0.3 times the thickness of the polyimide resin-containing layer (PI-1).
[0020] [6] The laminated film according to any one of [1] to [5], further comprising a layer (PI-3) containing a polyimide resin.
[0021] [7] The laminated film according to any one of [1] to [6], wherein at least one of the polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2) comprises a polyimide resin having a structural unit (A) derived from a tetracarboxylic anhydride,
[0022] The structural unit (A) includes a structural unit (A1) derived from a tetracarboxylic anhydride represented by the formula (A1) and / or a structural unit (A2) derived from a tetracarboxylic anhydride represented by the formula (A2).
[0023]
[0024] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0025] k represents an integer from 0 to 2]
[0026]
[0027] [In formula (A2), R a2 [ independently of one another, a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, and l independently of one another is an integer of 0 to 3]
[0028] [8] The laminated film according to any one of [1] to [7], wherein at least one of the polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2) comprises a polyimide resin having a structural unit (B) derived from a diamine,
[0029] The structural unit (B) includes a structural unit (B1) derived from a diamine represented by the formula (B1).
[0030]
[0031] [In formula (B1), R b1each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0032] W independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the aforementioned divalent linking group), R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted by a halogen atom,
[0033] m represents an integer from 1 to 4,
[0034] q independently represents an integer from 0 to 4]
[0035] [9] The laminated film according to any one of [1] to [8], wherein the polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2) comprise a polyimide resin having a structural unit (A) derived from a tetracarboxylic anhydride and a structural unit (B) derived from a diamine,
[0036] The structural unit (A) includes a structural unit (A1) derived from a tetracarboxylic anhydride represented by the formula (A1) and / or a structural unit (A2) derived from a tetracarboxylic anhydride represented by the formula (A2).
[0037] The structural unit (B) includes a structural unit (B1) derived from a diamine represented by the formula (B1).
[0038]
[0039] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0040] k represents an integer from 0 to 2]
[0041]
[0042] [In formula (A2), R a2 [ independently of one another, a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, and l independently of one another is an integer of 0 to 3]
[0043]
[0044] [In formula (B1), Rb1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0045] W independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the aforementioned divalent linking group), R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted by a halogen atom,
[0046] m represents an integer from 1 to 4,
[0047] q independently represents an integer from 0 to 4]
[0048]
[10] A laminate film as described in any one of [1] to [9], wherein the polyimide resin contained in the aforementioned polyimide resin-containing layer (PI-1) and the polyimide resin contained in the aforementioned polyimide resin-containing layer (PI-2) are different resins.
[0049]
[11] A laminated film as described in any one of [1] to
[10] , wherein the aforementioned polyimide resin-containing layer (PI-1) and the aforementioned polyimide resin-containing layer (PI-2) each contain a polyimide resin having at least two structural units (A) derived from tetracarboxylic anhydride.
[0050]
[12] The laminated film according to any one of [1] to
[11] , wherein at least the polyimide resin-containing layer (PI-1) comprises a polyimide resin having a structural unit (A) derived from a tetracarboxylic anhydride,
[0051] The structural unit (A) includes a structural unit (A3) derived from an ester bond-containing tetracarboxylic anhydride represented by the formula (A3).
[0052]
[0053] [In formula (A3), Z represents a divalent organic group,
[0054] R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0055] s independently represents an integer from 0 to 3]
[0056]
[13] A laminate film as described in any one of [9] to
[12] , wherein at least the aforementioned polyimide resin-containing layer (PI-1) comprises a polyimide resin having a structural unit (A) derived from tetracarboxylic anhydride, and the aforementioned structural unit (A) further comprises a structural unit (A3) derived from an ester-bonded tetracarboxylic anhydride represented by formula (A3) in an amount of 45 mol % or less relative to the total amount of the structural unit (A).
[0057]
[0058] [In formula (A3), Z represents a divalent organic group,
[0059] R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0060] s independently represents an integer from 0 to 3]
[0061]
[14] A laminated sheet comprising a metal layer on one or both sides of the laminated film according to any one of [1] to
[13] .
[0062]
[15] A flexible printed circuit board comprising the laminated sheet described in
[14] .
[0063] Effects of the Invention
[0064] According to the present invention, a laminated film having high puncture strength can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] [ Figure 1 ] is a schematic diagram showing the relationship between the polarization vibration direction of laser light and the direction of the sample cross section in the measurement method based on the laser Raman spectrometer in the present invention.
[0066] [ Figure 2 ] is a graph showing the relationship between the orientation parameter P and the distance in the thickness direction obtained by linear analysis using a laser Raman spectrometer in a laminate film involved in one embodiment of the present invention.
[0067] [ Figure 3 ] is a graph showing a force curve obtained at an arbitrary point on a cross section of a sample in a laminated film according to one embodiment of the present invention.
[0068] [ Figure 4 ] is a diagram showing a DMT elastic modulus image and coordinate axes of a cross section of a sample in a laminated film involved in one embodiment of the present invention.
[0069] [ Figure 5 ] to show Figure 4Figure 3 shows the locations of X=40, 80, 120, 160, and 200 in the DMT elastic modulus image.
[0070] [ Figure 6 ] to show Figure 4 A graph of the elastic modulus distribution diagram at X=40 in the DMT elastic modulus image.
[0071] [ Figure 7 ] is to show that Figure 4 The 9-point moving average of the average DMT elastic modulus distribution diagram obtained from the DMT elastic modulus image, the curve diagram of the middle area and its thickness.
[0072] [ Figure 8 ] is a schematic cross-sectional view showing an example of the layer structure of the laminated film of the present invention.
[0073] Description of Reference Numerals
[0074] 1: Sample (test piece)
[0075] 2: Layer (PI-2)
[0076] 3: Layer (PI-1)
[0077] 4: Thickness direction
[0078] 5: In-plane direction
[0079] 6: Laser polarization
[0080] 7: Vibration direction parallel to the in-plane direction
[0081] 8: Vibration direction parallel to the thickness direction
[0082] 9: Measurement location
[0083] 10: ±0.5μm range from the center of the layer (PI-2)
[0084] 11: Middle area
[0085] 11a: Interface between layer (PI-2) and the middle region
[0086] 11b: Interface between layer (PI-1) and the middle region
[0087] 12: The thickness direction of the layer (PI-1) from the end of the layer (PI-2) is within a range of 1.5 μm to 6.5 μm.
[0088] 13: ±2.5μm range from the center of the layer (PI-1)
[0089] 14: Laminated film
[0090] 15: Laminated Sheets
[0091] 16: Layer containing polyimide resin (corresponding to layer (PI-2))
[0092] 17: Layer containing polyimide resin (corresponding to layer (PI-1))
[0093] 18: Layer containing polyimide resin (corresponding to layer (PI-3))
[0094] 19: Metal foil layer DETAILED DESCRIPTION
[0095] Hereinafter, the embodiments of the present invention will be described in detail. It should be noted that the scope of the present invention is not limited to the embodiments described herein, and various changes can be made within the scope that does not damage the gist of the present invention. It should be noted that the multiple upper and lower limits described in this specification can be arbitrarily combined as a preferred numerical range.
[0096] [Laminated film]
[0097] The laminated film of the present invention comprises a layer (PI-1) containing a polyimide resin and a layer (PI-2) containing a polyimide resin, the thickness of the layer (PI-1) is greater than 10 μm, the thickness of the layer (PI-2) is greater than 2 μm, and the average orientation parameters of each layer obtained by linear analysis of a cross section along the thickness direction of the laminated film using a laser Raman spectrometer satisfy the relationship of formula (I).
[0098] (P1 / P2) / (|P1-P2|)≥0.70(I)
[0099] [wherein, P1 represents the average orientation parameter of layer (PI-1) within the range of 1.5 μm to 6.5 μm in the thickness direction as measured from the end of layer (PI-1) on the layer (PI-2) side, and P2 represents the average orientation parameter of layer (PI-2) within the range of ±0.5 μm in the thickness direction as measured from the center of layer (PI-2), and the average orientation parameter is obtained by (1615 cm in a polarization configuration consistent with the in-plane direction of the laminated film) -1 Peak intensity near 725 cm / 725 cm in a polarization configuration consistent with the in-plane direction of the laminated film -1 Peak intensity near) / (1615cm in polarization configuration consistent with the thickness direction of the laminated film -1 Peak intensity near 725 cm / 725 cm in polarization configuration aligned with the thickness direction of the laminated film -1 The peak intensity near ) represents the average value of the orientation parameter]
[0100] Hereinafter, “1615 cm in a polarization configuration aligned with the in-plane direction of the laminated film” may be referred to as -1Peak intensity near 725 cm / 725 cm in a polarization configuration consistent with the in-plane direction of the laminated film -1 The peak intensity near the IP , the 1615cm -1 Peak intensity near 725 cm / 725 cm in polarization configuration aligned with the thickness direction of the laminated film -1 The peak intensity near the ND . In this specification, the so-called layer containing polyimide resin refers to a layer composed of polyimide resin (sometimes referred to as PI resin). In the laminated film of the present invention, the PI resin contained in the layer containing PI resin usually contains aromatic PI resin. Aromatic PI resin is a PI resin containing an aromatic ring (preferably a benzene ring, a naphthalene ring, a biphenyl ring, etc.). In addition, the PI resin-containing layer containing aromatic PI resin is also particularly referred to as an aromatic PI resin-containing layer. In addition, in this specification, the layer (PI-1) containing polyimide resin is sometimes referred to as layer (PI-1), and the same is true for the layers containing polyimide resin other than layer (PI-1), which are sometimes expressed as layers (PI-2) and layers (PI-3).
[0101] In formula (I), P1 and P2 respectively represent average orientation parameters near the interface of layer (PI-1) and near the center of layer (PI-2) obtained by linear analysis of a cross section along the thickness direction of the laminated film using a laser Raman spectrometer. The orientation parameter (sometimes expressed as "P") is expressed by I IP / I ND express.
[0102] I in the orientation parameter P IP and I ND Medium, 1615cm -1 The peak intensity near 1615cm may be derived from the C=C stretching vibration of the aromatic ring in the PI resin. The C=C stretching vibration of the aromatic ring vibrates along the polymer chain of the PI resin. Therefore, the vibration direction of the C=C stretching vibration of the aromatic ring can be regarded as the orientation direction of the polymer chain. Therefore, if the orientation direction of the PI resin is consistent with the vibration direction of the laser polarization light, then 1615cm -1 If the peak intensity near 725cm is not consistent, the peak intensity will be weak. -1 The peak intensity near the PI resin may be derived from the CH angular vibration of the aromatic ring in the PI resin. The CH angular vibration of the aromatic ring is isotropic and hardly changes according to the vibration direction of the laser polarization light. Therefore, it can be used as a reference peak. IP / I ND ), I IPIt can be said that the ratio of the peak intensity derived from the C=C stretching vibration of the aromatic ring to the reference peak intensity when the cross section is irradiated with laser light having a polarization configuration consistent with the in-plane direction of the laminated film, i.e., a polarization vibration direction consistent with the in-plane direction, I ND It can be said that it is the ratio of the peak intensity from the CH angle vibration of the aromatic ring to the reference peak intensity when the laser beam with the polarization configuration consistent with the thickness direction of the laminated film, i.e., the polarization vibration direction consistent with the thickness direction, is irradiated to the cross section. That is, it can be said that: IP The larger the value, the higher the degree of in-plane orientation of the PI resin. ND The larger the value, the higher the degree of orientation of the PI resin in the thickness direction. Therefore, the orientation parameter P can be regarded as the ratio of the degree of orientation in the in-plane direction to the degree of orientation in the thickness direction. It should be noted that in this specification, the so-called "peak intensity" refers to the height of the peak, and the so-called "nearby" refers to ±30cm -1 The range is preferably ±10cm -1 The range is preferably ±5cm -1 For example, 1615cm -1 The peak intensity near 1615±30cm -1 In the range of 1615±10cm -1 More preferably, it is within the range of 1615±5cm -1 The maximum peak intensity within the range of. The in-plane direction of the aforementioned laminated film is not particularly limited as long as it is a direction perpendicular to the thickness direction of the laminated film, and any direction in the plane direction of the laminated film can be selected, preferably the TD direction. The so-called TD direction refers to the direction perpendicular to the mechanical travel direction when manufacturing the laminated film, and the so-called ND direction refers to the thickness direction of the laminated film, that is, the direction perpendicular to the laminated film surface.
[0103] P1 in formula (I) represents the average orientation parameter of layer (PI-1) within a range of 1.5 μm to 6.5 μm in the thickness direction from the end of layer (PI-1) on the layer (PI-2) side, that is, the average value of the orientation parameter P near the interface of layer (PI-1). In addition, P2 in formula (I) represents the average orientation parameter of layer (PI-2) within a range of ±0.5 μm in the thickness direction from the center of layer (PI-2), that is, the average value of the orientation parameter P near the center of layer (PI-2).
[0104] The inventors of the present application have conducted research focusing on the orientation of each layer that can be analyzed using a laser Raman spectrometer, and surprisingly found that if the specific average orientation parameter of each layer satisfies the relationship of formula (I): (P1 / P2) / (|P1-P2|)≥0.70, the puncture strength of the laminated film can be improved. Although the reason is unclear, it is believed that the balance of the orientation of each layer in the laminated film, that is, the balance of the mechanical properties of each layer caused by the orientation, is within a certain range, so that it becomes easy for the laminated film to absorb and disperse the force applied in the thickness direction.
[0105] The larger the P1 corresponding to the layer (PI-1), the smaller the P2 corresponding to the layer (PI-2), the larger the molecule (P1 / P2) in the formula (I). That is, the larger the (P1 / P2), the more differences will be produced in orientation between the PI-based resins constituting each layer, and the difference in orientation degree will be produced in the thickness direction of the laminated film, so it is easy to produce differences in the mechanical properties of each layer. Therefore, it becomes easy to disperse and absorb the force applied in the thickness direction, and it is believed that the puncture strength is improved. On the other hand, it is believed that if the absolute value of the difference between P1 and P2 in the denominator (|P1-P2|) in the formula (I) is too large, the difference in the mechanical property values of each layer becomes too large, and the mechanical properties of the laminated film are poorly balanced, resulting in the generation of strained parts or fragile parts, and the puncture strength cannot be fully improved. Therefore, it is believed that the smaller the denominator, the more conducive it is to improve the puncture strength. Therefore, it is considered that when (P1 / P2) / (|P1-P2|) in the laminated film increases to a predetermined value or more, the laminated film becomes less likely to break and the puncture strength is improved.
[0106] In the laminated film of the present invention, (P1 / P2) / (|P1-P2|) in formula (I) is preferably 0.80 or more, more preferably 0.90 or more, further preferably 1.00 or more, further more preferably 1.05 or more, particularly more preferably 1.20 or more, further particularly preferably 1.30 or more, and extremely preferably 1.40 or more. If the aforementioned (P1 / P2) / (|P1-P2|) is above the aforementioned lower limit, the puncture strength of the laminated film can be further improved. (P1 / P2) / (|P1-P2|) in formula (I) is preferably 10.0 or less, more preferably 8.00 or less, further preferably 6.00 or less, further preferably 4.00 or less, particularly preferably 3.00 or less, particularly more preferably 2.00 or less, for example, it may also be 1.50 or less, 1.43 or less, or 1.40 or less. If the aforementioned (P1 / P2) / (|P1-P2|) is below the aforementioned upper limit, the generation of burrs and the enlargement of burrs can be suppressed when a through hole is provided by processing using a drill or the like. It should be noted that, when the laminated film has three or more layers containing a PI-based resin, at least any two adjacent layers containing a PI-based resin satisfy the relationship of formula (I).
[0107] In one embodiment of the present invention, (P1 / P2) in formula (I) is preferably 0.50 or more, more preferably 0.70 or more, further preferably 0.90 or more, further preferably 1.20 or more, particularly preferably 1.50 or more, and particularly preferably 1.70 or more. If the aforementioned (P1 / P2) is above the aforementioned lower limit, it is easier to improve the puncture strength of the laminated film. (P1 / P2) in formula (I) is preferably 15.0 or less, more preferably 10.0 or less, further preferably 8.00 or less, further preferably 5.00 or less, particularly preferably 4.00 or less, particularly preferably 3.00 or less, further particularly preferably 2.00 or less, for example, it can also be 1.95 or less. If the aforementioned (P1 / P2) is below the aforementioned upper limit, when a through hole is provided by processing using a drill bit, etc., the generation of burrs and the enlargement of burrs can be suppressed.
[0108] In one embodiment of the present invention, (|P1-P2|) in formula (I) is preferably less than 10.0, more preferably less than 8.00, further preferably less than 5.00, further more preferably less than 4.00, particularly preferably less than 3.00, particularly more preferably less than 2.50, further particularly preferably less than 2.00, for example, it can also be less than 1.80. If the aforementioned (|P1-P2|) is below the aforementioned upper limit, it is easier to improve the puncture strength of the laminated film. The (|P1-P2|) in formula (I) is preferably more than 0.10, more preferably more than 0.30, further preferably more than 0.50, further more preferably more than 0.80, particularly preferably more than 1.00, for example, it can also be more than 1.20 or more than 1.30. If the aforementioned (|P1-P2|) is above the aforementioned lower limit, when a through hole is provided by processing using a drill bit, etc., the generation of burrs and the enlargement of burrs can be suppressed. It should be noted that, regarding |P1-P2|, from the viewpoint of improving the puncture strength, P1>P2 is preferred.
[0109] In one embodiment of the present invention, P1 in formula (I) is preferably less than 10.0, more preferably less than 8.00, further preferably less than 5.70, particularly preferably less than 4.50, particularly more preferably less than 3.80, further particularly preferably less than 3.50, and extremely preferably less than 3.00. In addition, P1 in formula (I) is preferably more than 0.50, more preferably more than 1.00, further preferably more than 1.50, further more preferably more than 2.00, particularly preferably more than 2.50, for example, more than 2.80 or more than 2.90. If the aforementioned P1 is the aforementioned range, it is easier to improve the puncture strength of the laminated film. In addition, when a through hole is provided by processing using a drill bit, the generation of burrs and the enlargement of burrs can be suppressed.
[0110] In one embodiment of the present invention, P2 in formula (I) is preferably 8.00 or less, more preferably 6.00 or less, further preferably 4.00 or less, further preferably 3.00 or less, particularly preferably 2.80 or less, particularly preferably 2.50 or less, further particularly preferably 2.00 or less, and extremely preferably 1.70 or less. In addition, P2 in formula (I) is preferably 0.10 or more, more preferably 0.50 or more, further preferably 0.80 or more, particularly preferably 1.00 or more, and particularly preferably 1.20 or more. If the aforementioned P2 is the aforementioned range, it is easier to improve the puncture strength of the laminated film. In addition, when a through hole is provided by processing using a drill bit, the generation of burrs and the enlargement of burrs can be suppressed.
[0111] In one embodiment of the present invention, for the laminated film of the present invention, it is preferred that when the average orientation parameter of layer (PI-1) within a range of ±2.5 μm in the thickness direction of the laminated film measured from the center of layer (PI-1) is set to P1c, the relationship of formula (II) is satisfied.
[0112] P1c / P1>0.84(II)
[0113] P1c in (II) represents the average value of the orientation parameter P near the center of layer (PI-1), and as mentioned above, P1 represents the average value of the orientation parameter P near the interface of layer (PI-2) side of layer (PI-1). Therefore, P1c / P1 is greater than 0.84, which means that in layer (PI-1), the average orientation parameter near the center is maintained at a high level or increases compared to the interface near the layer (PI-2) side. In addition, in this specification, (P1 / P2) / (|P1-P2|) in formula (I) and / or P1c / P1 in formula (II) are sometimes referred to as "parameter X".
[0114] If the laminated film of the present invention satisfies the relationship of formula (II), the puncture strength can be further improved. Although the reason is not clear, it is believed that the strength can be maintained at a high level not only near the interface on the layer (PI-2) side but also near the center of the layer (PI-1).
[0115] P1c / P1 in formula (II) is more preferably 0.85 or more, further preferably 0.86 or more, further preferably 0.90 or more, particularly preferably 0.95 or more, and particularly preferably 1.00 or more. If the aforementioned P1c / P1 is above the aforementioned lower limit, the puncture strength of the laminated film can be further improved. P1c / P1 in formula (II) is preferably 3.00 or less, more preferably 2.50 or less, further preferably 2.00 or less, further preferably 1.50 or less, particularly preferably 1.20 or less, and particularly preferably 1.12 or less. If the aforementioned P1c / P1 is below the aforementioned upper limit, when a through hole is provided by processing using a drill bit or the like, the generation of burrs and the enlargement of burrs can be suppressed.
[0116] P1c in formula (II) is preferably 0.50 or more, more preferably 1.00 or more, further preferably 2.00 or more, further more preferably 2.50 or more, particularly preferably 2.65 or more, for example, 3.00 or more, 3.50 or more, or 4.00 or more. In addition, P1c in formula (II) is preferably 15.0 or less, more preferably 10.0 or less, further preferably 8.00 or less, further more preferably 6.00 or less, particularly preferably 5.00 or less, particularly more preferably 4.00 or less, and further particularly preferably 3.50 or less. If the aforementioned P1c is within the aforementioned range, it is easier to improve the puncture strength of the laminated film, and in addition, when a through hole is provided by processing using a drill bit or the like, the generation of burrs and the enlargement of burrs can be suppressed.
[0117] Hereinafter, a measurement method of P1, P2, and P1c using a laser Raman spectrometer will be described. Figure 1 This is a schematic diagram showing the relationship between the polarization vibration direction of laser light and the direction of the sample cross section in the measurement method using a laser Raman spectrometer in the present invention.
[0118] Figure 2 This is a graph showing the relationship between the orientation parameter P and the distance in the thickness direction obtained by linear analysis using a laser Raman spectrometer in a laminated film according to one embodiment of the present invention. Figure 1 and Figure 2 These are diagrams for deepening understanding of the present invention, and the present invention is not limited to these embodiments.
[0119] (1-1) Preparation of test pieces (samples)
[0120] The method for preparing the test piece is not particularly limited as long as the cross section in the thickness direction of the laminated film can be observed, but in the case where the thickness of the laminated film is thin, it is preferred to embed a portion of the cut laminated film with resin to prepare a test piece cut by cross section. After embedding the resin in such a way that the cross section in the thickness direction is visible, the surface of the laminated film embedded with the resin (a cross section in the thickness direction in the laminated film) can be cut using, for example, a knife installed in a thin slicer, thereby cutting the cross section. It is preferred to cut along the in-plane direction and thickness direction (ND direction) of the laminated film to cut the cross section.
[0121] (1-2) Obtaining the Orientation Parameter P at Each Measurement Location on the Sample Cross Section
[0122] Sample 1 was placed in the laser Raman spectrometer so that the 1 / 2 wavelength plate was at 90°. Figure 1As shown, the angle of the sample 1 is adjusted in such a way that the vibration direction 7 of the laser polarization light 6 is parallel to the in-plane direction 5 (preferably the TD direction) of the sample 1, and Raman spectroscopic measurement is performed at multiple measurement locations 9 along the thickness direction 4 of the sample 1. The Raman spectroscopic measurement can be performed from the layer (PI-2) 2 side toward the layer (PI-1) 3 side, or vice versa.
[0123] Next, the 1 / 2 wavelength plate is changed to 0°, and the vibration direction of the laser polarized light 6 is changed from the vibration direction 7 to the vibration direction 8. As a result, the vibration direction 8 of the laser polarized light 6 becomes parallel to the thickness direction 4 of the sample 1. Under this setting, as above, Raman spectrometry is performed at multiple measurement locations 9 along the thickness direction 4 of the sample 1. It should be noted that the interval between the measurement locations 9 is less than 0.5 μm, preferably 0.5 μm. It should be noted that for the Raman spectrum obtained by Raman spectrometry, it is preferred to perform smoothing processing such as using a moving average method and fluorescence removal processing.
[0124] Next, in each case where the vibration direction of the laser polarization 6 coincides with the in-plane direction 5 (vibration direction 7) and the thickness direction 4 (vibration direction 8) of the sample 1, the Raman spectrum at 725 cm -1 The intensity of the peak near 1615 cm (attributable to the peak from the CH angle vibration of the aromatic ring) and -1 The intensity of the peak near the C=C stretching vibration of the aromatic ring can be obtained by the polarization configuration consistent with the in-plane direction 5. IP , and I under the polarization configuration consistent with the thickness direction 4 ND Thus, the orientation parameter P(I IP / I ND ).
[0125] (1-3) Calculation of average orientation parameters P1, P2, P1c, (P1 / P2) / (|P1-P2|) and P1c / P1
[0126] Using the method described in item (1-2) above, obtain Figure 1 After obtaining the orientation parameter P of each measuring position 9 along the thickness direction 4, the average value of the orientation parameter P measured at the measuring positions within the range specified by P1, P2 and P1c is calculated, thereby obtaining P1, P2 and P1c, and (P1 / P2) / (|P1-P2|) and P1c / P1 can be calculated from their values.
[0127] P1 is obtained by averaging the orientation parameter P in the range of 1.5 μm to 6.5 μm in the thickness direction from the end of the layer (PI-1) on the layer (PI-2) side. When the measurement is performed with the interval of the measurement position 9 being 0.5 μm (0.5 μm interval), it becomes the average value of the orientation parameter P of 11 points. Here, the end of the layer (PI-2) side of the layer (PI-1) represents the interface between the layer (PI-1) and the layer (PI-2). When there is an intermediate region described later between the layer (PI-1) and the layer (PI-2), it represents the interface between the layer (PI-1) and the intermediate region.
[0128] P2 is obtained by averaging the orientation parameter P within the range of ±0.5 μm in the thickness direction of the laminated film from the center of the layer (PI-2). When the interval between the measurement sites 9 is 0.5 μm (0.5 μm interval) and the measurement is performed, it becomes the average value of the orientation parameter P at three points. Here, when there is an intermediate region described later between the layers (PI-1) and (PI-2), the end of the layer (PI-2) on the side of the layer (PI-1) represents the interface between the layer (PI-2) and the intermediate region.
[0129] P1c is obtained by averaging the orientation parameters P within a range of ±2.5 μm in the thickness direction of the laminate film from the center of the layer (PI-1). When the measurement is performed with the intervals of the measurement points 9 being 0.5 μm (0.5 μm intervals), the orientation parameters P are averaged at 11 points.
[0130] In the laminated film of the present invention, the method for determining the end of layer (PI-1) on the layer (PI-2) side, the center of layer (PI-1), and the center of layer (PI-2) is not particularly limited, and examples thereof include a method using a scanning probe microscope (also referred to as SPM), a method using a laser microscope, and the like. In the case where there is no intermediate region, these positions can be determined by the thickness of each layer, and in the case where there is an intermediate region, these positions can be determined by determining the position of the intermediate region. For example, in Figure 2 The determination of these positions in a laminated film having an intermediate region between layer (PI-1) and layer (PI-2) is described in more detail in .
[0131] Figure 2The above Raman spectroscopic measurement is performed on a laminated film having a layer (PI-2), an intermediate region and a layer (PI-1) in sequence according to one embodiment of the present invention, and the orientation parameter P at each measurement position is measured, and the orientation parameter P is plotted on the vertical axis and the distance (μm) in the thickness direction is plotted on the horizontal axis to make a curve graph. The Raman spectroscopic measurement is measured from the surface of the layer (PI-2) toward the surface of the layer (PI-1), and therefore, from the left side of the curve graph to the right side, it corresponds to the layer (PI-2), the intermediate region and the layer (PI-1). The position of the intermediate region 11 is determined by the SPM measurement described later, thereby being able to determine the center of the layer (PI-2) [the center between the interface 11a between the layer (PI-2) and the intermediate region, and the surface of the layer (PI-2)] within a range of ±0.5μm 10. In addition, a range 12 of 1.5 μm to 6.5 μm in the thickness direction from the end of layer (PI-1) on the layer (PI-2) side [interface 11b between layer (PI-1) and the intermediate region] and a range 13 of ±2.5 μm from the center of layer (PI-1) [center between the end of layer (PI-1) on the layer (PI-2) side and the surface of layer (PI-1)]. It should be noted that P1, P2, P1c, (P1 / P2) / (|P1-P2|) and P1c / P1 can be obtained by, for example, the method described in the Examples.
[0132] In this specification, the intermediate region is a region where the DMT modulus of the cross section in the thickness direction of the laminated film is continuously measured along the thickness direction by SPM, and the DMT modulus of the cross section changes continuously from the average DMT modulus of the layer (PI-1) (1) to the average DMT modulus of the layer (PI-2) (2). It should be noted that in this specification, the "elastic modulus measured by a scanning probe microscope" is sometimes referred to as "elastic modulus based on SPM" or "DMT modulus".
[0133] Hereinafter, the intermediate region and the method of measuring its thickness using SPM will be described.
[0134] (2-1) Preparation of test pieces (samples)
[0135] The method for preparing the test piece is not particularly limited as long as the cross section in the thickness direction of the laminated film can be observed, and the sample can be obtained by the method described in the above-mentioned item (1-1).
[0136] (2-2) Obtaining DMT elastic modulus images of each layer
[0137] The DMT elastic modulus in the laminated film can be obtained by applying the DMT (Derjaguim-Muller-Toporov) theory to the relationship (force curve) between the deformation of the sample obtained by SPM and the load applied to the sample, and the mapping (mapping) measurement can be performed on the two-dimensional plane on the sample to obtain the DMT elastic modulus image. For example, a cantilever with a spring constant of 4 to 60 N / m can be installed on the SPM made by Bruker, and the P eak Force QNM (Quantitative Nanomechanical Mapping) mode is used for measurement to obtain the DMT elastic modulus image. It should be noted that it is preferred to include at least two adjacent layers and their interfaces within the range of obtaining the DMT elastic modulus image, and it is preferably set in a manner that the interface of the two adjacent layers is located near the center (near the center of the longitudinal axis (Y axis) of the DMT elastic modulus image).
[0138] Next, use Figure 3 and Figure 4 The details of the method for measuring the DMT elastic modulus at each point are described below. Figure 3 , Figure 4 and the following Figure 5 to Figure 7 These are diagrams for explaining the method of obtaining the position and thickness of the intermediate region in an easily understandable manner, and the present invention is not limited to these embodiments.
[0139] Figure 3 FIG. 4 is a graph showing a force curve obtained at an arbitrary point on a cross section of a sample in a laminated film according to an embodiment of the present invention. Figure 4 This is a diagram showing a DMT elastic modulus image and coordinate axes of a cross section of a sample in a laminated film according to one embodiment of the present invention. Figure 3 In the force curve, the vertical axis (applied load / nN) is represented by the load F=kd, and the horizontal axis (indentation depth / nm) is represented by the deformation of the sample δ=Δz-d. k represents the spring constant (N / m), d represents the spring deflection (m), and z represents the needle position (m). d can be detected by laser, and z can be sensed by a piezoelectric scanner.
[0140] First, if the cantilever is brought close to the sample, the tip of the cantilever probe is pressed into the sample until the maximum load is reached after contact with the sample. Figure 3As shown in the figure, the force curve of the pressing process can be obtained (point A → point B → point C). At point B, when in contact with the sample, the load is applied in the negative direction due to the influence of the adhesion force. Next, if the cantilever that has been pressed into the sample to the maximum load is pulled back, the cantilever probe will be unloaded and adhered to the sample surface, and then it will leave the sample surface. Figure 3 As shown, the force curve of the pulling back process can be obtained (point C→point D→point E).
[0141] The DMT modulus of elasticity at each point can be calculated by analyzing the force curve of the pullback process based on the DMT theoretical formula. Specifically, when the numerical value of the minimum to maximum value of the load F value in the pullback process of the force curve is replaced with a numerical value of 0 to 1, fitting is performed for a range of 0.05 to 0.7 to calculate the DMT modulus of elasticity. The DMT modulus of elasticity is obtained by obtaining the DMT modulus of elasticity at all measuring points within the range of the DMT modulus of elasticity image. In addition, the analysis based on the DMT theoretical formula can be performed by using the analysis software (e.g., NanoScope Analysisver.2.00) attached to SPM, a known method, and in the latter case, it can be calculated using, for example, the following formula (a) etc.
[0142] [Mathematical formula 1]
[0143]
[0144] [Where F represents the load (force induced by the cantilever (spring)), F elas Stress representing elastic deformation, F adh represents adhesion, E represents elastic modulus (Pa or N / m 2 ), R is the tip radius of the cantilever probe (m), δ is the indentation depth (m), and w is the adhesion energy (N / m or J / m 2 ), as F adh , which can be substituted into the minimum value of the force curve (the F value at point E)]
[0145] In the SPM measurement, the measurement atmosphere can be carried out at room temperature, for example, 24°C, in the atmosphere, and the moving speed of the cantilever can be set to 0.4 μm / s and the maximum load can be set to 40 nN. In addition, the spring constant of the cantilever and the tip radius of the probe can be calculated using the values built into the SPM device or using a known method. For example, the spring constant can be a value calculated using the Sader method, and the tip radius of the probe can be a value calculated using the reconstruction method.
[0146] (2-3) Calculation of average DMT elastic modulus of each layer
[0147] When the DMT elastic modulus image obtained above [the upper side is layer (PI-2), the lower side is layer (PI-1), and the interface of the two adjacent layers is set to a position near the center of the Y axis of the DMT elastic modulus image] is converted into coordinates, for example, when the Y coordinate of the DMT elastic modulus image is recorded as 0 to 1 from top to bottom and the X coordinate is recorded as 0 to 1 from left to right, the average value of the DMT elastic modulus from (X, Y) = (0, 0) to (1, 0.4) is calculated, and the average DMT elastic modulus (2) of the layer (PI-2) can be obtained. In addition, the average value of the DMT elastic modulus from (X, Y) = (0, 0.6) to (1, 1) is calculated, and the average DMT elastic modulus (1) of the layer (PI-1) can be obtained. Figure 4 The figure shows a DMT modulus image obtained by measuring 256 points in the horizontal direction and 256 points in the vertical direction within a range of 5 μm in the horizontal direction (in-plane direction) and 5 μm in the vertical direction (thickness direction) of the sample cross section, and the coordinates are arranged such that the upper left end is (X, Y) = (0, 0), the lower left end is (X, Y) = (0, 255), the upper right end is (X, Y) = (255, 0), and the lower right end is (X, Y) = (255, 255). The average DMT modulus (2) of the layer (PI-2) can be obtained by calculating the average value of the DMT modulus of 256 × 100 points from (0, 0) to (255, 99), and the average DMT modulus (1) of the layer (PI-1) can be obtained by calculating the average value of the DMT modulus of 256 × 129 points from (X, Y) = (0, 126) to (255, 255).
[0148] In the above-described manner, the average DMT elastic modulus (1) of the layer (PI-1) and the average DMT elastic modulus (2) of the layer (PI-2) can be determined.
[0149] For the range of obtaining the above-mentioned DMT elastic modulus image, the distance in the horizontal direction (in-plane direction) and the vertical direction (thickness direction) is preferably 0.05 to 0.6 times the thickness of the laminated film, more preferably 0.08 to 0.5 times, and further preferably 0.1 to 0.4 times. For example, in a laminated film with a thickness of 20 to 65 μm, the range of obtaining the DMT elastic modulus image is 3 μm or more in horizontal direction × 3 μm or more in vertical direction, preferably 5 μm or more in horizontal direction × 5 μm or more in vertical direction, more preferably 10 μm or more in horizontal direction × 10 μm or more in vertical direction, and can be 10 μm or more in horizontal direction × 10 μm or more in vertical direction. In addition, from the viewpoint of improving the accuracy of obtaining the intermediate region, the number of points (parts) for measuring the DMT elastic modulus may be 100 points or more × 100 points or more, preferably 128 points or more × 128 points or more, more preferably 200 points or more × 200 points or more, further preferably 256 points or more × 256 points or more, and further more preferably 512 points × 512 points. The resolution is uniquely determined by the range of obtaining the DMT elastic modulus image and the number of measurement points. When the thickness of the intermediate region is small, it is preferred to measure at a resolution of preferably 40 nm / pixel or less, more preferably 20 nm / pixel or less.
[0150] (2-4) Middle area and its thickness
[0151] An example of a method of calculating the thickness of the intermediate region will be described. Figure 5 To show Figure 4 Figure 3 shows the locations of X=40, 80, 120, 160, and 200 in the DMT elastic modulus image. Figure 6 To show Figure 4 A graph of the DMT elastic modulus distribution diagram at X=40 in the DMT elastic modulus image. Figure 7 To show that Figure 4 The 9-point moving average of the average DMT elastic modulus distribution diagram and the thickness curve of the middle area obtained from the DMT elastic modulus image (the middle area near the 9-point moving average of the average DMT elastic modulus distribution diagram is selected, and the Y coordinate is re-marked in such a way that the middle area is near the center).
[0152] In the DMT elastic modulus image obtained above (the DMT elastic modulus image in which the Y coordinate is recorded as 0 to 1 from top to bottom and the X coordinate is recorded as 0 to 1 from left to right), for example, at positions separated by an interval of 0.2 on the X coordinate, a DMT elastic modulus distribution diagram corresponding to Y=0 to 1 is obtained (horizontal axis: pixel, vertical axis: DMT elastic modulus (GP a)). Specifically, in the DMT elastic modulus image, the DMT elastic modulus at X=0.2, Y=0 to 1 [(X, Y)=(0.2, 0) to (0.2, 1)] is plotted as the vertical axis and the corresponding Y coordinate is plotted as the horizontal axis, thereby obtaining a DMT elastic modulus distribution diagram at X=0.2. This DMT elastic modulus distribution diagram is also prepared for other X positions. That is, in the DMT elastic modulus image, a distribution diagram of the DMT elastic modulus continuously measured along the thickness direction of the laminated film is obtained on a plurality of lines spaced at equal intervals along the in-plane direction of the laminated film.
[0153] Next, for the obtained multiple DMT elastic modulus distribution maps, the average value of the DMT elastic modulus is calculated according to the Y coordinate (0 to 1) of each DMT elastic modulus image, and an average DMT elastic modulus distribution map is prepared. Furthermore, in the average DMT elastic modulus distribution map, a 9-point moving average line of the average DMT elastic modulus distribution map is prepared. At this time, the Y coordinate of the DMT elastic modulus image on the horizontal axis is converted from the pixel unit to the nm unit. Next, if a horizontal line (referred to as horizontal line 1) corresponding to the average DMT elastic modulus (1) of the layer (PI-1) obtained above and a horizontal line (referred to as horizontal line 2) corresponding to the average DMT elastic modulus (2) of the layer (PI-2) obtained above are drawn in the curve chart of the 9-point moving average line of the average DMT elastic modulus distribution map, the area between these horizontal lines 1 and 2 can be regarded as the intermediate area, and the width of the area (the distance of the Y coordinate) can be regarded as the thickness of the intermediate area. That is, the intermediate region can be said to be a region where, when the DMT elastic modulus of the thickness direction cross section of the laminated film is continuously measured along the thickness direction, the DMT elastic modulus continuously changes from the average DMT elastic modulus (1) of the layer (PI-1) to the average DMT elastic modulus (2) of the layer (PI-2).
[0154] The number of distribution graphs acquired to obtain the average DMT elastic modulus distribution graph may be 3 or more points, preferably 5 or more points, and more preferably 5 points. In addition, the moving average may be 5 or more points, preferably 9 or more points, and more preferably 9 points.
[0155] From the viewpoint of accurately measuring the average DMT elastic modulus (1) of the layer (PI-1), the average DMT elastic modulus (2) of the layer (PI-2), and the thickness of the intermediate region, when the thickness of the intermediate region exceeds 60% of the range for obtaining the elastic modulus image, it is preferred to enlarge the field of view and measure again. The thickness of the intermediate region is preferably less than 60% of the range for obtaining the elastic modulus image.
[0156] The range of the average DMT elastic modulus of the measured layer (PI-1) and the layer (PI-2) is the range excluding the middle area between the layer (PI-1) and the layer (PI-2), and can be appropriately changed according to the range of the obtained DMT elastic modulus image and the size of the middle area. The range can be determined by predicting the approximate position of the middle area from the aforementioned DMT elastic modulus image, but it is preferably determined on the basis of confirming the area where the DMT elastic modulus changes discontinuously on the moving average line of the aforementioned average DMT elastic modulus distribution diagram. Although not limited, in one embodiment of the present invention, for example, Figure 7 In the 9-point moving average shown, there is an intermediate region where the DMT modulus changes continuously between the roughly wavy portion (1) corresponding to the layer (PI-1) and the roughly wavy portion (2) corresponding to the layer (PI-2), and the range from the top (maximum value) of the mountain closest to the intermediate region of the roughly wavy portion (1) to the top (minimum value) of the valley closest to the intermediate region of the roughly wavy portion (2) can be excluded, and the average DMT modulus (1) of the layer (PI-1) and the average DMT modulus (2) of the layer (PI-2) can be measured. In addition, the average DMT modulus (1) and the average DMT modulus (2) are each preferably obtained from measurement values of preferably 1500 points or more, more preferably 2000 points or more, further preferably 3000 points or more, and particularly preferably 5000 points or more.
[0157] The position and thickness of the intermediate region can be determined by the above-mentioned method. It should be noted that the intermediate region and its thickness can be obtained by, for example, the method described in the examples.
[0158] Below, use Figure 5 to Figure 7 , an example of a method for calculating the position and thickness of the intermediate area is described in more detail. Figure 5 To show Figure 4 Figure 3 shows the locations of X=40, 80, 120, 160, and 200 in the DMT elastic modulus image. Figure 6 for Figure 4The DMT elastic modulus distribution graph at X=40 in the DMT elastic modulus image is a graph obtained by plotting the DMT elastic modulus at X=40, Y=0~255 [(X, Y)=(40, 0)~(40, 255)] as the vertical axis and the corresponding Y coordinate as the horizontal axis. In the same manner, in the DMT elastic modulus image, DMT elastic modulus distribution graphs corresponding to Y=0~255 are prepared at X=80, 120, 160, and 200, respectively, thereby obtaining distribution graphs of the DMT elastic modulus continuously measured along the thickness direction of the laminated film on 5 lines. For the 5 obtained DMT elastic modulus distribution graphs, the average value of the DMT elastic modulus is calculated according to the Y coordinate (0~255) of each DMT elastic modulus image to prepare an average DMT elastic modulus distribution graph, and then, in the average DMT elastic modulus distribution graph, a distribution graph as shown in the following is prepared. Figure 7 The 9-point moving average line of the average DMT elastic modulus distribution diagram shown in FIG. The position of the middle region and the thickness of the middle region can be obtained based on the graph of the 9-point moving average line of the average DMT elastic modulus distribution diagram, the horizontal line 1 representing the average DMT elastic modulus value of the layer (PI-1), and the horizontal line 2 representing the average DMT elastic modulus value of the layer (PI-2).
[0159] In one embodiment of the present invention, the laminated film of the present invention preferably has the aforementioned intermediate region between layer (PI-1) and layer (PI-2). By making the laminated film of the present invention have the aforementioned intermediate region, the puncture strength of the laminated film can be further improved. It is inferred that this is because if there is an intermediate region in which the DMT elastic modulus of the pullback process corresponding to the elastic deformation changes continuously along the thickness direction, it becomes easy to disperse and absorb the force applied along the thickness direction.
[0160] The thickness of the middle region is usually 50 nm or more, preferably 100 nm or more, more preferably 250 nm or more or more than 250 nm, further preferably 270 nm or more, further more preferably 300 nm or more, particularly preferably 350 nm or more, particularly preferably 380 nm or more, further particularly preferably 450 nm or more, further more particularly preferably 600 nm or more, extremely preferably 1000 nm or more, extremely more preferably 1500 nm or more, further extremely preferably 1700 nm or more, extremely particularly preferably 2000 nm or more, extremely particularly preferably 2300 nm or more, for example, 2600 nm or more or 2700 nm or more. If the thickness of the middle region is above the aforementioned lower limit, it becomes easier to disperse and absorb the force applied in the thickness direction, so the puncture strength of the laminated film can be further improved. In addition, the thickness of the middle region is usually less than 10000nm, preferably less than 8000nm, more preferably less than 5000nm, and more preferably less than 3500nm. For example, it can be less than 3000nm, less than 2800nm, or less than 2700nm. If the thickness of the middle region is below the above-mentioned upper limit, when the through hole is set by processing using a drill bit, the generation of burrs and the enlargement of burrs can be suppressed. It should be noted that when the laminated film has more than 3 layers of PI-containing resin layers, it is preferred that the thickness of the middle region between at least any two adjacent layers of PI-containing resin layers satisfies the above-mentioned range.
[0161] (P1 / P2) / (|P1-P2|) in formula (I), P1c / P1 in formula (II), and the thickness of the intermediate region can be controlled by appropriately adjusting the types of structural units of the PI resin contained in each PI resin-containing layer and their composition, the molecular weight of the PI resin, the composition of each PI resin-containing layer in the laminated film and its combination, and / or the coating conditions during film formation, the state of the multilayer coating film during imidization, the imidization conditions and other manufacturing methods. For example, (P1 / P2) / (|P1-P2|) in formula (I), P1c / P1 in formula (II), and the thickness of the intermediate region can be appropriately adjusted based on the preferred modes that are advantageous for the improvement of puncture strength, the reduction of Df, etc., such as the structural units and their contents of the preferred PI resin described later, the solvents contained in the preferred PI resin precursor solution described later, the state of the multilayer coating film during imidization described later, the preferred imidization conditions described later, etc. In particular, as described later, by imidizing in a state where the solvent is sufficiently present in the entire multilayer coating film (or in a well-fused state), preferably after a standing step described later, there is a tendency for (P1 / P2) / (|P1-P2|) in formula (I), P1c / P1 in formula (II), and the thickness of the intermediate region to increase, and the parameter X and the thickness of the intermediate region can be adjusted to the above-mentioned desired range. In addition, by making the solvent sufficiently present in the entire multilayer coating film during imidization, making each adjacent PI-containing resin layer different layers (preferably mPI layers and TPI layers, respectively), and / or making each adjacent PI-containing resin layer have different thicknesses, there is a tendency for (P1 / P2) / (|P1-P2|) in formula (I), P1c / P1 in formula (II), and the thickness of the intermediate region to increase, and it is easy to adjust these parameters X and the thickness of the intermediate region to the desired range.
[0162] <Layer composition>
[0163] A preferred configuration for obtaining a laminated film satisfying formula (I) is described. The laminated film satisfying formula (I) has high puncture strength, and particularly preferably has high puncture strength and dielectric properties suitable for high-speed communication applications such as 5G.
[0164] It should be noted that in this specification, so-called dielectric properties refer to the dielectric-related properties such as Df and Dk, and the so-called dielectric properties increase or improve, which means that Df and / or Dk reduce. In addition, so-called mechanical properties refer to the mechanical properties including puncture strength, bending resistance and elastic modulus (including DMT elastic modulus), and the so-called mechanical properties increase or improve, which means that for example puncture strength, bending resistance and / or elastic modulus become higher. In addition, thermal properties may include CTE, glass transition temperature (hereinafter, sometimes recorded as Tg), the degree of degeneration and deterioration caused by heat, etc., and the so-called thermal properties increase or improve, which means that for example CTE becomes lower, Tg becomes higher, and / or the degeneration and deterioration caused by heat are less, etc.
[0165] The laminated film of the present invention comprises a layer (PI-1) containing a PI-based resin and a layer (PI-2) containing a PI-based resin. The laminated film of the present invention may include other layers containing PI-based resins in addition to these layers containing PI-based resins, and may also include other layers in addition to the layers containing PI-based resins. As other layers, an adhesive layer for bonding the layer containing PI-based resin to a metal layer (e.g., a metal foil layer) and the like can be cited. In a preferred embodiment of the present invention, from the viewpoint of improving the puncture strength of the laminated film, the laminated film of the present invention preferably includes a layer (PI-3) containing a PI-based resin in addition to the layer (PI-1) containing a PI-based resin and the layer (PI-2) containing a PI-based resin. In such an embodiment, from the viewpoint of improving the puncture strength of the laminated film, the laminated film of the present invention preferably comprises a layer (PI-2) containing a PI-based resin, a layer (PI-1) containing a PI-based resin, and a layer (PI-3) containing a PI-based resin in sequence, and more preferably comprises a layer (PI-2) containing a PI-based resin, a layer (PI-1) containing a PI-based resin, and a layer (PI-3) containing a PI-based resin in sequence in an adjacent manner. It should be noted that a laminated film comprising a layer (PI-1) containing a PI-based resin, a layer (PI-2) containing a PI-based resin, and a layer (PI-3) containing a PI-based resin (sometimes expressed as layers (PI-1) to (PI-3) containing a PI-based resin or layers (PI-1) to (PI-3)) is sometimes referred to as a laminated film (L).
[0166] The laminated film 14 in the preferred embodiment of the present invention is as follows Figure 8As shown, it is composed of three adjacent layers of PI-containing resin 16, PI-containing resin 17 and PI-containing resin 18, which are stacked on a metal foil 19 to form a laminated sheet 15. From the perspective of easily controlling the parameter X and the thickness of the middle region within the above-mentioned specific range and achieving higher puncture strength and dielectric properties, it is preferred that the PI-containing resin layer 16 is equivalent to layer (PI-2), the PI-containing resin layer 17 is equivalent to layer (PI-1), and the PI-containing resin layer 18 is equivalent to layer (PI-3). In addition, the laminated film 14 may also include other PI-containing resin layers other than layer (PI-1), layer (PI-2) and layer (PI-3), and other layers other than the PI-containing resin layer. As other layers, adhesive layers formed by polymer materials such as acrylic resins other than PI resins can be cited.
[0167] In one embodiment of the present invention, the thickness of the laminated film is preferably 20 μm or more, more preferably 25 μm or more, further preferably 30 μm or more, further preferably 35 μm or more, particularly preferably 40 μm or more, preferably 150 μm or less, more preferably 130 μm or less, further preferably 100 μm or less, further preferably 90 μm or less, particularly preferably 80 μm or less, particularly preferably 70 μm or less, and further particularly preferably 60 μm or less. If the thickness of the laminated film is within the aforementioned range, the laminated film can have mechanical properties such as high puncture strength and flexibility suitable for flexible printed circuit boards. In addition, the Df of the laminated film can be reduced and the puncture strength can be increased, so that a laminated film with mechanical properties suitable for flexible printed circuit boards and dielectric properties suitable for high-speed communication applications such as 5G can be obtained with good balance.
[0168] In the laminated film of the present invention, the thickness of layer (PI-1) is more than 10 μm, and the thickness of layer (PI-2) is more than 2 μm. If the thickness of layer (PI-1) and layer (PI-2) is more than the aforementioned lower limit, the puncture strength of the laminated film can be further improved. The thickness of layer (PI-1) is preferably more than 15 μm, more preferably more than 20 μm, more preferably more than 30 μm, preferably less than 80 μm, more preferably less than 60 μm, more preferably less than 55 μm, and further more preferably less than 50 μm. In addition, the thickness of layer (PI-2) is preferably more than 2.5 μm, more preferably more than 3 μm, more preferably more than 3.5 μm, preferably less than 20 μm, more preferably less than 15 μm, more preferably less than 10 μm, and further more preferably less than 8 μm. It should be noted that the thickness of each layer can be measured using, for example, a laser microscope, SPM, etc. For example, when the laminated film has an intermediate region between layer (PI-1) and layer (PI-2), the intermediate region and its thickness can be obtained using SPM, and the distance to the interface between the surface of layer (PI-1) and the intermediate region is used as the thickness of layer (PI-1), and the distance to the interface between the surface of layer (PI-2) and the intermediate region is used as the thickness of layer (PI-2). In addition, for example, when the laminated film (L) has an intermediate region 1 between layer (PI-1) and layer (PI-2), and an intermediate region 2 between layer (PI-1) and layer (PI-3), the thickness of layer (PI-1) can be obtained by calculating intermediate region 1, intermediate region 2, layer (PI-2) and layer (PI-3) as described above and deducting their total thickness from the thickness (total thickness) of the laminated film. It should be noted that the thickness of each layer can be obtained using, for example, the method described in the embodiment.
[0169] When the laminated film of the present invention has a layer (PI-3), the thickness of the layer (PI-3) can be selected from the range of the thickness of the above-mentioned layer (PI-2). The thickness of the layer (PI-2) and the thickness of the layer (PI-3) may be the same as or different from each other, but from the viewpoint of suppressing the warping of the laminated film, the value of one is preferably within the range of ±25% of the value of the other, and more preferably within the range of ±20%.
[0170] In one embodiment of the present invention, the thickness of layer (PI-2) is preferably 0.05 to 0.3 times the thickness of layer (PI-1). When the aforementioned thickness is in the aforementioned relationship, the laminated film can have mechanical properties such as high puncture strength and flexibility suitable for flexible printed circuit boards. In addition, the Df of the laminated film can be reduced, and the puncture strength can be increased, so that a laminated film with mechanical properties suitable for flexible printed circuit boards and dielectric properties suitable for high-speed communication purposes such as 5G can be obtained with good balance. Especially when the thickness of the laminated film is 20 to 100 μm and the thickness of the layer (PI-2) is 0.05 to 0.3 times the thickness of the layer (PI-1), it is easier to obtain the aforementioned effect of the present invention. The thickness of the layer (PI-2) is more preferably 0.08 times or more relative to the thickness of the layer (PI-1), more preferably 0.10 times or more, particularly preferably 0.12 times or more, more preferably 0.25 times or less, more preferably 0.23 times or less, and particularly preferably 0.20 times or less. In addition, when the laminated film of the present invention has a layer (PI-3), the thickness of the layer (PI-3) can be selected from the range of the above-mentioned layer (PI-2).
[0171] In the laminated film of the present invention, the polyimide resin constituting layer (PI-1) and layer (PI-2) is not particularly limited in type as long as it satisfies formula (I), but from the viewpoint of maintaining excellent dielectric properties and improving puncture strength, layer (PI-1) and layer (PI-2) are each preferably a layer containing a non-thermoplastic polyimide resin (hereinafter sometimes described as an mPI layer) or a layer containing a thermoplastic polyimide resin (hereinafter sometimes described as a TPI layer), and more preferably, one of layer (PI-1) and layer (PI-2) is an mPI layer and the other is a TPI layer.
[0172] The mPI layer is generally the main layer containing PI-based resin in the laminated film used for flexible printed circuit substrates. The TPI layer is a layer that can also function as an adhesive layer for bonding the laminated film to a metal layer (e.g., a metal foil layer such as copper foil), and is preferably located in the outermost layer in the laminated film that can be in contact with the metal layer.
[0173] In a laminated film including layers of a PI-based resin having three or more layers, it is preferable that at least one layer of the PI-based resin layer is an mPI layer, and at least one layer (preferably at least two layers) of the PI-based resin layer is a TPI layer. More preferably, a TPI layer, an mPI layer, and a TPI layer are provided in this order. Therefore, in the laminated film (L), the layer (PI-1) is preferably an mPI layer, and each of the layer (PI-2) and the layer (PI-3) is preferably a TPI layer. If the laminated film (L) has such a layer structure, improved thermal properties can be ensured in the mPI layer, thermal deformation and deterioration can be suppressed, and the dimensional stability of the laminated film can be ensured. Also, the adhesiveness with a metal layer (for example, a metal foil layer such as a copper foil) can be improved using the TPI layer.
[0174] In the case where the laminated film (L) includes multiple layers of TPI layers or mPI layers, the structures of the multiple layers of TPI layers or mPI layers included can be the same or different from each other. Also, in the laminated film (L), generally, the structure of the layer (PI-1) is different from the structures of the layer (PI-2) and the layer (PI-3), but the structures of the layer (PI-2) and the layer (PI-3) can be the same or different.
[0175] <PI-based resin>
[0176] In the laminated film of the present invention, the PI-based resin constituting each PI-based resin layer only needs to be a PI-based resin that can form a PI-based resin layer in a manner that satisfies formula (I). The PI-based resin is a resin containing a repeating structural unit including an imide group, and may also contain a repeating structural unit including both an imide group and an amide group.
[0177] It should be noted that in the present invention, the so-called "non-thermoplastic" polyimide-based resin means that the storage elastic modulus at 40°C measured using a dynamic viscoelasticity measuring device (DMA) is 1.0×10 9 Pa or more, and the storage elastic modulus at 300°C is 1.0×10 8 Pa or more. The so-called "thermoplastic" polyimide-based resin means that the storage elastic modulus at 40°C is 1.0×10 9 Pa or more, and the storage elastic modulus at 300°C is less than 1.0×10 8 Pa. It should be noted that the storage elastic modulus can be measured using, for example, the method described in the examples.
[0178] In the present invention, from the viewpoint of improving the puncture strength and dielectric properties of the laminated film, the PI-based resin constituting each layer containing the PI-based resin preferably comprises a structural unit (A) derived from tetracarboxylic anhydride and a structural unit (B) derived from a diamine. It should be noted that in the present invention, the so-called "structural unit derived from..." refers to "structural unit derived from...", for example, "structural unit (A) derived from tetracarboxylic anhydride" refers to "structural unit (A) derived from tetracarboxylic anhydride". In addition, the so-called "layer containing the PI-based resin includes structural unit (A)" means that the "PI-based resin constituting the layer containing the PI-based resin includes structural unit (A)", and the same applies to other structural units.
[0179] (Structural unit (A) derived from tetracarboxylic anhydride)
[0180] The structural unit (A) derived from a tetracarboxylic anhydride (hereinafter, sometimes simply referred to as structural unit (A)) is preferably a structural unit derived from a tetracarboxylic anhydride represented by the formula (1), for example.
[0181]
[0182] [In formula (1), Y represents a tetravalent organic group]
[0183] In formula (1), Y each independently represents a tetravalent organic group, preferably a tetravalent organic group having 4 to 40 carbon atoms, and more preferably a tetravalent organic group having 4 to 40 carbon atoms having a cyclic structure. Examples of the cyclic structure include alicyclic rings, aromatic rings, and heterocyclic structures. For the aforementioned organic group, the hydrogen atoms in the organic group may be substituted by a halogen atom, a hydrocarbon group, an alkoxy group, or a halogenated hydrocarbon group, in which case the carbon atoms of these groups are preferably 1 to 8. In the present invention, the PI-based resin may contain a plurality of Ys, and the plurality of Ys may be the same or different. Examples of Y include: groups or structures represented by formulas (31) to (40); groups obtained by replacing the hydrogen atoms in the groups represented by formulas (31) to (40) with methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, fluoro, chloro, or trifluoromethyl groups; and tetravalent chain hydrocarbon groups having 1 to 8 carbon atoms.
[0184]
[0185] [In formula (31) to formula (33), R 19 ~R 26 and R 23’ ~R 26’ each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms, and R 19 ~R 26 and R 23’ ~R 26’The hydrogen atoms contained in may be replaced by halogen atoms independently of one another,
[0186] V 1 and V 2 Each independently represents a single bond (excluding the case where e+d=1), -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -SO2-, -S-, -CO-, -N(R j )-, or formula (a):
[0187]
[0188] (In formula (a), R 27 ~R 30 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms,
[0189] D independently represents a single bond, -C(CH3)2- or -C(CF3)2,
[0190] i represents an integer from 1 to 3,
[0191] * indicates a connection key),
[0192] R j represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted by a halogen atom,
[0193] e and d independently represent an integer from 0 to 2 (wherein e+d is not 0),
[0194] f represents an integer from 0 to 3,
[0195] g and h independently represent an integer of 0 to 4,
[0196] In formula (39), Z represents a divalent organic group,
[0197] R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0198] s independently represent an integer from 0 to 3,
[0199] In formula (40), R a2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0200] l independently represent integers from 0 to 3,
[0201] * indicates a connection key].
[0202] In the present invention, from the viewpoint of improving the puncture strength, dielectric properties, thermal properties, etc. of the laminated film, the PI-based resins constituting each PI-based resin-containing layer preferably contain at least one structure selected from the group consisting of structures represented by formula (31), formula (32), formula (33), formula (39) and formula (40) as Y in formula (1), more preferably contain at least one structure selected from the group consisting of structures containing a benzene skeleton as Y in formula (1), and further preferably contain at least one structure selected from the group consisting of structures represented by formula (32), formula (39) and formula (40) as Y in formula (1).
[0203] In formula (31) to formula (33), R 19 ~R 26 and R 23’ ~R 26’ Independently of each other, they are preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and still more preferably a hydrogen atom.
[0204] In formula (31), V 1 and V 2 Preferably, each independently represents a single bond (excluding the case where e+d=1), -O-, -CH2-, -C(CH3)2-, -C(CF3)2- or -CO-, and more preferably represents a single bond (excluding the case where e+d=1), -O-, -C(CH3)2- or -C(CF3) 2- .
[0205] In formula (31), e and d are each independently preferably 0 or 1 (wherein e+d is not 0). In addition, e+d is preferably 1. It should be noted that in formula (31), when e is 0, it means that the two benzene rings are not connected by V 1 When d is 0, it means that the two benzene rings are not bonded through V 2 Perform bonding.
[0206] In formula (32) and formula (33), f preferably represents 0 or 1, and more preferably represents 0.
[0207] In formula (33), g and h are preferably an integer of 0 to 2, more preferably 0 or 1. In addition, g+h is preferably an integer of 0 to 2. When f is 1 or more, a plurality of g and h may be the same or different from each other independently.
[0208] In formula (a), R 27 ~R 30 Each of them independently represents preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably represents a hydrogen atom. i is preferably 1 or 2. When i is 2 or more, a plurality of D and R 27 ~R30 They can be the same or different independently of each other.
[0209] In formula (39), Z preferably represents a divalent organic group having 4 to 40 carbon atoms, more preferably represents a divalent organic group having 4 to 40 carbon atoms having a cyclic structure, further preferably represents a divalent organic group having 4 to 40 carbon atoms having an aromatic ring, particularly preferably represents a divalent organic group selected from the group consisting of formula (z1), formula (z2) and formula (z3), and particularly more preferably represents a divalent organic group represented by formula (z1).
[0210]
[0211] [In formula (z1) to formula (z3), R z11 ~R z14 Each independently represents a hydrogen atom or a monovalent hydrocarbon group which may have a halogen atom, and R z2
[0066] independently represent a monovalent hydrocarbon group which may have a halogen atom, n represents an integer of 1 to 4, j independently represent an integer of 0 to 3, and * represents a connecting bond]
[0212] In formula (z1), R z11 ~R z14 Preferably, they are independently a hydrogen atom or an alkyl group which may have a halogen atom, more preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, further preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms which may have a halogen atom, and particularly preferably a hydrogen atom. z11 ~R z14 In the benzene ring, R z11 ~R z14 At least one of them may be a monovalent hydrocarbon group which may have a halogen atom, but R z11 ~R z14 All are hydrogen atoms.
[0213] In formula (z1), n preferably represents an integer of 1 to 3, more preferably represents 1 or 2, and further preferably represents 2.
[0214] In formula (z2), R z2 Independently of each other, preferably, they represent an alkyl group which may have a halogen atom, more preferably, they represent an alkyl group which may have a halogen atom and has 1 to 6 carbon atoms, and even more preferably, they represent an alkyl group which may have a halogen atom and has 1 to 3 carbon atoms.
[0215] In the formula (z2), j's are preferably independently 0 or 1, more preferably 0, and even more preferably all j's are 0.
[0216] In formula (39), R a3Preferably, they each independently represent an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms.
[0217] R a3 The hydrogen atoms contained in may be substituted by halogen atoms independently of each other, among which R a3 Each of them independently represents preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.
[0218] In formula (39), s each independently represents an integer of preferably 0 to 2, and more preferably represents 0 or 1.
[0219] In formula (40), R a2 Preferably, they each independently represent an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms.
[0220] R a2 The hydrogen atoms contained in can be substituted by halogen atoms independently of each other, among which, as R a2 , independently of each other, preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms.
[0221] In formula (40), l each independently represents an integer of preferably 0 to 2, and more preferably represents 0 or 1.
[0222] Specific examples of the structures represented by Formulae (31) to (33), (39) and (40) include structures represented by Formulae (41) to (56). In these formulae, * represents a connecting bond.
[0223]
[0224] In one embodiment of the present invention, when the PI resin constituting the layer containing the PI resin contains at least one selected from the group consisting of structures represented by formula (31) to formula (33), formula (39) and formula (40) as Y in formula (1), the ratio of the structural unit derived from the tetracarboxylic anhydride represented by at least one selected from the group consisting of structures represented by formula (31) to formula (33), formula (39) and formula (40) relative to the total amount of structural unit (A), especially the ratio of the structural unit derived from the tetracarboxylic anhydride represented by at least one selected from the group consisting of structures represented by formula (32), formula (39) and formula (40) in formula (1) is preferably 30 mol% or more, more preferably 50 mol% or more, further preferably 70 mol% or more, particularly preferably 90 mol% or more, and preferably 100 mol% or less. If the above ratio is within the above range, it is advantageous from the perspective of improving the puncture strength and dielectric properties of the laminated film.
[0225] The ratio of the aforementioned structural units can be determined using, for example, 1 H-NMR can be used to measure, or it can be calculated from the input ratio of raw materials. Below, it is the same in the calculation of the ratio of the structural unit of PI-based resin. In addition, in this specification, the "total amount" of the so-called structural unit, when the structural unit is formed by one unit, represents the amount of the unit, and when the structural unit is formed by more than two units, represents the total amount of these units.
[0226] (Structural unit (A1) and structural unit (A2))
[0227] In one embodiment of the present invention, it is preferred that the PI-based resin contained in at least one of the layers (PI-1) and (PI-2), or at least one of the layers (PI-1) to (PI-3) constituting the laminated film of the present invention comprises a structural unit (A), wherein the structural unit (A) comprises a structural unit (A1) derived from a tetracarboxylic anhydride represented by formula (A1) (hereinafter, sometimes abbreviated as structural unit (A1)) and / or a structural unit (A2) derived from a tetracarboxylic anhydride represented by formula (A2) (hereinafter, sometimes abbreviated as structural unit (A2)).
[0228]
[0229] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0230] k represents an integer from 0 to 2]
[0231]
[0232] [In formula (A2), R a2 [ independently of one another, a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, and l independently of one another is an integer of 0 to 3]
[0233] It should be noted that, in the present specification, "at least one layer among the layers containing a PI-based resin" or "at least one layer containing a PI-based resin" can be replaced by "at least one layer among the layers (PI-1) containing a PI-based resin and the layers (PI-2) containing a PI-based resin, or at least one layer among the layers (PI-1) to (PI-3) containing a PI-based resin."
[0234] If the PI-based resin contains structural unit (A1) and / or structural unit (A2) as structural unit (A), it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which can improve the puncture strength and dielectric properties. In addition, there is a tendency for the CTE of the laminated film to decrease, and it is expected that the dimensional stability of the laminated film will be improved.
[0235] From the viewpoint of improving puncture strength, dielectric properties, CTE, etc., in formula (A1) and formula (A2), R a1 and R a2 Preferably, they are each independently an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms.
[0236] Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 2-methylbutyl, 3-methylbutyl, 2-ethylpropyl, and n-hexyl.
[0237] Examples of the alkoxy group having 1 to 6 carbon atoms include methoxy, ethoxy, propyloxy, isopropyloxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, pentyloxy, hexyloxy and cyclohexyloxy.
[0238] Examples of the aryl group having 6 to 12 carbon atoms include phenyl, tolyl, xylyl, naphthyl and biphenyl.
[0239] R a1 and R a2 The hydrogen atoms contained in may be independently substituted by halogen atoms, and examples of the halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. a1 and R a2 Each of them is independently preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.
[0240] The bonding positions of the two carboxylic anhydrides bonded to the benzene ring in formula (A1) are not particularly limited, but are preferably 1,2-position and 4,5-position, or 1,2-position and 3,4-position, more preferably 1,2-position and 4,5-position from the viewpoint of improving puncture strength, dielectric properties, CTE, etc. k is preferably 0 or 1, more preferably 0.
[0241] The bonding positions of the two carboxylic anhydrides bonded to the benzene ring constituting the biphenyl skeleton in formula (A2) are not particularly limited, and can be 3,4-, or 2,3- independently of each other, based on the single bond bonding the two benzene rings. From the perspective of improving puncture strength, dielectric properties, CTE, etc., 3,4- is preferred.
[0242] In the formula (A2), 1 is preferably an integer of 0 to 2, more preferably 0 or 1, and further preferably 0, each independently.
[0243] In a preferred embodiment of the present invention, formula (A1) is a structural unit (A1-1) represented by formula (A1-1). In another preferred embodiment of the present invention, formula (A2) is a structural unit (A2-1) represented by formula (A2-1).
[0244]
[0245] If the PI-based resin contains structural unit (A1-1) and / or structural unit (A2-1) as structural unit (A), it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which is beneficial for improving the puncture strength and dielectric properties. In addition, there is a tendency for the CTE of the laminated film to decrease, and it is expected that the dimensional stability of the laminated film will be improved.
[0246] In one embodiment of the present invention, the layer containing the PI-based resin preferably includes any one or more of the following structures.
[0247] In the layer (PI-1) and the layer (PI-2), or the layers (PI-1) to (PI-3) in the laminated film, the PI-based resin each contains at least one of the structural unit (A1) and the structural unit (A2);
[0248] In the layer (PI-1) and the layer (PI-2), or the layers (PI-1) to (PI-3) in the laminated film, the PI-based resins each contain the structural unit (A1);
[0249] In at least one layer containing a PI-based resin in the laminated film, preferably a TPI layer, the PI-based resin contains a structural unit (A1) and a structural unit (A2);
[0250] In at least one layer containing a PI-based resin in the laminate film, preferably a TPI layer, the PI-based resin contains structural units (A1) and structural units (A2), and in at least another layer containing a PI-based resin, preferably an mPI layer, the PI-based resin contains structural units (A1) and / or structural units (A2).
[0251] · In at least one layer containing a PI-based resin in the laminated film, preferably a TPI layer, the PI-based resin contains structural units (A1) and structural units (A2), and in at least one other layer containing a PI-based resin, preferably an mPI layer, the PI-based resin contains structural units (A1) and substantially does not contain structural units (A2). It should be noted that in this specification, the so-called "substantially free of structural units" means: the content of the structural unit is 1% by mass or less, preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and particularly preferably 0.001% by mass or less. For example, the so-called substantially free of structural units (A2) means: relative to the total amount of structural units (A), the content of structural units (A2) is 1% by mass or less, preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and particularly preferably 0.001% by mass or less. Below, unless otherwise clearly stated, the same applies to other structural units.
[0252] In one embodiment of the present invention, when the PI resin includes structural units (A1) and / or structural units (A2), relative to the total amount of structural units (A), the content thereof is preferably 10 mol% or more, more preferably 15 mol% or more, further preferably 20 mol% or more, further preferably 25% or more, particularly preferably 30 mol% or more, and preferably 90 mol% or less, more preferably 85 mol% or less, further preferably 80 mol% or less, further preferably 75 mol% or less, particularly preferably 70 mol% or less. If the contents of structural units (A1) and structural units (A2) are each within the above range, it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which is conducive to improving the puncture strength and dielectric properties. In addition, there is a tendency for the CTE of the laminated film to decrease, and it is expected that the dimensional stability of the laminated film will be improved.
[0253] In addition, in one embodiment of the present invention, when the PI-based resin contains the structural unit (A1) and the structural unit (A2), the content ratio (molar ratio, (A1): (A2)) is preferably 10:90 to 90:10, more preferably 15:85 to 80:20, further preferably 20:80 to 70:30, and further more preferably 25:75 to 65:35. If the content ratio of the structural unit (A1) to the structural unit (A2) is within the above range, the above-mentioned effect of the present invention that can be expected due to the PI-based resin having the structural unit (A1) and / or the structural unit (A2) can be easily obtained, and the effect can be further improved.
[0254] (Structural unit (A3))
[0255] In one embodiment of the present invention, the PI-based resin contained in at least one of the layers (PI-1) and (PI-2), or at least one of the layers (PI-1) to (PI-3) constituting the laminated film of the present invention may also contain a structural unit (A3) derived from an ester-bonded tetracarboxylic anhydride represented by formula (A3) (hereinafter sometimes abbreviated as structural unit (A3)) as the structural unit (A).
[0256]
[0257] [In formula (A3), Z represents a divalent organic group,
[0258] R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0259] s independently represents an integer from 0 to 3]
[0260] If the PI-based resin contains structural unit (A3) as structural unit (A), it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which will be beneficial to improve the puncture strength and dielectric properties of the laminated film. In addition, there is a tendency for the CTE of the laminated film to decrease, and it is expected that the dimensional stability of the laminated film will be improved. In addition, even at a relatively low temperature (e.g., below 360°C) of the imidization temperature, the puncture strength and dielectric properties can be improved. Therefore, even if the PI-based resin precursor coating is thermally imidized to manufacture a laminated sheet by stacking with a metal layer (e.g., a metal foil layer such as copper foil), the degradation of the metal layer surface can be suppressed, and a laminated sheet having high puncture strength and excellent high-frequency characteristics can be obtained.
[0261] As R in formula (A3) a3 , which is the same as R in the formula (39) described above. a3 The same groups as exemplified have the same preferred aspects.
[0262] In formula (A3), s's are each independently preferably 0 or 1, and more preferably 0.
[0263] Examples of Z in the formula (A3) include the same divalent organic groups as exemplified as Z in the above-described formula (39), and preferred aspects are also the same.
[0264] In a preferred embodiment of the present invention, formula (A3) is preferably a structural unit (A3-1) represented by formula (A3-1) or a structural unit (A3-2) represented by formula (A3-2).
[0265]
[0266] If the PI-based resin contained in at least one layer of the PI-based resin-containing layer constituting the laminated film contains structural units (A3-1) and / or structural units (A3-2) as structural units (A), it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which will be beneficial to improve the puncture strength and dielectric properties of the laminated film. In addition, there is a tendency for the CTE of the laminated film to decrease, and it is expected that the dimensional stability of the laminated film will be improved. In addition, even at a relatively low temperature (e.g., below 360°C) of the imidization temperature, the puncture strength and dielectric properties can be improved. Therefore, even if the PI-based resin precursor coating is thermally imidized to manufacture a laminated sheet by stacking it with a metal layer (e.g., a metal foil layer such as copper foil), the degradation of the metal layer surface can be suppressed, and a laminated sheet having high puncture strength and excellent high-frequency characteristics can be obtained.
[0267] In one embodiment of the present invention, if the PI resin constituting at least one layer of the laminated film, preferably at least layer (PI-1), more preferably the mPI layer, contains a structural unit (A3), especially a structural unit (A3-1) and / or a structural unit (A3-2) as a structural unit (A), the PI resin is not too rigid and becomes a soft structure with a certain degree of freedom. Therefore, it is easy to form a branched structure by heating during imidization, which can further improve the puncture strength of the laminated film. In addition, there is a tendency that the Df of the laminated film is easy to be further reduced, and the CTE is reduced, and the dimensional stability of the laminated film is increased.
[0268] In one embodiment of the present invention, when the PI-based resin contains structural units (A3), the content thereof is preferably 3 mol% or more, more preferably 5 mol% or more, further preferably 7 mol% or more, further more preferably 10 mol% or more, for example, 20 mol% or more, 30 mol% or more, or 40 mol% or more. In addition, the content of structural units (A3) is preferably 80 mol% or less, more preferably 70 mol% or less, further preferably 65 mol% or less, further more preferably 60 mol% or less. If the content of structural units (A3) is within the above range, it is easy to obtain the above-mentioned effect of the present invention that can be expected due to the PI-based resin having structural units (A3), and in addition, the effect can be further improved.
[0269] In another embodiment of the present invention, the structural unit (A) possessed by the PI-based resin contained in at least the layer (PI-1) containing the PI-based resin contains a structural unit (A3) preferably at a content of 45 mol% or less (0 to 45 mol%) relative to the total amount of the structural unit (A). That is, in such an embodiment, the structural unit (A) possessed by the PI-based resin may not contain the structural unit (A3), or may contain the structural unit (A3). When the structural unit (A3) is contained, it is contained in an amount of 45 mol% or less. In addition, relative to the total amount of the structural unit (A), the content of the structural unit (A3) is more preferably 35 mol% or less, further preferably 25 mol% or less, further more preferably 15 mol% or less, particularly preferably 5 mol% or less, particularly more preferably 1 mol% or less, and the lower limit may be 0 mol%. If the content of the structural unit (A3), especially the structural unit (A3-1) and / or the structural unit (A3-2) in the PI-based resin is below the above upper limit, it is easier to control the parameter X in the laminated film and the thickness of the intermediate region within the desired range, and the puncture strength and dielectric properties of the laminated film can be further improved. In addition, there is a tendency for the CTE of the laminated film to decrease, and it is expected that the dimensional stability of the laminated film will be improved.
[0270] In one embodiment of the present invention, in at least one layer containing a PI-based resin constituting a laminated film, preferably a TPI layer, the PI-based resin comprises structural units (A1) and structural units (A2), and in at least one other layer containing a PI-based resin, preferably an mPI layer, the PI-based resin more preferably comprises at least two structural units selected from structural units (A1), structural units (A2) and structural units (A3) (preferably structural units (A1) and structural units (A2) and / or structural units (A3)).
[0271] (Structural unit (A4))
[0272] In one embodiment of the present invention, the PI-based resin may contain, as the structural unit (A), a structural unit (A4) derived from tetracarboxylic anhydride other than the structural unit (A1), the structural unit (A2) and the structural unit (A3) (hereinafter, sometimes simply referred to as the structural unit (A4)).
[0273] It should be noted that, in the present specification, the “structural unit (A4) derived from tetracarboxylic anhydride other than the structural unit (A1), the structural unit (A2) and the structural unit (A3)” refers to a structural unit derived from tetracarboxylic anhydride that does not belong to any of the structural unit (A1), the structural unit (A2) and the structural unit (A3), and the “content of the structural unit (A4)” refers to the total amount of the structural unit (A4) when a plurality of structural units (A4) are present.
[0274] In one embodiment of the present invention, as the structural unit (A4), for example, a structural unit derived from a tetracarboxylic anhydride in which Y in formula (1) is represented by formula (31), formula (33) to formula (38) can be cited. From the viewpoint of improving the puncture strength and dielectric properties of the laminated film, a structural unit derived from a tetracarboxylic anhydride in which Y in formula (1) is represented by formula (42), formula (44) to formula (49) or formula (53) is preferred, and a structural unit derived from a tetracarboxylic anhydride in which Y in formula (1) is represented by formula (42), formula (46), formula (49) or formula (53) is more preferred.
[0275] In one embodiment of the present invention, when the PI-based resin contains structural units (A4), its content relative to the total amount of structural units (A) can be, for example, 0.01 to 55 mol%, or 0.01 to 40 mol%, preferably 40 mol% or less, more preferably 35 mol% or less, further preferably 30 mol% or less, particularly preferably 25 mol% or less, and is generally 0.01 mol% or more, preferably 10 mol% or more.
[0276] (Structural unit (B) derived from diamine)
[0277] The PI resin constituting each PI resin-containing layer generally contains a structural unit (B) derived from a diamine (hereinafter, sometimes simply referred to as structural unit (B)). The structural unit (B) is preferably a structural unit derived from a diamine represented by formula (2).
[0278] H2N—X—NH2(2)
[0279] [In formula (2), X represents a divalent organic group]
[0280] In formula (2), X represents a divalent organic group, preferably a divalent organic group having 2 to 100 carbon atoms. As the divalent organic group, for example, a divalent aromatic group, a divalent aliphatic group, etc. can be cited, and as the divalent aliphatic group, for example, a divalent non-cyclic aliphatic group or a divalent cyclic aliphatic group can be cited. Among them, from the viewpoint of improving the puncture strength and dielectric properties of the laminated film, a divalent cyclic aliphatic group and a divalent aromatic group are preferred, and a divalent aromatic group is more preferred. For the divalent organic group, the hydrogen atom in the organic group can be substituted by a halogen atom, a hydrocarbon group, an alkoxy group or a halogenated hydrocarbon group, in which case, the carbon number of these groups is preferably 1 to 8. It should be noted that in this specification, a divalent aromatic group is a divalent organic group having an aromatic group, and may contain an aliphatic group or other substituents in a part of its structure. In addition, a divalent aliphatic group is a divalent organic group having an aliphatic group, and may contain other substituents in a part of its structure, but does not contain an aromatic group.
[0281] In one embodiment of the present invention, the PI-based resin may contain a plurality of Xs, and the plurality of Xs may be the same or different from each other. Examples of X in formula (2) include: groups (structures) represented by formulas (60) to (65); groups in which hydrogen atoms in the groups represented by formulas (60) to (65) are replaced by methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, fluoro, chloro or trifluoromethyl groups; and the like.
[0282]
[0283] [In formula (60) and formula (61), R a and R b Each of them independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, and R a and R b The hydrogen atoms contained in may be replaced by halogen atoms independently of one another,
[0284] W independently represents a single bond, -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )-or-CONH-, R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom,
[0285] t' represents an integer from 0 to 4, u represents an integer from 0 to 4, and n represents an integer from 0 to 4.
[0286] In formula (62), ring A represents a cycloalkane ring having 3 to 8 carbon atoms,
[0287] R d represents an alkyl group having 1 to 20 carbon atoms,
[0288] r represents an integer of 0 or more and (the number of carbon atoms in ring A - 2) or less,
[0289] S1 and S2 independently represent an integer from 0 to 20,
[0290] In formulas (60) to (65), * represents a connecting bond].
[0291] Other examples of X in formula (2) include divalent acyclic aliphatic groups such as ethylene, 1,3-propylene, 1,4-butylene (tramethylene group), 1,5-pentylene, 1,6-hexylene, 1,2-propylene, 1,2-butanediyl, 1,3-butanediyl, 1,12-dodecanediyl, 2-methyl-1,2-propanediyl, and 2-methyl-1,3-propanediyl. Hydrogen atoms in the divalent acyclic aliphatic group may be substituted with halogen atoms, and carbon atoms may be substituted with heteroatoms such as oxygen atoms and nitrogen atoms.
[0292] Among them, from the viewpoint of improving the puncture strength and dielectric properties of the laminated film, the PI-based resin in the present invention preferably includes structures represented by formula (60) and formula (61) as X in formula (2), and more preferably includes a structure represented by formula (60).
[0293] In formula (60) and formula (61), the connecting bond of each benzene ring or each cyclohexane ring can be bonded to any position in the ortho position, meta position or para position, or α position, β position or γ position based on -W- or the single bond connecting each benzene ring or each cyclohexane ring. From the viewpoint of improving the puncture strength and dielectric properties of the laminated film, it can be preferably bonded to the meta position or para position, or β position or γ position, and can be more preferably bonded to the para position or γ position. If the amino group directly connected to the benzene ring is in the meta position with the divalent connecting group -W-, there is a tendency that the flexibility of the polyimide molecular chain is improved.
[0294] In formula (60) and formula (61), R a and R b Each of them is preferably a halogen atom, or an alkyl group, alkoxy group or aryl group which may have a halogen atom, and more preferably a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, and the aryl group having 6 to 12 carbon atoms include the groups exemplified above. a and R b The hydrogen atoms contained in R may be independently substituted by a halogen atom, and examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom and an iodine atom. a and R b Independently of each other, an alkyl group having 1 to 6 carbon atoms or a fluorinated alkyl group having 1 to 6 carbon atoms is preferred. From the viewpoint of adhesion to a metal layer, etc., an alkyl group having 1 to 6 carbon atoms not containing fluorine is more preferred, an alkyl group having 1 to 3 carbon atoms not containing fluorine is further preferred, and a methyl group is particularly preferred.
[0295] In formula (60) and formula (61), t′ and u are each independently preferably an integer of 0 to 2, and more preferably 0 or 1.
[0296] In formula (60) and formula (61), W is preferably independently a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2-, -S-, -COO-, -OOC- or -CO-, more preferably a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC- or -CO-, further preferably a single bond, -O-, -CH2- or -C(CH3)2-, particularly preferably -O- or -C(CH3)2-.
[0297] In formula (60) and formula (61), n is preferably an integer of 0 to 3, and more preferably 1 to 3. When n is 2 or more, a plurality of W, R a , and t' may be the same or different from each other, and the positions of the bonds connecting the benzene rings based on -W- may be the same or different.
[0298] When the PI-based resin in the present invention contains two or more structures represented by any one of the formulas (60) and (61) as X in the formula (2), W, n, and R in one of the formulas (60) and (61) are a , R b , t' and u can be independently combined with W, n, R in another formula (60) and formula (61) a , R b , t' and u are the same or different.
[0299] In formula (62), examples of the cycloalkane ring having 3 to 8 carbon atoms represented by ring A include cyclopropane ring, cyclobutane ring, cyclopentane ring, cyclohexane ring, cycloheptane ring, and cyclooctane ring, and preferably cycloalkane ring having 4 to 6 carbon atoms. In ring A, each connecting bond may be adjacent to each other or may not be adjacent to each other. For example, when ring A is a cyclohexane ring, the two connecting bonds may be at the α position, β position, or γ position, and may preferably be at the β position or γ position.
[0300] R in formula (62) d It is preferably an alkyl group having 1 to 10 carbon atoms. r in formula (62) is preferably 0 or more and preferably 4 or less. S1 and S2 in formula (62) are each independently preferably 0 or more, more preferably 2 or more and preferably 15 or less.
[0301] Specific examples of the structures represented by formula (60) to formula (62) include structures represented by formula (71) to formula (92). In these formulas, * represents a connecting bond.
[0302]
[0303] In one embodiment of the present invention, when the PI resin constituting the layer containing the PI resin contains at least one structural unit of a diamine represented by formula (60) and formula (61) as X in formula (2), relative to the total amount of structural unit (B), the proportion of the structural unit of the diamine represented by formula (60) and formula (61) in formula (2) is preferably 30 mol% or more, more preferably 50 mol% or more or more than 50 mol%, further preferably 70 mol% or more, particularly preferably 90 mol% or more, preferably 100 mol% or less. If the proportion of the structural unit of the diamine represented by formula (60) and formula (61) in formula (2) is within the above range, it is easy to control the parameter X in the laminated film and the thickness of the intermediate region within the desired range, and the puncture strength and dielectric properties of the laminated film can be improved. In addition, there is a tendency for the CTE of the laminated film to decrease, and the dimensional stability of the laminated film can be expected to be improved.
[0304] (Structural unit (B1))
[0305] In one embodiment of the present invention, it is preferred that at least one of layers (PI-1) and (PI-2), or at least one of layers (PI-1) to (PI-3) contains a PI-based resin having a structural unit (B) derived from a diamine, wherein the structural unit (B) contains a structural unit (B1) derived from a diamine represented by formula (B1) (hereinafter, sometimes simply referred to as structural unit (B1)).
[0306]
[0307] [In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0308] W independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the aforementioned divalent linking group), R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom,
[0309] m represents an integer from 1 to 4,
[0310] q independently represents an integer from 0 to 4]
[0311] If the PI-based resin contains structural unit (B1) as structural unit (B), it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which can improve the puncture strength and dielectric properties. In addition, the CTE can be reduced, and the dimensional stability of the laminated film can be expected to be improved, and it can also contribute to the improvement of the adhesion to the metal layer. In addition, even at a relatively low temperature (e.g., below 360°C) of the imidization temperature, the puncture strength and dielectric properties of the obtained laminated film can be improved. Therefore, even if the PI-based resin precursor coating is thermally imidized to manufacture a laminated sheet with a laminated structure with a metal layer (e.g., a metal foil layer such as copper foil), the degradation of the metal layer surface can be suppressed, and a laminated sheet having high puncture strength and excellent high-frequency characteristics can be obtained.
[0312] As R in formula (B1) b1 , which is the same as R in the formula (60) described above. a and R b The q in formula (B1) is preferably an integer of 0 to 2 independently of each other, and more preferably 0 or 1. In addition, from the viewpoint of improving the puncture strength, dielectric properties, CTE, etc. of the laminated film, m in formula (B1) is preferably an integer of 1 to 3, and more preferably 2 or 3. In formula (b2), a plurality of W, R b2 , and q may be the same or different, and the position of -W- based on -NH2 of each benzene ring may be the same or different.
[0313] In formula (B1), -W- can be independently bonded to the ortho position, meta position or para position, or any position in the α position, β position or γ position based on the -NH2 of each benzene ring, preferably bonded to the meta position or para position, or β position or γ position, and more preferably bonded to the para position or γ position. When m is 2 or more, on the benzene ring to which 2 W are bonded, the bonding positions of 2 W can be the ortho position, meta position or para position, or the α position, β position or γ position, preferably the meta position or para position, or the β position or γ position.
[0314] Specific examples of the structure represented by formula (B1) include structures represented by formula (B1-1) to formula (B1-6).
[0315]
[0316] R in formula (B1-1) to formula (B1-6) b1 and q and R in formula (B1) b1 and q are defined in the same way, W 1 ~W 6Each independently represents a group consisting of -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )- and -CONH-, a divalent linking group, R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted by a halogen atom. In addition, the compound of formula (B1-4) which repeats the formula (B1-3) is regarded as the compound of formula (B1-3).
[0317] As R in Formula (B1-1) to Formula (B1-6) b1 and q, which can be exemplified as R in formula (B1): b1 The embodiments are the same as those exemplified by q, and the preferred embodiments are also the same.
[0318] W in formula (B1-1) to formula (B1-6) 1 ~W 6 Preferably, each independently of the other is -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO2-, -S-, -CO- or -CONH-. W in formula (B1-1) 1 Preferably, it is -O-, -CH2-, -C(CH3)2-, -SO2-, -S- or -CO-. W in formula (B1-2), formula (B1-4) and formula (B1-6) 2 , W 4 and W 6 Each is preferably -O-. W in formula (B1-3) 3 Preferably, W in formula (B1-5) is -O-, -CH2-, -C(CH3)2-, -SO2-, -CO- or -CONH-. 5 Preferred is -C(CH3)2-, -O-, -SO2- or -CO-.
[0319] In one embodiment of the present invention, the PI-based resin constituting at least one of the layers (PI-1) and (PI-2) in the laminated film of the present invention, or at least one of the layers (PI-1) to (PI-3), preferably contains a structural unit from a diamine in which m in formula (B1) is 1 or 2, such as the aforementioned structural unit (B1-1) and / or structural unit (B1-2) as structural unit (B). As a structural unit from a diamine in which m is 2, for example, the aforementioned structural unit (B1-2) is preferably included. If such a structural unit is included, it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, and the puncture strength and dielectric properties can be improved. In addition, there is a tendency for the CTE of the laminated film to decrease, and the dimensional stability of the laminated film can be expected to be improved. In addition, the inclusion of these structural units will also help to improve the adhesion between the laminated film and the metal layer.
[0320] In another embodiment of the present invention, in the PI-based resin constituting at least one of the layers (PI-1) and (PI-2) in the laminated film of the present invention, or at least one of the layers (PI-1) to (PI-3), as a structural unit (B), preferably comprises a structural unit derived from a diamine in which m is 3 or 4, such as the aforementioned structural unit (B1-3) to structural unit (B1-6), and more preferably comprises a structural unit derived from a diamine in which m is 3. As a structural unit derived from a diamine in which m is 3, for example, the aforementioned structural unit (B1-5) is preferably included. If such a structural unit is included, it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, and the puncture strength and dielectric properties can be improved. In addition, there is a tendency for the CTE of the laminated film to decrease, and the dimensional stability of the laminated film can be expected to be improved. In addition, the inclusion of these structural units will also help to improve the adhesion between the laminated film and the metal layer.
[0321] In one embodiment of the present invention, the structural unit (B1) is preferably the structural unit (B1-2), and the structural unit (B1-2) is more preferably a structural unit represented by the formula (B1-2') and / or the formula (B1-2").
[0322]
[0323] R in formula (B1-2') and formula (B1-2") b1 , W 2 , and q and R in formula (B1-2) b1 , W 2 , and q are defined similarly.
[0324] In one embodiment of the present invention, the structural unit represented by formula (B1-2') or formula (B1-2") is preferably a structural unit represented by formula (B1-2'a) or formula (B1-2"a), respectively.
[0325]
[0326] If the above structural unit is included as structural unit (B), it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, and the puncture strength and dielectric properties can be improved. In addition, there is a tendency for the CTE of the laminated film to decrease, and it is expected that the dimensional stability of the laminated film will be improved. In addition, the inclusion of these structural units will also help to improve the adhesion between the laminated film and the metal layer.
[0327] In another embodiment of the present invention, the structural unit (B1) is preferably the structural unit (B1-5), and the structural unit (B1-5) is more preferably a structural unit represented by the formula (B1-5a).
[0328]
[0329] When the structural unit described above is included as the structural unit (B), it is easy to control the parameter X in the laminate film and the thickness of the intermediate region within the desired range, which is advantageous in improving the puncture strength and dielectric properties of the laminate film and reducing CTE.
[0330] In one embodiment of the present invention, when the PI resin constituting the layer containing the PI resin contains the structural unit (B1), the content thereof is preferably 3 mol% or more, more preferably 5 mol% or more, further preferably 7 mol% or more, further more preferably 10 mol% or more, for example, it may be 20 mol% or more, 30 mol% or more, or 40 mol% or more. If the content of the structural unit (B1) is above the above lower limit, it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which is beneficial to the puncture strength of the laminated film, the improvement of dielectric properties, the reduction of CTE, etc. In addition, if the total amount of the structural unit (B1) increases, there is a tendency for the adhesion to the metal layer to increase. Therefore, from such a viewpoint, the content of the structural unit (B1) may be, for example, 50 mol% or more, 60 mol% or more, or 70 mol% or more relative to the total amount of the structural unit (B). The content of the structural unit (B1) is preferably 99 mol% or less, more preferably 95 mol% or less, and even more preferably 90 mol% or less, based on the total amount of the structural unit (B).
[0331] <Structural unit (B2)>
[0332] In one embodiment of the present invention, the PI-based resin constituting at least one of the layers (PI-1) and (PI-2), or at least one of the layers (PI-1) to (PI-3) in the laminated film of the present invention preferably contains a structural unit (B2) (hereinafter sometimes abbreviated as structural unit (B2)) derived from a diamine containing a biphenyl skeleton represented by formula (B2) as a structural unit (B).
[0333]
[0334] [In formula (B2), R b2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom,
[0335] p represents an integer from 0 to 4]
[0336] If the structural unit (B) contains the aforementioned structural unit (B2), the PI-based resin is not excessively rigid but has a soft structure having a certain degree of freedom. Therefore, it is easy to form a branched structure by heating during imidization. In addition, there is a tendency for the crystallinity to increase. Therefore, it is easy to control the parameter X in the laminated film and the thickness of the intermediate region within the desired range, which is beneficial to the improvement of the puncture strength and dielectric properties of the laminated film, the reduction of CTE, etc.
[0337] In formula (B2), R b2 Preferably, they are independently a halogen atom, or an alkyl group, an alkoxy group, or an aryl group which may have a halogen atom, and more preferably a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, and the aryl group having 6 to 12 carbon atoms include the groups exemplified above. b2 The hydrogen atoms contained in R may be independently substituted by halogen atoms, and examples of the halogen atoms include the same halogen atoms as those mentioned above. b2 Independently of each other, an alkyl group having 1 to 6 carbon atoms or a fluorinated alkyl group having 1 to 6 carbon atoms is preferred. Furthermore, from the viewpoint of adhesion to a metal layer, etc., an alkyl group having 1 to 6 carbon atoms not containing fluorine is more preferred, an alkyl group having 1 to 3 carbon atoms not containing fluorine is further preferred, and a methyl group is particularly preferred.
[0338] In formula (B2), p is preferably an integer of 0 to 2, and more preferably 0 or 1, each independently of the other.
[0339] In formula (B2), the -NH2 group bonded to each benzene ring can be bonded to any position of the ortho, meta or para position, or the α, β or γ position based on the single bond connecting each benzene ring. From the viewpoint of the dielectric properties of the laminated film, the improvement of the puncture strength and the reduction of the CTE, it can be preferably bonded to the meta or para position, or the β or γ position, and it can be more preferably bonded to the para or γ position.
[0340] In a preferred embodiment of the present invention, formula (B2) is preferably represented by formula (B2').
[0341]
[0342] If the PI resin constituting at least one layer containing a PI resin contains a PI resin having a structural unit (B2), especially a structural unit derived from a diamine represented by formula (B2') as a structural unit (B), the PI resin is not too rigid but has a soft structure with a certain degree of freedom, so it is easy to form a branched structure by heating during imidization. In addition, there is a tendency for the crystallinity to increase, so it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which is beneficial to the puncture strength, dielectric properties, CTE reduction, etc. of the laminated film. In addition, the above-mentioned effects can be obtained even at a relatively low temperature (e.g., below 360°C) of the imidization temperature, so even if a laminated sheet is manufactured by thermally imidizing the PI resin precursor coating film in a laminated structure with a metal layer (e.g., a metal foil layer such as copper foil), it is possible to suppress the deterioration of the metal layer surface, and obtain a laminated sheet having high puncture strength and excellent high-frequency properties.
[0343] In one embodiment of the present invention, when the PI resin contains structural units (B2), the content thereof is preferably 1 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more, for example, 20 mol% or more, 30 mol% or more, greater than 30 mol%, 40 mol% or more, or 50 mol% or more. If the content of structural unit (B2) is above the above lower limit, it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, which is beneficial to the puncture strength of the laminated film, the improvement of dielectric properties, the reduction of CTE, etc. In addition, relative to the total amount of structural unit (B), structural unit (B1) is preferably 99 mol% or less, more preferably 95 mol% or less, and further preferably 92 mol% or less, for example, 90 mol% or less, 80 mol% or less, 70 mol% or less, or 60 mol% or less.
[0344] In one embodiment of the present invention, when the PI-based resin constituting the layer containing the PI-based resin includes the structural unit (B1) and the structural unit (B2), the total content thereof is preferably 30 mol% or more, more preferably 40 mol% or more, further preferably 60 mol% or more, particularly preferably 70 mol% or more, particularly more preferably 80 mol% or more, further particularly preferably 90 mol% or more, further more particularly preferably 95 mol% or more, and preferably 100 mol% or less. If the total content of the structural unit (B1) and the structural unit (B2) is above the aforementioned lower limit, the above-mentioned effect of the present invention that can be expected due to the PI-based resin having the structural unit (B1) and the structural unit (B2) can be easily obtained, and the effect can be further improved.
[0345] In one embodiment of the present invention, when the PI-based resin contains the structural unit (B1) and the structural unit (B2), the content ratio (molar ratio, (B1): (B2)) is preferably 99:1 to 1:99, more preferably 95:5 to 5:95, and further preferably 92:8 to 8:92, for example, 92:8 to 20:80, or 90:10 to 60:40. If the content ratio of the structural unit (B1) to the structural unit (B2) is within the above range, the above-mentioned effect of the present invention that can be expected due to the PI-based resin having the structural unit (B1) and the structural unit (B2) can be easily obtained, and the effect can be further improved.
[0346] In one embodiment of the present invention, the PI-based resin-containing layer constituting the laminated film preferably includes any one or more of the following structures.
[0347] In the layer (PI-1) and the layer (PI-2), or the layers (PI-1) to (PI-3) in the laminated film, the PI-based resin contains at least one of the structural unit (B1) and the structural unit (B2);
[0348] In the layer (PI-1) and the layer (PI-2), or the layer (PI-1) to the layer (PI-3) in the laminated film, the PI-based resin contains the structural unit (B1);
[0349] In the layer (PI-1) and the layer (PI-2), or the layer (PI-1) to the layer (PI-3) in the laminated film, the PI-based resin contains the structural unit (B1) and the structural unit (B2).
[0350] In at least one layer containing a PI-based resin in the laminated film, the PI-based resin contains a structural unit (B1) and a structural unit (B2);
[0351] (Structural unit (B3))
[0352] In one embodiment of the present invention, the structural unit (B) may include a structural unit (B3) derived from a diamine other than the structural unit (B1) and the structural unit (B2) (hereinafter, sometimes simply referred to as the structural unit (B3)). Examples of the structural unit (B3) include a structural unit derived from a diamine in which m in the formula (B1) is 0, a structural unit derived from a diamine in which X in the formula (2) is represented by the formula (61) to the formula (64), and the like. Among them, a structural unit derived from a diamine in which X in the formula (2) is represented by the formula (74) (a structural unit derived from p-phenylenediamine) is preferred. In the present specification, the so-called "structural unit (B3) derived from a diamine other than the structural unit (B1) and the structural unit (B2)" refers to a structural unit derived from a diamine that is different from either the structural unit (B1) or the structural unit (B2).
[0353] In one embodiment of the present invention, when the structural unit (B) contains the structural unit (B3), the content of the structural unit (B3) is preferably 25 mol% or less, more preferably 20 mol% or less, further preferably 10 mol% or less, and usually 0.01 mol% or more, relative to the total amount of the structural unit (B).
[0354] In one embodiment of the present invention, the polyimide resin contained in the layer (PI-1) containing the PI resin and the PI resin contained in the layer (PI-2) containing the PI resin may be the same resin or different resins. From the viewpoints of the puncture strength of the laminated film, the improvement of dielectric properties, the reduction of CTE, etc., the PI resin contained in each layer is preferably a different resin. It should be noted that the meaning of the different resins includes not only resins with different types of structural units, but also resins with different contents (or ratios) even if the types of the structural units are the same.
[0355] In one embodiment of the present invention, the PI-containing resin layer (PI-1) and the PI-containing resin layer (PI-2) each preferably contain a polyimide resin having at least two structural units (A) derived from tetracarboxylic anhydride. In such an embodiment, it is easy to improve the puncture strength and dielectric properties of the laminated film, and it is easy to reduce CTE.
[0356] In one embodiment of the present invention, preferably, in the layer (PI-1) containing a PI-based resin and the layer (PI-2) containing a PI-based resin, or the layers (PI-1) to (PI-3) containing a PI-based resin, preferably the mPI layer and the TPI layer, the PI-based resin contains a structural unit (A1) and / or a structural unit (A2) as the structural unit (A), and a structural unit (B1) as the structural unit (B) (preferably the structural unit (B1) and the structural unit (B2)).
[0357] In a preferred embodiment of the present invention, the PI-based resin contained in the layer (PI-1) containing a PI-based resin constituting the laminated film, preferably the mPI layer, contains at least two structural units selected from the group consisting of structural unit (A1), structural unit (A2) and structural unit (A3) (preferably structural unit (A1) and structural unit (A2) and / or structural unit (A3)) as structural unit (A), the PI-based resin contained in the layer (PI-2) containing a PI-based resin, preferably the TPI layer, contains structural unit (A1) and structural unit (A2) as structural unit (A), and the PI-based resins constituting the layer (PI-1) containing a PI-based resin and the layer (PI-2) containing a PI-based resin, preferably the mPI layer and the TPI layer, each contain a structural unit (B1) (preferably structural unit (B1) and structural unit (B2)) as structural unit (B).
[0358] In a preferred embodiment of the present invention, when a layer (PI-3) containing a PI-based resin is also included, the PI-based resin contained in the layer (PI-1) containing a PI-based resin, preferably the mPI layer, constituting the laminated film (L) contains at least two structural units selected from the group consisting of the structural unit (A1), the structural unit (A2) and the structural unit (A3) (preferably the structural unit (A1) and the structural unit (A2) and / or the structural unit (A3)) as the structural unit (A), the PI-based resin contained in the layer (PI-2) containing a PI-based resin and the layer (PI-3) containing a PI-based resin, preferably the TPI layer, contains the structural unit (A1) and the structural unit (A2) as the structural unit (A), and the PI-based resins constituting the layers (PI-1) to (PI-3) containing a PI-based resin, preferably the mPI layer and the TPI layer, each contain the structural unit (B1) (preferably the structural unit (B1) and the structural unit (B2)) as the structural unit (B).
[0359] If the mPI layer, TPI layer, layer (PI-1), layer (PI-2) and any layer (PI-3) are each combined to contain the above-mentioned structural units, the PI-based resin of each layer is not too rigid and will become a soft structure with a certain degree of freedom. Therefore, it is easy to form a branched structure by heating during imidization, and there is a tendency to improve crystallinity. In addition, the interaction between two adjacent layers can be improved. Therefore, it is easy to control the parameter X and the thickness of the middle region in the laminated film composed of these layers within the desired range, and it is easy to obtain the above-mentioned effects of the present invention that can be expected due to the PI-based resin having each structural unit, and in addition, the effect can be further improved.
[0360] <Layer (PI-1)>
[0361] In one embodiment of the present invention, the PI-based resin constituting the layer (PI-1) contains, as the structural unit (A), a structural unit (A1) and / or a structural unit (A2), preferably contains at least two structural units selected from the structural unit (A1), the structural unit (A2) and the structural unit (A3), and more preferably contains the structural unit (A1) and the structural unit (A2) and / or the structural unit (A3). When the layer (PI-1) contains these structural units, the content of the structural unit (A1) is preferably 20 mol% or more, more preferably 30 mol% or more, further preferably 35 mol% or more, particularly preferably 40 mol% or more, preferably 80 mol% or less, more preferably 75 mol% or less, further preferably 70 mol% or less, and particularly preferably 65 mol% or less. The content of the structural unit (A2) is preferably 20 mol% or more, more preferably 30 mol% or more, further preferably 35 mol% or more, particularly preferably 40 mol% or more, preferably 80 mol% or less, more preferably 75 mol% or less, further preferably 70 mol% or less, and particularly preferably 65 mol% or less, relative to the total amount of the structural unit (A). In addition, the content of the structural unit (A3) is preferably 3 mol% or more, more preferably 5 mol% or more, further preferably 7 mol% or more, further more preferably 10 mol% or more, for example, 20 mol% or more, 30 mol% or more, or 40 mol% or more, preferably 75 mol% or less, more preferably 70 mol% or less, further preferably 65 mol% or less, and particularly preferably 60 mol% or less, relative to the total amount of the structural unit (A). In addition, in another embodiment, the content of the structural unit (A3) is preferably 45 mol% or less, more preferably 35 mol% or less, further preferably 25 mol% or less, further more preferably 15 mol% or less, particularly preferably 5 mol% or less, particularly more preferably 1 mol% or less, and the lower limit may be 0 mol%.
[0362] If the contents of the structural unit (A1), the structural unit (A2) and / or the structural unit (A3) are each within the above range, the PI-based resin is not too rigid but has a soft structure with a certain degree of freedom, so that it is easy to form a branched structure by heating during imidization, and there is a tendency to increase crystallinity. As a result, it is easy to control the parameter X in the laminated film and the thickness of the middle region within the desired range, and a laminated film with excellent puncture strength, dielectric properties, and thermal properties can be obtained.
[0363] On the other hand, in another embodiment of the present invention, the content of the structural unit (A2) in the PI-based resin constituting the layer (PI-1) is preferably less than 30 mol%, more preferably 25 mol% or less, further preferably 20 mol% or less, and particularly preferably 10 mol% or less, relative to the total amount of the structural unit (A). In one embodiment of the present invention, the layer (PI-1) may be substantially free of the structural unit (A2), and the lower limit of the content of the structural unit (A2) may be 0 mol%.
[0364] In one embodiment of the present invention, the PI-based resin constituting the layer (PI-1) preferably contains the structural unit (B1) as the structural unit (B). As the structural unit (B1), it is preferred to contain the structural unit (B1-2) and the structural unit (B1-5), more preferably contain the structural unit (B1-2), and further preferably contain the structural unit (B1-2"). Regarding the content of the structural unit (B1) in the PI-based resin constituting the layer (PI-1), relative to the total amount of the structural unit (B), it is preferably 3 mol% or more, more preferably 5 mol% or more, further preferably 7 mol% or more, and further preferably 10 mol% or more. For example, it may be 20 mol% or more, 30 mol% or more, or 40 mol% or more. In addition, it is preferably 80 mol% or less, more preferably 75 mol% or less, and further preferably 10 mol% or more. It is 70 mol% or less, and it is particularly preferably 65 mol% or less. In addition, the PI-based resin constituting the layer (PI-1) preferably further comprises a structural unit (B2) as the structural unit (B), and its content relative to the total amount of the structural unit (B) is preferably 10 mol% or more, more preferably 20 mol% or more, further preferably 30 mol% or more or more than 30 mol%, further more preferably 35 mol% or more, particularly preferably 40 mol% or more, preferably 99 mol% or less, more preferably 95 mol% or less, further preferably 92 mol% or less, for example, it may be 90 mol% or less, 80 mol% or less, 70 mol% or less, or 60 mol% or less.
[0365] If the content of the structural unit (B1) and / or the structural unit (B2) is within the above range, the PI-based resin is not too rigid but has a soft structure with a certain degree of freedom, so it is easy to form a branched structure by heating during imidization, and there is a tendency to increase crystallinity. As a result, the puncture strength of the layer (PI-1) can be improved, the Df can be reduced, and the CTE can be effectively reduced, so that a laminated film with excellent puncture strength, dielectric properties, and thermal properties can be obtained.
[0366] <Layer (PI-2) and Layer (PI-3)>
[0367] In one embodiment of the present invention, the laminated film includes layer (PI-2) and may further include layer (PI-3). The PI-based resins constituting layer (PI-2) and layer (PI-3) each include structural unit (A1) as structural unit (A), preferably including structural unit (A1) and structural unit (A2) as structural unit (A). In the case of including these structural units, relative to the total amount of structural unit (A), the content of structural unit (A1) is preferably 10 mol% or more, more preferably 15 mol% or more, more preferably 20 mol% or more, preferably 80 mol% or less, more preferably 70 mol% or less, more preferably 60 mol% or less. In addition, relative to the total amount of structural unit (A), the content of structural unit (A2) is preferably 20 mol% or more, more preferably 30 mol% or more, more preferably 40 mol% or more, more preferably 50 mol% or more, particularly preferably 60 mol% or more, preferably 90 mol% or less, more preferably 85 mol% or less, more preferably 80 mol% or less, more preferably 75 mol% or less.
[0368] If the content of structural unit (A1) and / or structural unit (A2) is each within the above range, PI-based resin is not too rigid and will become a soft structure with a certain degree of freedom, therefore, it is easy to form a branched structure by heating during imidization, and in addition, there is a tendency to improve crystallinity. Thus, it is possible to achieve an increase in the puncture strength of layer (PI-2) and layer (PI-3), a decrease in Df, and then it is also possible to effectively reduce CTE, therefore, it is possible to obtain a laminated film with excellent puncture strength, dielectric properties, and thermal properties. In addition, it is expected that the effect of improving the adhesion to the metal layer can be expected.
[0369] In one embodiment of the present invention, the content of the structural unit (A3) in the PI-based resin constituting the layer (PI-2) and the layer (PI-3) is preferably 10 mol% or less, more preferably 8 mol% or less, further preferably 5 mol% or less, and particularly preferably 3 mol% or less, relative to the total amount of the structural unit (A). In one embodiment of the present invention, the layer (PI-2) and the layer (PI-3) may be substantially free of the structural unit (A3), and the lower limit of the content of the structural unit (A3) may be 0 mol%.
[0370] In one embodiment of the present invention, the PI-based resin constituting the layer (PI-2) and the layer (PI-3) preferably contains the structural unit (B1) as the structural unit (B). As the structural unit (B1), it is preferably contained the structural unit (B1-2), and more preferably contains the structural unit (B1-2') that improves the flexibility of the PI-based resin. Regarding the content of the structural unit (B1) in the PI-based resin constituting these layers, relative to the total amount of the structural unit (B), it is preferably 20 mol% or more, more preferably 30 mol% or more, further preferably 35 mol% or more, particularly preferably 40 mol% or more, preferably 99 mol% or less, more preferably 95 mol% or less, further preferably 92 mol% or less, for example, it may also be 90 mol% or less, 80 mol% or less, 70 mol% or less, or 60 mol% or less. In addition, as the structural unit (B), it is preferred to also contain the structural unit (B2), and its content is preferably 1 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more. For example, it can also be 20 mol% or more, 30 mol% or more, greater than 30 mol%, or 40 mol% or more. In addition, it is preferably 80 mol% or less, more preferably 70 mol% or less, further preferably 65 mol% or less, and particularly preferably 60 mol% or less.
[0371] In the PI resin of the constituent layer (PI-2) and the layer (PI-3), if the content of the structural unit (B1) and / or the structural unit (B2) is each within the above range, the PI resin is not too rigid and will become a soft structure with a certain degree of freedom, therefore, it is easy to form a branched structure by heating during imidization, and in addition, there is a tendency to improve crystallinity. Thus, the improvement of the puncture strength of the layer (PI-2) and the layer (PI-3) and the reduction of Df can be achieved, and CTE can also be effectively reduced, therefore, it is possible to obtain a laminated film with more excellent puncture strength, dielectric properties, and thermal properties. In addition, it is expected to improve the adhesion to the metal layer.
[0372] The various physical properties (molecular weight, glass transition temperature, etc.) of the PI-based resin composed of the above-mentioned structural unit (A) and / or structural unit (B) can be appropriately determined based on, for example, the following preferred ranges, depending on the role and purpose of each PI-based resin-containing layer in the laminated film.
[0373] In one embodiment of the present invention, the PI resin constituting each PI resin-containing layer may contain, for example, a halogen atom, preferably a fluorine atom, which can be introduced using the above-mentioned halogen atom-containing substituent. When the PI resin contains fluorine atoms, it is easy to reduce the relative dielectric constant of the obtained PI resin-containing layer, resulting in an improvement in the dielectric properties of the laminated film. As a fluorine-containing substituent preferably used to make the PI resin contain fluorine atoms, for example, a fluorine group and a trifluoromethyl group can be cited.
[0374] In addition, in another embodiment of the present invention, from the viewpoint of improving the adhesion between the obtained PI-containing resin layer and the metal layer, the PI-containing resin preferably does not contain fluorine atoms. Therefore, for example, it is preferred that the PI-containing resin layer in contact with the metal layer, preferably the TPI layer, especially the layer (PI-2) and the layer (PI-3) in the laminated film do not contain fluorine atoms. In addition, if the PI-containing resin contains fluorine, there is a tendency to weaken the interaction between the molecular chains, and therefore, when the PI-containing resin does not contain fluorine atoms, there is a tendency to reduce the Df of the PI film.
[0375] When the PI resin contains halogen atoms, the content of halogen atoms, especially fluorine atoms, in the PI resin is preferably 0.1 to 35% by mass, more preferably 0.1 to 30% by mass, further preferably 0.1 to 20% by mass, and particularly preferably 0.1 to 10% by mass, based on the mass of the PI resin. If the content of halogen atoms is above the above lower limit, it is easy to improve the heat resistance and dielectric properties of the obtained layer containing the PI resin, resulting in an improvement in the dielectric properties and thermal properties of the laminated film. If the content of halogen atoms is below the above upper limit, it is advantageous in terms of cost, it is easy to reduce CTE, and it is easy to synthesize the PI resin.
[0376] In one embodiment of the present invention, the imidization rate of the PI resin is preferably 90% or more, more preferably 93% or more, further preferably 95% or more, and usually 100% or less. From the viewpoint of improving the puncture strength, dielectric properties, and thermal properties of the laminated film, the imidization rate is preferably above the above-mentioned lower limit. The imidization rate represents the ratio of the molar amount of the imide bond in the PI resin to the value of 2 times the molar amount of the structural unit from the tetracarboxylic acid compound in the PI resin. It should be noted that, when the PI resin contains a tricarboxylic acid compound, the imidization rate represents the ratio of the molar amount of the imide bond in the PI resin to the value of 2 times the molar amount of the structural unit from the tetracarboxylic acid compound in the PI resin to the total molar amount of the structural unit from the tricarboxylic acid compound. In addition, the imidization rate can be obtained using IR method, NMR method, etc.
[0377] In one embodiment of the present invention, from the viewpoint of improving the puncture strength, the weight average molecular weight (Mw) of the PI-based resin in terms of polystyrene is preferably 5,000 or more, more preferably 10,000 or more, further preferably 15,000 or more, and particularly preferably 20,000 or more. In addition, from the viewpoint of the ease of manufacture and film-forming properties of the varnish, it is preferably 1,200,000 or less, more preferably 1,000,000 or less, further preferably 800,000 or less, and particularly preferably 700,000 or less. For example, the Mw of the PI-based resin constituting the mPI layer, especially the layer (PI-1) in the laminated film, is preferably 5,000 to 800,000, and more preferably 10,000 to 700,000. In addition, the Mw of the PI-based resin constituting the TPI layer, especially the layer (PI-2) and the layer (PI-3) in the laminated film, is preferably 10,000 to 1,000,000, and more preferably 20,000 to 900,000.
[0378] In one embodiment of the present invention, from the viewpoint of puncture strength and adhesion to the metal layer, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the PI-based resin of the present invention is preferably 1.1 or more, more preferably 1.3 or more, further preferably 1.5 or more, particularly preferably 1.7 or more, preferably 15 or less, more preferably 12 or less, further preferably 11 or less, and particularly preferably 10 or less. For example, the Mw / Mn of the mPI layer, especially the layer (PI-1) in the laminated film, is preferably 1.1 to 15, more preferably 1.5 to 10. In addition, the Mw / Mn of the TPI layer, especially the layer (PI-2) and the layer (PI-3) in the laminated film, is preferably 1.1 to 15, more preferably 1.5 to 10. It should be noted that, for Mw and Mn, gel permeation chromatography (hereinafter, sometimes described as GPC) can be performed to obtain them by converting them to standard polystyrene.
[0379] In one embodiment of the present invention, from the viewpoint of improving the puncture strength of the obtained laminated film and reducing Df, the Tg of the PI-based resin is preferably 350°C or less, more preferably 330°C or less, further preferably 310°C or less, and particularly preferably 300°C or less. In addition, from the viewpoint of improving the puncture strength of the laminated film, reducing Df, and improving thermal properties, the Tg of the PI-based resin is preferably 200°C or more, more preferably 205°C or more, further preferably 210°C or more, and particularly preferably 220°C or more. In the case of including an mPI layer and a TPI layer as the PI-based resin-containing layer, the Tg of the PI-based resin constituting the mPI layer is preferably 350°C or less, more preferably 330°C or less, further preferably 310°C or less, and particularly preferably 295°C or less, preferably 220°C or more, more preferably 230°C or more, further preferably 250°C or more, further more preferably 260°C or more, and particularly preferably 270°C or more. If the Tg of the PI-based resin constituting the mPI layer is within the above range, the puncture strength of the laminated film can be improved, and the dielectric properties and thermal properties can be improved. The Tg of the PI-based resin constituting the TPI layer is preferably 310°C or less, more preferably 300°C or less, further preferably 290°C or less, further preferably 270°C or less, particularly preferably 250°C or less, preferably 200°C or more, more preferably 210°C or more, further preferably 220°C or more, and particularly preferably 230°C or more. If the Tg of the PI-based resin constituting the TPI layer is within the above range, the puncture strength of the laminated film can be improved, and in addition to being able to reduce Df and improve thermal properties, the adhesion to the metal layer can also be improved. The Tg of the PI-based resin can be measured by dynamic viscoelasticity measurement. For example, it can be calculated based on the peak of the tanδ curve obtained using a dynamic viscoelasticity measuring device as the ratio of the storage modulus (Storage modulus, E') to the loss modulus (Loss modulus, E').
[0380] In an embodiment including an mPI layer and a TPI layer as a layer containing a PI-based resin, when the Tg of the PI-based resin constituting the mPI layer is within the above range, preferably 250 to 330°C, and the Tg of the PI-based resin constituting the TPI layer is within the above range, preferably 220 to 300°C, there is a tendency for each PI-based resin to easily form an ideal higher-order structure in which rotational motion is suppressed. Therefore, it is believed that in the case of this embodiment, each PI-based resin-containing layer can be formed using a PI-based resin having a higher-order structure in which orientation is maintained, and the strength of the PI-based resin-containing layer relative to the impact applied in the thickness direction is increased, and the puncture strength of the laminated film is improved. In addition, it is inferred that the rotation of the polar groups in each PI-based resin is suppressed and the loss of electrical energy in the form of thermal motion is reduced. Therefore, it is believed that by using a PI-based resin with a Tg in the above range, a laminated film with a low Df can be obtained. In addition, by using such a PI-based resin, the puncture strength and dielectric properties of the resulting laminated film can be improved even if the imidization temperature is a low temperature, for example, below 360°C. Therefore, even if a laminated sheet is manufactured by thermally imidizing a PI-based resin precursor coating film in a laminated structure with a metal layer (metal foil such as copper foil), degradation of the metal layer surface can be suppressed, and a laminated sheet (CCL) having high puncture strength and excellent high-frequency characteristics can be obtained.
[0381] The Tg of the PI-based resin can be adjusted by appropriately adjusting the types of structural units constituting the PI-based resin, their composition, the molecular weight of the PI-based resin, the production method, especially the imidization conditions, etc., for example, it can be adjusted to the above range by adjusting it to the range described as a preferred embodiment in this specification.
[0382] <Method for producing laminated film>
[0383] The laminated film of the present invention can be manufactured, for example, by a method comprising the following steps: a step of reacting tetracarboxylic anhydride and diamine appropriately selected according to the composition of the PI-containing resins of each PI-containing layer contained in the laminated film to obtain a PI-containing resin precursor; and a step of imidizing the obtained PI-containing resin precursor.
[0384] For example, as a method for manufacturing the laminated film of the present invention, the following method can be cited: a solution of a corresponding PI-based resin precursor is applied to a supporting substrate, pre-dried, thereby obtaining a multilayer coating film, and then imidized. Imidization can also be performed in a state where the supporting substrate has been peeled off. In one embodiment of the present invention, imidization is performed in a state where the solvent fully remains in the entire coating film or the resin layers are well fused, so that (P1 / P2) / (|P1-P2|) is easily adjusted to within the range of formula (I), (P1c / P1) is adjusted to within the range of formula (II), and in addition, the thickness of the intermediate region is easily adjusted to within the above-mentioned desired range. The reason is unclear, but it is believed to be the following reasons.
[0385] If the solvent is sufficiently left in the state of the whole coating or the state of good fusion between the resin layers, the degree of freedom of the resin molecules until imidization becomes high, therefore, there is a tendency that the plane orientation of the PI-based resin contained in each obtained layer containing PI-based resin is moderately reduced. Moreover, the layers containing PI-based resins of different thicknesses, preferably mPI layers and TPI layers, each produce differences in the degree of disorder of the plane orientation. Here, in the case where the disorder of the plane orientation is more likely to occur in layer (PI-2), the reduction value of P2 corresponding to layer (PI-2) will become larger than the reduction value of P1 corresponding to layer (PI-1), therefore, there is a tendency that the value of the molecule (P1 / P2) increases. On the other hand, since the plane orientation of both layers is reduced (the values of P1 and P2 are reduced), the difference between the numerical values of P1 and P2 also has a tendency to decrease. Therefore, it is believed that there is a tendency that (P1 / P2) / (|P1-P2|) in formula (I) increases. It is also believed that even in the case where the planar orientation disorder is more likely to occur in the layer (PI-1), as described above, since the planar orientation of both layers is reduced, the value of the denominator (|P1-P2|) decreases to a degree greater than the value of the numerator (P1 / P2), and there is a tendency for (P1 / P2) / (|P1-P2|) in formula (I) to increase.
[0386] In addition, it is believed that if it is in the above state, the orientation is easily disturbed until the center of the thick layer (PI-1), so there is a tendency for P1c / P1 to be greater than a predetermined value. It is further believed that if it is in the above state, the PI-based resins constituting each layer are easily mixed with each other near the interface of each layer, and an intermediate region is easily formed, so the thickness of the intermediate region becomes larger.
[0387] In a preferred embodiment of the present invention, the laminated film of the present invention can be manufactured, for example, by a method including the following steps: a step of coating a solution of a corresponding PI-based resin precursor on a supporting substrate and pre-drying to obtain a multilayer coating (also referred to as a coating and pre-drying step); a step of allowing the obtained multilayer coating to stand (also referred to as a standing step); and a step of heating the multilayer coating to imidize the PI-based resin (also referred to as an imidization step). It should be noted that the supporting substrate can be peeled off or removed. Since such a manufacturing method includes a standing step, preferably a standing step at a low temperature described later, it is easy to adjust the parameter X in the obtained laminated film and the thickness of the intermediate region to the desired range.
[0388] (Preparation of PI-based resin precursor)
[0389] As tetracarboxylic anhydride used in the synthesis of PI-based resin precursors, for example, aromatic tetracarboxylic acid compounds such as aromatic tetracarboxylic dianhydride and aliphatic tetracarboxylic acid compounds such as aliphatic tetracarboxylic dianhydride can be mentioned. The tetracarboxylic acid compound can be used alone or in combination of two or more. In addition to the dianhydride, the tetracarboxylic acid compound can also be a tetracarboxylic acid compound analog such as an acyl chloride compound.
[0390] Examples of the tetracarboxylic acid compound include tetracarboxylic anhydride represented by formula (A1), tetracarboxylic anhydride represented by formula (A2), and tetracarboxylic anhydride represented by formula (A3), and any tetracarboxylic acid compound known in the art can be appropriately selected and used.
[0391] Examples of such tetracarboxylic acid compounds include pyromellitic dianhydride (hereinafter, sometimes referred to as PMDA), 4,4'-(4,4'-isopropylidene diphenoxy) diphthalic anhydride (hereinafter, sometimes referred to as BPADA), 1,4,5,8-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter, sometimes referred to as BPDA), 4,4'-(hexafluoroisopropylidene) diphthalic dianhydride (hereinafter, sometimes referred to as 6FDA), 4,4'-oxydiphthalic dianhydride (hereinafter, sometimes referred to as ODPA), 2,2',3,3'-, 2,3,3',4'- or 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, Acid dianhydride, 2,2',3,3'-biphenyltetracarboxylic acid dianhydride, p-phenylenebis(trimellitic acid monoester acid dianhydride) (hereinafter, sometimes referred to as TAHQ), an ester of trimellitic acid anhydride and 2,2',3,3',5,5'-hexamethyl-4,4'-biphenol (hereinafter, sometimes referred to as TMPBP), 4,4'-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl (hereinafter, sometimes referred to as BP-TME), 2,3',3,4'-diphenyl ether tetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl) ether dianhydride, 3,3",4,4"-p-terphenyl tetracarboxylic acid dianhydride, 2,3,3",4"-p-terphenyl tetracarboxylic acid dianhydride, 2,2",3,3"-p-terphenyl Tetracarboxylic dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-, 1,2,6,7-phenanthrenetetracarboxylic dianhydride, 1,2,9,10-phenanthrenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride (hereinafter, sometimes referred to as HPMDA), 2,3,5,6-cyclohexanetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride (hereinafter, sometimes referred to as CBDA), norbornane-2-spiro-α'-spiro-2"-norbornane-5,5',6,6'-tetracarboxylic dianhydride, p-phenylenebis(trimellitic anhydride), 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7-dichloronaphthalene-1,4,5,8-Tetracarboxylic acid dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic acid dianhydride, 2,3,6,7-tetrachloronaphthalene-2,3,6,7-tetracarboxylic acid dianhydride, 1,4,5,8-tetrachloronaphthalene-1,4,5,8-tetracarboxylic acid dianhydride, 1,4,5,8-tetrachloronaphthalene-2,3,6,7-tetracarboxylic acid dianhydride, 2,3,8,9-perylenetetracarboxylic acid dianhydride, 3,4 ,9,10-perylenetetracarboxylic acid dianhydride, 4,5,10,11-perylenetetracarboxylic acid dianhydride, 5,6,11,12-perylenetetracarboxylic acid dianhydride, pyrazine-2,3,5,6-tetracarboxylic acid dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic acid dianhydride, thiophene-2,3,4,5-tetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, etc. Among them, from the viewpoint of improving the puncture strength of the obtained laminated film, reducing Df and CTE, it is preferred to use BPDA, PMDA, TAHQ and / or BP-TME in combination. These tetracarboxylic acid compounds can be used alone or in combination of two or more. ,
[0392] As the diamine compound used in the synthesis of the PI-based resin precursor, for example, aliphatic diamines, aromatic diamines and mixtures thereof can be cited. It should be noted that, in the present embodiment, the so-called "aromatic diamine" means a diamine having an aromatic ring, which may contain an aliphatic group or other substituents in a part of its structure. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring and a fluorene ring, but are not limited thereto. Among them, a benzene ring is preferably used. In addition, the so-called "aliphatic diamine" means a diamine having an aliphatic group, which may contain other substituents in a part of its structure, but does not have an aromatic ring.
[0393] Examples of the diamine compound include diamines represented by formula (B1), diamines represented by formula (B2), and diamines represented by formula (2). A diamine compound known in the art can be appropriately selected and used.
[0394] Examples of such diamine compounds include 1,4-diaminocyclohexane, 4,4'-diamino-2,2'-dimethylbiphenyl (hereinafter, sometimes referred to as m-Tb), 4,4'-diamino-3,3'-dimethylbiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (hereinafter, sometimes referred to as TFMB), 4,4'-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene (hereinafter, sometimes referred to as 1,3-APB), 1,4-bis(4-aminophenoxy)benzene (hereinafter, sometimes referred to as TPE-Q), 1,3-bis(4-aminophenoxy)benzene (hereinafter, sometimes referred to as TPE-R), 2,2-bis[4-(4-aminophenoxy)phenyl] propane (hereinafter, sometimes referred to as BAPP), 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)]biphenyl, bis[1-(4-aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)benzophenone, bis[4-(3-aminophenoxy)phenyl] 4,4'-methylenebis-o-toluidine, 4,4'-methylenebis-2,6-dimethylaniline, 4,4'-methylenebis-2,6-diethylaniline, 4,4'-methylenebis-aniline, 3,3'-methylenebis-aniline, 4,4'-diaminodiphenylpropane, 3,3'-diaminodiphenylpropane, 4,4'-diaminodiphenylethane, 3,3'-diaminodiphenylethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3-diaminodiphenylether, 3,4'-diaminodiphenylether , benzidine, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 4,4"-diamino-p-terphenyl, 3,3"-diamino-p-terphenyl, m-phenylenediamine, p-phenylenediamine (hereinafter sometimes referred to as p-PDA), resorcinol-bis(3-aminophenyl) ether, 4,4'-[1,4-phenylenebis(1-methylethylidene)] dianiline, 4,4'-[1,3-phenylenebis(1-methylethylidene)] dianiline, bis(p-aminocyclohexyl)methane, bis(p-β-amino-tert-butylphenyl) ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-Diaminonaphthalene, 2,4-bis(β-amino-tert-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-phenylenediamine, p-phenylenediamine, piperazine, 4,4'-diamino-2,2'-bis(trifluoromethyl)bicyclohexane, 4,4'-diaminodicyclohexylmethane, 4,4"-diamino-p-terphenyl, terephthalic acid bis(4-aminophenyl) ester, 1,4-bis(4-aminophenoxy)-2,5-di-tert-butylbenzene, 4,4'-(1, 3-phenylenediisopropyl) diphenylamine, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 2,4-diamino-3,5-diethyltoluene, 2,6-diamino-3,5-diethyltoluene, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-(hexafluoropropylene) diphenylamine, 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,2-diaminopropane, 1,2-diaminobutane , 1,3-diaminobutane, 2-methyl-1,2-diaminopropane, 2-methyl-1,3-diaminopropane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, norbornanediamine, 2'-methoxy-4,4'-diaminobenzanilide, 4,4'-diaminobenzanilide, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene, 9,9-bis[4 -(3-aminophenoxy)phenyl]fluorene, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,5-diamino-1,3,4-oxadiazole, bis[4,4'-(4-aminophenoxy)]benzanilide, bis[4,4'-(3-aminophenoxy)]benzanilide, 2,6-diaminopyridine, 2,5-diaminopyridine, etc. Among them, from the viewpoint of improving the puncture strength of the obtained laminated film, reducing Df and CTE, etc., it is preferred to use m-Tb, BAPP, TPE-Q, 1,3-bis(4-aminophenoxy)benzene and / or TPE-R in combination. The diamine compound can be used alone or in combination of two or more. ,
[0395] The PI-based resin precursor may be a product obtained by reacting other tetracarboxylic acids, dicarboxylic acids, tricarboxylic acids, and anhydrides and derivatives thereof in addition to the tetracarboxylic acid compound used in the synthesis of the PI-based resin precursor, within a range that does not impair the various physical properties of the obtained PI-based film.
[0396] As other tetracarboxylic acids, water addition products of anhydrides of the above-mentioned tetracarboxylic acid compounds can be mentioned.
[0397] As dicarboxylic acid compounds, aromatic dicarboxylic acids, aliphatic dicarboxylic acids and their similar acyl chloride compounds, acid anhydrides, etc. can be cited, and two or more kinds can be used in combination. As specific examples, terephthalic acid; isophthalic acid; naphthalene dicarboxylic acid; 4,4'-biphenyl dicarboxylic acid; 3,3'-biphenyl dicarboxylic acid; dicarboxylic acid compounds of chain hydrocarbons with a carbon number of 8 or less, and compounds in which two benzoic acids are linked by a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2- or phenylene, and their acyl chloride compounds can be cited.
[0398] As tricarboxylic acid compounds, aromatic tricarboxylic acids, aliphatic tricarboxylic acids and their similar acid chloride compounds, acid anhydrides, etc. can be cited, and two or more kinds can be used in combination. As specific examples, 1,2,4-benzenetricarboxylic acid anhydride; 2,3,6-naphthalenetricarboxylic acid-2,3-anhydride; a compound formed by phthalic anhydride and benzoic acid linked by a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2- or phenylene can be cited.
[0399] In the production of the PI-based resin precursor, the usage-amounts of the diamine compound, the tetracarboxylic acid compound, the dicarboxylic acid compound, and the tricarboxylic acid compound can be appropriately selected according to the ratio of each structural unit of the desired PI-based resin precursor.
[0400] In the present invention, the total number of moles of diamine compounds used relative to 1 mole of the total amount of tetracarboxylic acid compounds is defined as the amine ratio. In a preferred embodiment of the present invention, the amine ratio is preferably 0.90 moles or more, preferably 0.999 moles or less, relative to 1 mole of the total amount of tetracarboxylic acid compounds. In another embodiment, the amine ratio is preferably 1.001 moles or more, preferably 1.10 moles or less, relative to 1 mole of the total amount of tetracarboxylic acid compounds.
[0401] In one embodiment of the present invention, when the amine ratio is 1 or less, the amine ratio is preferably 0.90 mol to 0.999 mol, more preferably 0.95 mol to 0.997 mol, and even more preferably 0.97 mol to 0.995 mol.
[0402] In one embodiment of the present invention, when the amine ratio is 1 or more, the amine ratio is preferably 1.001 mol to 1.10 mol, more preferably 1.002 mol to 1.06 mol, and further preferably 1.003 mol to 1.05 mol.
[0403] If the amine ratio is close to 1.0 mol, the molecular weight tends to increase sharply during synthesis, and if the amine ratio is significantly different from 1.0 mol, the molecular weight of the obtained PI-based resin tends to decrease easily. If the molecular weight increases sharply, it tends to grow unevenly in the synthetic material, and the physical properties of the PI-based resin obtained from the PI-based resin precursor tend to be difficult to stabilize. On the other hand, if the molecular weight is too low, the mechanical properties tend to decrease.
[0404] The reaction temperature of the diamine compound and the tetracarboxylic acid compound is preferably 50°C or less, more preferably 40°C or less, and further preferably 30°C or less. In addition, the reaction temperature of the diamine compound and the tetracarboxylic acid compound is preferably 5°C or more, more preferably 10°C or more, and further preferably 15°C or more. If the reaction temperature is within the range of the upper and lower limits above, the effect of the present invention is easily obtained, and there is a tendency to increase the reaction rate and shorten the polymerization time. The reaction time is not particularly limited, and for example, it can be about 0.5 to 36 hours, and preferably 1 to 24 hours.
[0405] The reaction of the diamine compound and the tetracarboxylic acid compound is preferably carried out in a solvent. As a solvent, there is no particular limitation as long as it does not affect the reaction, and examples thereof include: alcohol solvents such as water, methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, 1-methoxy-2-propanol, 2-butoxyethanol, and propylene glycol monomethyl ether; phenol solvents such as phenol and cresol; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, propylene glycol methyl ether acetate, and ethyl lactate; lactone solvents such as γ-butyrolactone (hereinafter, sometimes recorded as GBL) and γ-valerolactone; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; Aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; alicyclic hydrocarbon solvents such as ethylcyclohexane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorinated solvents such as chloroform and chlorobenzene; amide solvents such as N,N-dimethylacetamide (hereinafter, sometimes described as DMAc) and N,N-dimethylformamide (hereinafter, sometimes described as DMF); sulfur-containing solvents such as dimethyl sulfone, dimethyl sulfoxide, and cyclopentane; carbonate solvents such as ethylene carbonate and propylene carbonate; pyrrolidone solvents such as N-methylpyrrolidone (hereinafter, sometimes described as NMP); and combinations thereof. Among them, from the viewpoint of solubility, phenol solvents, lactone solvents, amide solvents, and pyrrolidone solvents can be preferably used appropriately, and amide solvents are more preferred.
[0406] In one embodiment of the present invention, the boiling point of the solvent used in the reaction of the diamine compound and the tetracarboxylic acid compound is preferably suitable for the imidization conditions for controlling the parameter X in the laminated film and the thickness of the intermediate region within the desired range, preferably 230°C or less, more preferably 200°C or less, further preferably 180°C or less, preferably 100°C or more, more preferably 120°C or more.
[0407] The reaction of the diamine compound and the tetracarboxylic acid compound can be carried out in an inert atmosphere such as a nitrogen atmosphere or an argon atmosphere or under reduced pressure as necessary, and is preferably carried out in an inert atmosphere such as a nitrogen atmosphere or an argon atmosphere while stirring in a strictly controlled dehydrated solvent.
[0408] The obtained PI-based resin precursor can be temporarily isolated by a common method, but can also be used without isolation by appropriately diluting the reaction liquid containing the PI-based resin precursor obtained by synthesizing the PI-based resin precursor with a solvent as needed to prepare a PI-based resin precursor solution.
[0409] (Coating and pre-drying process)
[0410] In the manufacture of the laminated film in the present invention, the coating and pre-drying process is a process of coating a solution of a corresponding PI-based resin precursor on a supporting substrate and pre-drying it to obtain a multi-layer coating film. Specifically, the following methods can be cited: a method of obtaining a multi-layer coating film by repeating the process of coating a solution of a corresponding PI-based resin precursor on a supporting substrate and pre-drying it multiple times (sometimes referred to as a stepwise mode); a method of obtaining a multi-layer coating film by simultaneously coating and pre-drying the solution of a PI-based resin precursor corresponding to each layer in a state of stacking multiple layers by multi-layer extrusion (sometimes referred to as a simultaneous mode).
[0411] For example, in the case of a laminated film (L) having a layer (PI-2) containing a PI-based resin, a layer (PI-1) containing a PI-based resin, and a layer (PI-3) containing a PI-based resin in sequence, in a step-by-step mode, the following process can be performed: a PI-based resin precursor solution corresponding to the layer (PI-2) containing a PI-based resin is coated on a supporting substrate, and pre-dried to form a coating film; then, a PI-based resin precursor solution corresponding to the layer (PI-1) containing a PI-based resin is coated on the coating film, and pre-dried to form a two-layer coating film; then, a PI-based resin precursor solution corresponding to the layer (PI-3) containing a PI-based resin is coated on the two-layer coating film, and pre-dried to form a three-layer coating film. In addition, in the simultaneous mode, the following process can be performed: a PI-based resin precursor solution corresponding to a layer (PI-2) containing a PI-based resin, a PI-based resin precursor solution corresponding to a layer (PI-1) containing a PI-based resin, and a PI-based resin precursor solution corresponding to a layer (PI-3) containing a PI-based resin are simultaneously coated on a supporting substrate by multi-layer extrusion, etc., and pre-dried to form a three-layer coating film.
[0412] The solvent contained in the PI-based resin precursor solution may be a solvent exemplified as a solvent used in the reaction of a diamine compound and a tetracarboxylic acid compound in the manufacture of a PI-based resin precursor, preferably a lactone solvent, an amide solvent, a pyrrolidone solvent, and more preferably an amide solvent. In addition, in one embodiment of the present invention, the boiling point of the solvent contained in the PI-based resin precursor solution is preferably suitable for the imidization conditions for controlling the parameter X in the laminated film and the thickness of the intermediate region within the desired range, preferably 230°C or less, more preferably 200°C or less, further preferably 180°C or less, particularly preferably 170°C or less, preferably 100°C or more, and more preferably 120°C or more.
[0413] The content of the PI-based resin precursor contained in the PI-based resin precursor solution is preferably 8% by mass or more, more preferably 10% by mass or more, further preferably 12% by mass or more, particularly preferably 13% by mass or more, preferably 30% by mass or less, more preferably 25% by mass or less, further preferably 23% by mass or less, particularly preferably 20% by mass or less, relative to the total amount of the PI-based resin precursor solution. If the content of the PI-based resin precursor is within the above range, the processability during film formation is excellent.
[0414] The coating film of the PI-based resin precursor solution can be formed by applying the PI-based resin precursor solution on the supporting substrate using a known coating method or coating method. As a known coating method, for example, a wire rod coating method, a reverse coating method, a gravure coating method, a roller coating method such as a die coating method, a comma coating method, a lip coating method, a spin coating method, a screen printing coating method, a spray-type doctor blade coating method, a dipping method, a spray coating method, a curtain coating method, a slit coating method, a cast molding method, etc. can be cited. The PI-based resin precursor solution can be applied to the supporting substrate in a single layer or in multiple times to form a multi-layer coating film of the PI-based resin precursor solution, and a multi-layer laminated coating film of the PI-based resin precursor solution can also be formed simultaneously. As a method for simultaneously forming a multi-layer coating film, for example, a co-extrusion processing method, a multi-layer curtain coating method, etc. can be used.
[0415] As an example of a supporting substrate, metal plates (such as copper plates, etc.), SUS plates such as SUS foil and SUS tape, glass substrates, PET films, PEN films, other PI resin films except the layer containing PI resin in the present invention, polyamide resin films, etc. can be cited as metal foil (such as copper foil) and other metal plates (such as copper plates, etc.), SUS foil, SUS tape, etc., glass substrates, PET films, PEN films, etc. can be cited. Wherein, from the viewpoint of excellent heat resistance, preferably copper plates, SUS plates, glass substrates, PET films, PEN films, etc. can be cited, and from the viewpoint of adhesion and cost, copper plates, SUS plates, glass substrates or PET films, etc. can be more preferably cited. In one embodiment of the present invention, as the metal constituting the metal plate, for example, aluminum, copper, iron, nickel, chromium, titanium, tantalum, stainless steel and their alloys, etc. can be cited. Among them, metal foil is preferably copper foil, copper alloy foil, SUS foil, aluminum foil, etc., and from the viewpoint of electrical conductivity and metal processing, copper foil or copper alloy foil is more preferably, and copper foil is particularly preferably. By using a metal layer (such as metal foil, etc.) as a supporting substrate, a resin film can also be directly formed on the metal layer.
[0416] In the coating and pre-drying process, the temperature for pre-drying the multilayer coating film is preferably 60°C or more, more preferably 70°C or more, more preferably 80°C or more, more preferably 90°C or more, preferably 200°C or less, more preferably 150°C or less, and more preferably 130°C or less. In addition, the pre-drying time is preferably 30 seconds or more, more preferably 1 minute or more, more preferably 5 minutes or more, and more preferably 10 minutes or more, for example, 15 minutes or more, 20 minutes or more, or 25 minutes or more, and preferably 24 hours or less, more preferably 12 hours or less, more preferably 6 hours or less, and particularly preferably 1 hour or less. If the pre-drying temperature and pre-drying time are within the above range, it is easy to become a state where the solvent remains in the multilayer coating film during imidization.
[0417] (Stationary process)
[0418] The standing process is a process for standing the multilayer coating obtained in the coating and pre-drying process. By being supplied to the standing process before the imidization process, it is easy to become a state in which the solvent fully remains in the entire coating or a state in which the resin layers are well fused during imidization, and the degree of freedom of the resin molecules can be increased until the imidization. Due to this influence, the plane orientation of the PI-based resin contained in each layer containing the PI-based resin is moderately reduced, that is, the orientation in the plane direction is appropriately disordered. Moreover, the degree of disorder of the orientation in each layer of the layers (preferably mPI layers and TPI layers) containing PI-based resins with different thicknesses is different, therefore, differences will be produced in the degree of reduction of P1 and P2. Here, as described above, in the case where the layer (PI-2) (preferably TPI layer) is more likely to produce a disorder of the plane orientation, the reduction value of P2 will become greater than the reduction value of P1, therefore, there is a tendency for the value of the molecule (P1 / P2) to increase. On the other hand, since the planar orientation of both layers is reduced, the difference between the numerical values of P1 and P2 also tends to become smaller. In addition, even in the case where the planar orientation disorder of layer (PI-1) (preferably mPI layer) is more likely to occur, as described above, since the planar orientation of both layers is reduced, there is a tendency that the value of the denominator (|P1-P2|) is reduced to a degree greater than the value of the numerator (P1 / P2). Therefore, it is believed that by being provided to the static process, there is a tendency that the (P1 / P2) / (|P1-P2|) in formula (I) increases, and it is easy to satisfy formula (I). It is also believed that if it is provided to the static process, it is easy to produce a moderate disorder of orientation until the center of the layer (PI-1), therefore, there is a tendency that P1c / P1 becomes more than a specified value, and it is easy to satisfy formula (II). It is also believed that by being provided to the static process, the PI-based resins constituting each layer are easily mixed with each other near the interface of each layer, so the thickness of the intermediate region will become larger.
[0419] In the standing process, the time (also referred to as the standing time) of the multilayer coating film being standing can be suitably selected according to the temperature (also referred to as the standing temperature) when standing, it is not particularly limited, but preferably more than 3 hours, more preferably more than 6 hours, more preferably more than 12 hours, more preferably more than 18 hours, particularly preferably more than 22 hours, for example, more than 24 hours, more than 30 hours, more than 36 hours or more than 45 hours. The upper limit of the standing time of the multilayer coating film is not particularly limited, and can usually be less than 450 hours, preferably less than 100 hours. If the standing time of the multilayer coating film is the aforementioned range, then when imidization, it is easy to become the state (or the state of good fusion) that the solvent fully remains in the entire coating film, therefore, it is easy to adjust the parameter X in the laminated film, the thickness of the intermediate region to the desired range.
[0420] In addition, in a preferred embodiment of the present invention, the standing step is preferably a step of standing (or storing) the multilayer coating film at low temperature (preferably under refrigeration). By standing (or storing) at low temperature, it is easy to make the solvent more fully remain in the entire coating film, or the resin layers are more well fused, so that the degree of freedom of the resin molecules until imidization can be higher, so it is easier to adjust the above-mentioned parameter X and the thickness of the intermediate region to the desired range.
[0421] In the standing process, the standing temperature of the multilayer coating is preferably below 20°C, more preferably below 15°C, further preferably below 10°C, further more preferably below 8°C, and particularly preferably below 5°C. When the standing temperature of the multilayer coating is below the aforementioned upper limit, it is easier to make a state in which the solvent fully remains in the entire coating (or a well-fused state) during imidization, so it is easier to adjust the above-mentioned parameter X and the thickness of the middle region in the laminated film to the desired range. In addition, the lower limit of the standing temperature of the multilayer coating is usually above -30°C, preferably above -20°C, further preferably above -10°C, further more preferably above -5°C, and particularly preferably above 0°C. It should be noted that the standing process can be carried out, for example, in air or in an inert gas atmosphere, or in a closed space.
[0422] In addition, in a preferred embodiment of the present invention, the laminated film obtained by the manufacturing method including the above-mentioned standing step easily satisfies formula (I) and formula (II), and the thickness of the middle region easily satisfies the above-mentioned range. Therefore, it is not only easy to obtain high puncture strength, but also easy to maintain Df at a low level.
[0423] (Imidization step)
[0424] The imidization step is a step of imidizing each PI-based resin in the multilayer coating film on the supporting substrate by heat treatment at, for example, 200° C. to 500° C.
[0425] In one embodiment of the present invention, the imidization process preferably includes the following steps: heating from a low temperature (referred to as the first temperature) to a high temperature (referred to as the second temperature) at a faster rate, and maintaining at the high temperature. By performing imidization at a faster rate, preferably rapidly heating, and maintaining the temperature for a certain period of time after reaching a high temperature to complete the imidization, it is advantageous in terms of the formation of a higher-order structure and a branched structure of the PI-based resin, and therefore, the obtained laminated film maintains Df at a low level and easily improves the puncture strength. In addition, it can also be advantageous from the perspective of obtaining a smooth laminated film.
[0426] In one embodiment of the present invention, the first temperature is preferably 20°C to 50°C, more preferably 25°C to 35°C, and the second temperature is preferably 220°C to 450°C, more preferably 250°C to 400°C, further preferably 300°C to 380°C, and particularly preferably 330°C to 360°C. According to the laminated film of the present invention, even if imidization is performed at a relatively low temperature of, for example, 360°C or less (preferably 350°C or less), it can exhibit high puncture strength or reduce Df. In addition, if the imidization temperature is 360°C or less (preferably 350°C or less), even when copper foil is used as a supporting substrate, thermal degradation of the copper foil can be suppressed, and therefore, a laminated sheet with excellent high-frequency characteristics can be easily obtained. In addition, from the viewpoint of sufficiently improving the imidization rate, improving the puncture strength, and reducing the Df, the imidization temperature is preferably 200°C or more, more preferably 210°C or more, and more preferably 220°C or more.
[0427] In one embodiment of the present invention, the temperature rise from the first temperature to the second temperature may be carried out at a temperature rise rate of one stage, or at a temperature rise rate of two or more stages. In one embodiment of the present invention, when the temperature rise from the first temperature to the second temperature is carried out in one stage, the temperature rise rate is preferably 3.5°C / min or more, more preferably 5°C / min or more, further preferably 7°C / min or more, further more preferably 10°C / min or more, particularly preferably 15°C / min or more, particularly preferably 20°C / min or more, preferably 50°C / min or less, more preferably 40°C / min or less, and further preferably 35°C / min or less. When the temperature rise rate is carried out in two or more stages, the temperature rise rate of the first stage may be the same as or different from the temperature rise rate of the second stage, and preferably the temperature rise rate after the second stage is faster than that of the first stage. The heating rate in the first stage may preferably be 1 to 15°C / min or less, more preferably 3 to 12°C / min or less, and the heating rate in the second and subsequent stages may preferably be 3 to 35°C / min or less, more preferably 8 to 25°C / min or less.
[0428] If the above-mentioned heating rate is adopted, it is advantageous in terms of the formation of the higher-order structure and the branched structure of the PI-based resin, so that the obtained laminated film maintains Df at a low level and easily improves the puncture strength. In addition, it is also advantageous from the viewpoint of obtaining a smooth laminated film.
[0429] In one embodiment of the present invention, the heating time from the first temperature to the second temperature can be appropriately selected according to their temperature and heating rate, preferably less than 5 hours, more preferably less than 3 hours, further preferably less than 2 hours, particularly preferably less than 1 hour, and according to the circumstances, it can also be less than 50 minutes, in addition, preferably more than 3 minutes, more preferably more than 5 minutes, and more preferably more than 7 minutes. If the heating time from the first temperature to the second temperature is the above-mentioned range, the obtained laminated film maintains Df at a low level and easily improves the puncture strength.
[0430] In one embodiment of the present invention, the holding time at the second temperature is preferably 1 minute or more, more preferably 3 minutes or more, preferably 30 minutes or less, more preferably 20 minutes or less, and further preferably 10 minutes or less. When the heating rate from the first temperature to the second temperature is within the above range and the holding time at the second temperature is within the above range, it is advantageous in terms of the formation of a higher-order structure and a branched structure of the PI-based resin, and therefore, the obtained laminated film maintains Df at a low level and is easy to improve the puncture strength.
[0431] After imidization, the multilayer coating film formed on the supporting substrate is peeled off from the supporting substrate to obtain a laminated film. In one embodiment of the present invention, when the supporting substrate is a metal foil (e.g., copper foil), the coating film may not be peeled off from the metal foil to obtain a laminated sheet having a laminated film stacked on the metal foil.
[0432] <Physical Properties of Laminated Film>
[0433] In one embodiment of the present invention, the content of the PI-based resin in each layer containing PI-based resin constituting the laminated film is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more relative to the mass of the layer containing PI-based resin. In addition, the upper limit of the content of the PI-based resin is not particularly limited, and relative to the mass of the layer containing the PI-based resin, for example, it can be 100% by mass or less, 99% by mass or less, or 95% by mass or less. If the content of the PI-based resin is within the above range, a laminated film having improved puncture strength, dielectric properties, and thermal properties can be obtained.
[0434] In the laminated film of the present invention, each layer containing PI-based resin can contain fillers as needed. As fillers, metal oxide particles such as silica, aluminum oxide, inorganic salts such as calcium carbonate, fluororesins, polymer particles such as cycloolefin polymers, etc. can be cited. Fillers can be used alone or in combination of two or more. In the case of containing fillers, relative to the mass of the layer containing PI-based resin, its content is preferably 50% by mass or less, more preferably 40% by mass or less, further preferably 30% by mass or less, preferably 0.01% by mass or more.
[0435] In addition, in one embodiment of the present invention, each layer containing PI resin constituting the laminated film of the present invention can contain additives as needed. As additives, for example, antioxidants, flame retardants, crosslinking agents, surfactants, compatibilizers, imidization catalysts, weathering agents, lubricants, anti-blocking agents, antistatic agents, anti-corona agents, drip-free agents, pigments, etc. can be cited. Additives can be used alone or in combination of two or more. The content of various additives can be appropriately selected within the scope of not damaging the effect of the present invention. In the case of including various additives, relative to the mass of each layer containing PI resin, its total content is preferably 7% by mass or less, more preferably 5% by mass or less, further preferably 4% by mass or less, particularly preferably 1% by mass or less, preferably 0.001% by mass or more.
[0436] Printed circuits are required to reduce transmission loss. Transmission loss is represented by the sum of dielectric loss, which is loss caused by the electric field generated by the dielectric, and conductor loss, which is loss caused by the current flowing through the conductor. In addition, it is known that dielectric loss is approximately proportional to the index E represented by formula (i).
[0437] E=Df×(Dk) 1 / 2 (i)
[0438] [In formula (i), Df represents dielectric loss tangent, and Dk represents relative dielectric constant]
[0439] In the high-frequency region used for FPCs for high-speed communications such as 5G, there is a tendency for dielectric loss to increase, and therefore, a material having a small value of the index E and capable of suppressing dielectric loss is particularly required.
[0440] On the other hand, the current of high-frequency signals is concentrated on the outermost surface of the conductor. Therefore, the conductor loss is related to the dielectric properties of the dielectric in contact, and it is known that it is related to (Dk) 1 / 2 Approximately proportional.
[0441] The Df and Dk of the laminated film of the present invention are small, and the dielectric loss index E and the conductor loss are also reduced, so that the transmission loss can be reduced in the circuit including the laminated film. Therefore, the laminated film of the present invention can maintain excellent dielectric properties (especially maintain low Df) and show high puncture strength.
[0442] In one embodiment of the present invention, the dielectric loss index E of the laminated film at 10 GHz is preferably 0.0080 or less, more preferably 0.0075 or less, further preferably 0.0070 or less, further more preferably 0.0065 or less, particularly preferably 0.0060 or less, and particularly preferably 0.0059 or less. The smaller the index E, the lower the transmission loss of the electronic circuit including the laminated film, and therefore, the lower limit of the index E is not particularly limited, and for example, it can be 0 or more.
[0443] In one embodiment of the present invention, from the viewpoint of reducing the transmission loss of the electronic circuit when the laminated film is assembled in the electronic circuit, the Df of the laminated film at 10 GHz is preferably 0.0040 or less, more preferably 0.0035 or less, further preferably 0.0034 or less, further more preferably 0.0033 or less, and particularly preferably 0.0032 or less. The smaller the Df, the lower the transmission loss of the electronic circuit including the laminated film, and therefore, the lower limit of the Df is not particularly limited, and for example, it can be 0 or more.
[0444] In one embodiment of the present invention, Dk of the laminated film at 10 GHz is preferably 3.500 or less, more preferably 3.450 or less, and even more preferably 3.400 or less.
[0445] Df and Dk of the laminated film can be measured using a vector network analyzer and a resonator, for example, by the method described in Examples.
[0446] In one embodiment of the present invention, the coefficient of linear expansion (CTE) of the laminated film is preferably less than 45ppm / K, more preferably less than 40ppm / K, further preferably less than 35ppm / K, further more preferably less than 32ppm / K, for example, less than 31ppm / K, less than 30ppm / K, less than 28ppm / K, less than 25ppm / K, or less than 23ppm / K. If the CTE of the laminated film is less than the above-mentioned upper limit, the thermal properties are excellent and high dimensional stability can be expected. In addition, the CTE of the laminated film is preferably more than 0ppm / K, more preferably more than 5ppm / K, more preferably more than 8ppm / K, and particularly preferably more than 10ppm / K. If the CTE of the laminated film is within the range of the above-mentioned upper and lower limits, the CTE of the metal layer (especially the copper layer such as copper foil) and the layer containing the PI-based resin of the laminated film becomes close, so the effect of suppressing the laminated film from peeling off the metal layer can be obtained. In addition, CTE can be measured using, for example, a thermomechanical analyzer (hereinafter, sometimes referred to as "TMA") and can be obtained by the method described in the Examples.
[0447] The laminated film of the present invention may be subjected to surface treatment such as corona discharge treatment, plasma treatment, ozone treatment, etc. by a method generally used in industry.
[0448] In one embodiment of the present invention, for the laminated film of the present invention, the puncture strength (value) when the thickness of the laminated film is converted to 50 μm is preferably 12.0N or more, more preferably 14.0N or more, further preferably 16.0N or more, further preferably 20.0N or more, and particularly preferably 23.0N or more. In other words, the puncture strength per unit thickness of the laminated film of the present invention is preferably 0.24N / μm or more, more preferably 0.28N / μm or more, further preferably 0.32N / μm or more, further preferably 0.40N / μm or more, and particularly preferably 0.46N / μm or more. If the puncture strength of the laminated film is above the aforementioned lower limit, it is possible to effectively suppress the damage when impacted in the thickness direction of the film. The upper limit of the puncture strength of the laminated film is not limited, for example, it can be 50N or less. For the puncture strength, it can be measured using a small desktop tester in accordance with JIS Z 1707 at a temperature of 23°C and a relative humidity of 50%. Specifically, it can be measured by the method described in Examples described later, for example.
[0449] The laminated film of the present invention has high puncture strength, and therefore, can be suitably used for substrate materials that can cope with printed circuit boards, antenna substrates, etc. In addition, the laminated film of the present invention has low D f, and therefore, even in a high-frequency band for transmitting high-frequency signals, low transmission loss can be achieved. Therefore, it is suitable as a substrate material for printed circuit boards and antenna substrates that can cope with high-speed communication applications such as 5G, in particular.
[0450] [Laminated sheet]
[0451] The laminated film of the present invention has a sufficiently high puncture strength and can reduce Df, and can therefore be suitably used to form a metal-clad laminate used in an FPC. Therefore, the present invention includes a laminated sheet comprising the laminated film of the present invention and a metal layer. In one embodiment of the present invention, the laminated sheet of the present invention may include a metal layer only on one side of the laminated film of the present invention, or may include a metal layer on both sides of the laminated film of the present invention.
[0452] In one embodiment of the present invention, as the metal constituting the metal layer, for example, aluminum, copper, iron, nickel, chromium, titanium, tantalum, stainless steel and their alloys etc. can be cited. Among them, the metal layer is preferably a copper layer, a copper alloy layer, a SUS layer, an aluminum layer etc., and from the viewpoint of electrical conductivity and metal processability, a copper layer or a copper alloy layer is more preferably used, and a copper layer is particularly preferably used. In addition, from the viewpoint of metal processability, the metal layer is preferably a metal foil layer. As the metal constituting the metal foil layer, the metals described above can be cited. Among them, as the metal foil layer, a copper foil layer, a copper alloy foil layer, a SUS foil layer, an aluminum foil layer etc. are preferably used, and from the viewpoint of electrical conductivity and metal processability, a copper foil layer or a copper alloy foil layer is more preferably used, and a copper foil layer is particularly preferably used.
[0453] The metal layer can be manufactured by plastic processing such as electrolytic casting, rolling, etc., such as electroplating, or commercially available products. When the metal layer is a metal foil, a surface treatment layer can be set on the surface of at least one side of the metal foil by electroplating. As the surface treatment layer, a roughening layer, an antirust layer, an alloy layer further provided between the surface of the metal foil and the aforementioned roughening layer as required, a chromate layer provided on the surface of the antirust layer, a silane coupling agent layer, etc. can be cited. When the metal layer is a copper foil, electrolytic copper foil and rolled copper foil can be used, and the metal layer preferably has a roughening layer formed by two or more elements of copper, zinc, titanium, tungsten, molybdenum, nickel, cobalt, iron or them, and / or an antirust layer formed by two or more elements of zinc, tin, nickel, cobalt, chromium, molybdenum or them. From the viewpoint of uniformly setting the roughening layer, it is preferred to further pre-set an alloy layer of copper and at least one or more elements selected from molybdenum, zinc, tungsten, nickel, cobalt and iron on the surface of the copper foil.
[0454] In one embodiment of the present invention, the thickness of the metal layer, especially the metal foil layer such as the copper foil layer, is preferably 1 μm or more, more preferably 5 μm or more, and from the viewpoint of easy miniaturization of the circuit and easy improvement of bending resistance, it is preferably 100 μm or less, more preferably 50 μm or less, further preferably 30 μm or less, and particularly preferably 20 μm or less. The thickness of the metal layer, especially the copper foil layer, can be measured using a film thickness meter or the like. It should be noted that when both sides of the laminated film include metal foil layers, especially copper foil layers, the thickness of each metal foil layer, especially each copper foil layer, may be the same or different from each other.
[0455] The laminated sheet of the present invention may include other layers such as a functional layer in addition to the laminated film of the present invention and the metal layer, especially a metal foil layer such as a copper foil layer. As the functional layer, for example, an adhesive layer can be mentioned. The functional layer can be used alone or in combination of two or more.
[0456] In one embodiment of the present invention, the laminated sheet of the present invention can be a metal-clad laminated plate composed of a laminated film comprising a metal layer and two or more layers containing a PI-based resin, or can be a metal-clad laminated plate composed of a laminated film comprising a metal layer, two or more layers containing a PI-based resin and an adhesive layer, but from the viewpoint of heat resistance, dimensional stability and lightweight, a metal-clad laminated plate without an adhesive layer is preferred.
[0457] In addition, the laminated film of the present invention can be formed at a relatively low imidization temperature, and even when a laminated sheet having a copper foil as a metal layer is produced by thermal imidization of a PI-based resin precursor coating on a copper foil, degradation of the copper foil surface can be suppressed, and sufficiently high puncture strength and low Df can be achieved. Therefore, the laminated sheet of the present invention has excellent high-frequency characteristics even if it does not contain an adhesive layer.
[0458] In addition, in one embodiment of the present invention, the laminated film of the present invention and the metal layer, especially the metal foil layer such as the copper foil layer, can be directly connected, or a functional layer can be inserted between the laminated film and the metal layer, especially the metal foil layer such as the copper foil layer, so that they are connected via the functional layer. However, from the viewpoint of improving the puncture strength and thermal properties, it is preferred that the laminated film and the metal layer, especially the metal foil layer such as the copper foil layer, are directly connected.
[0459] <Method for producing laminated sheet>
[0460] The laminated sheet of the present invention can be produced, for example, by a method comprising the following steps:
[0461] A process of coating a corresponding PI-based resin precursor solution on the metal layer and pre-drying the solution to obtain a multilayer coating film;
[0462] a step of allowing the obtained multilayer coating film to stand; and
[0463] A step of heating the multilayer coating film to imidize the PI-based resin, thereby forming the laminated film of the present invention on the metal layer.
[0464] In the above-mentioned production method, the description of each step in the production method of the laminated film of the present invention described above is similarly applicable, and the preferred embodiments and the like are also the same.
[0465] The laminated sheet of the present invention can also be manufactured by a method other than the above method, such as the following method: a PI-based resin precursor solution is applied to other supporting substrates other than the metal layer (such as metal foil) contained in the laminated sheet and dried, and the multilayer coating of the PI-based resin precursor thus obtained is peeled off from the aforementioned substrate, and the peeled multilayer coating of the aforementioned PI-based resin precursor is bonded to the metal layer. As a method for bonding the multilayer coating of the PI-based resin precursor to the metal layer, a pressurization-based method, a lamination method using a hot roller, etc. can be adopted. In the bonding process, the imidization of the PI-based resin precursor can also be carried out simultaneously. However, the laminated film of the present invention can be formed at a relatively low imidization temperature. Even if a laminated sheet having a metal layer of copper foil is manufactured by thermal imidization of the PI-based resin precursor coating on copper foil, the deterioration of the copper foil surface can be suppressed, and high puncture strength and low Df can be achieved. Therefore, even if the laminated sheet of the present invention is not manufactured through the above-mentioned bonding process, it has excellent high-frequency characteristics.
[0466] In addition, the laminated sheet of the present invention can also be manufactured by the following methods: a method of preparing a resin film as described in the <Method for Manufacturing Laminated Film> and then laminating it with a metal layer by heat pressing, heat lamination, etc.; a method of performing metal plating on the surface of the laminated film to thereby provide a metal layer (metal plated layer) on the surface of the laminated film. From the viewpoint of the conductivity of the laminated sheet, the metal plated layer is preferably a copper plated layer or a copper alloy plated layer, and more preferably a copper plated layer.
[0467] [Flexible printed circuit board]
[0468] The laminated film of the present invention has excellent puncture strength, so it can be suitably used as an FPC substrate material. In addition, the laminated film of the present invention can have a lower Df, so it is possible to reduce the transmission loss of the electrical circuit formed by assembling the laminated film. In addition, the CTE of the laminated film of the present invention is also low, and the thermal properties are also excellent, so it can be suitably used as an FPC substrate material, especially an FPC substrate material for high-speed communication purposes such as 5G. Therefore, the present invention also includes a flexible printed circuit substrate, which includes the laminated film or laminated sheet of the present invention.
[0469] Example
[0470] Hereinafter, the present invention will be described in more detail based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0471] The abbreviations used in Examples and Comparative Examples represent the following compounds.
[0472] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride
[0473] BP-TME: 4,4'-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl
[0474] PMDA: pyromellitic dianhydride
[0475] m-Tb: 4,4'-diamino-2,2'-dimethylbiphenyl
[0476] TPE-Q: 1,4-bis(4-aminophenoxy)benzene
[0477] TPE-R: 1,3-bis(4-aminophenoxy)benzene
[0478] 1. Preparation of polyimide resin precursor solution
[0479] (1) Polyimide resin precursor solution 1
[0480] 48.61 g (228.9 mmol) of m-Tb and 66.92 g (228.9 mmol) of TPE-Q were dissolved in 1598 g of DMAc, and then 118.22 g (221.2 mmol) of BP-TME was added, and the mixture was stirred at 20° C. for 1 hour under a nitrogen atmosphere. Then, 48.25 g (221.2 mmol) of PMDA was added, and the mixture was stirred at 20° C. for 3 hours under a nitrogen atmosphere to obtain a PI-based resin precursor solution 1. The molar ratio of the diamine monomer to the acid dianhydride monomer used was 1.04.
[0481] (2) Polyimide resin precursor solution 2
[0482] 9.87 g (46.5 mmol) of m-Tb and 122.35 g (418.5 mmol) of TPE-R were dissolved in 1890 g of DMAc, and then 30.26 g (138.7 mmol) of PMDA and 95.25 g (323.7 mmol) of BPDA were added in sequence, and stirred at 20° C. for 3 hours under a nitrogen atmosphere to obtain a PI-based resin precursor solution 2. The molar ratio of the diamine monomer to the acid dianhydride monomer used was 1.01.
[0483] (3) Polyimide resin precursor solution 3
[0484] 14.40 g (67.8 mmol) of m-Tb and 19.82 g (67.8 mmol) of TPE-Q were dissolved in 405 g of DMAc, and then 7.11 g (13.3 mmol) of BP-TME was added, and the mixture was stirred at 20° C. for 1 hour under a nitrogen atmosphere. Then, 14.50 g (66.5 mmol) of PMDA and 15.65 g (53.2 mmol) of BPDA were added, and the mixture was stirred at 20° C. for 3 hours under a nitrogen atmosphere to obtain a PI-based resin precursor solution 3. The molar ratio of the diamine monomer to the acid dianhydride monomer used was 1.02.
[0485] (4) Polyimide resin precursor solution 4
[0486] 57.72 g (271.9 mmol) of m-Tb and 8.83 g (30.2 mmol) of TPE-Q were dissolved in 810 g of DMAc, and then 32.53 g (149.1 mmol) of PMDA and 43.87 g (149.1 mmol) of BPD A were added, and stirred at 20° C. for 3 hours under a nitrogen atmosphere to obtain a PI-based resin precursor solution 4. The molar ratio of the diamine monomer to the acid dianhydride monomer used was 1.01.
[0487] 2. Fabrication of laminated films
[0488] (1) Embodiment 1
[0489] On the roughened side (surface roughness; Rz = 0.6 μm) of the electrolytic copper foil (thickness of 12 μm), the PI-based resin precursor solution 2 / PI-based resin precursor solution 1 / PI-based resin precursor solution 2 prepared above were simultaneously applied as the upper layer / middle layer / lower layer in a manner of 5 μm / 40 μm / 5 μm in dry thickness, thereby forming a three-layer laminated coating of the PI-based resin precursor solution. Next, the three-layer laminated coating was heated at 100°C for 12 minutes to dry it, and then the laminate formed by the copper foil and the three-layer laminated coating was placed in a sealed container and allowed to stand for 24 hours at a temperature of 4°C. Then, after confirming that the laminated body taken out of the sealed container had reached room temperature, it was fixed to a metal frame, and in an atmosphere with an oxygen concentration of 1%, the temperature was raised from 30°C to 320°C over 10 minutes, and then maintained at 320°C for 5 minutes. The obtained laminated film with copper foil formed by the layer containing PI-based resin and copper foil was immersed in a large volume of 40% by mass ferric chloride aqueous solution at room temperature for 10 minutes, and then the ferric chloride aqueous solution was washed with pure water. After visually confirming that there was no copper residue, it was dried at 80°C for 1 hour to obtain a laminated film 1 laminated in the order of layer (PI-2) (copper foil layer side), layer (PI-1) and layer (PI-3) (TPI layer, mPI layer and TPI layer). The thickness of the laminated film 1 is 50 μm, the thickness of the intermediate region between the layer (PI-2) and the layer (PI-1) is 1800 nm, the thickness of the layer (PI-2) and the layer (PI-3) is 4.1 μm each, and the thickness of the layer (PI-1) is 38.2 μm.
[0490] (2) Embodiment 2
[0491] On the roughened side (surface roughness; Rz = 0.6 μm) of the electrolytic copper foil (thickness 12 μm), PI-based resin precursor solution 2 is applied in a manner that the dry thickness becomes 5 μm to obtain a coating film. The aforementioned coating film is heated at 120°C for 10 minutes to be dried, and on the dried coating film, PI-based resin precursor solution 3 is applied in a manner that the dry thickness becomes 36 μm to obtain a double-layer laminated coating film. The aforementioned double-layer laminated coating film is heated at 120°C for 30 minutes to be dried, and on the dried double-layer laminated coating film, PI-based resin precursor solution 2 is applied in a manner that the dry thickness becomes 5 μm to obtain a three-layer laminated coating film. After the aforementioned three-layer laminated coating film is heated at 120°C for 30 minutes to be dried, the laminate formed by the copper foil and the aforementioned three-layer laminated coating film is placed in a sealed container and allowed to stand for 24 hours at a temperature of 4°C. Then, after confirming that the aforementioned laminate taken out from the sealed container has become room temperature, the laminate formed by the copper foil and the PI-based resin precursor is fixed to a metal frame, and in an atmosphere with an oxygen concentration of 1%, after heating from 30°C to 320°C over 10 minutes, it is maintained at 320°C for 5 minutes. The obtained laminated film with copper foil formed by the layer containing the PI-based resin and the copper foil is immersed in a large volume of 40% by mass ferric chloride aqueous solution at room temperature for 10 minutes, and then the ferric chloride aqueous solution is washed with pure water. After visually confirming that there is no copper residue, it is dried at 80°C for 1 hour to obtain a laminated film 2 stacked in the order of layer (PI-2) (copper foil layer side), layer (PI-1) and layer (PI-3) (TPI layer, mPI layer and TPI layer). The thickness of the laminated film 2 is 46 μm, the thickness of the intermediate region between the layers (PI-2) and (PI-1) is 2500 nm, the thicknesses of the layers (PI-2) and (PI-3) are 3.8 μm each, and the thickness of the layer (PI-1) is 33.5 μm.
[0492] (3) Embodiment 3
[0493] As the upper layer / middle layer / lower layer, PI-based resin precursor solution 2 / PI-based resin precursor solution 4 / PI-based resin precursor solution 2 were applied in a manner to have a dry thickness of 5 μm / 36 μm / 5 μm, respectively. In the same manner as in Example 2, a laminated film 3 was obtained in which layer (PI-2) (copper foil layer side), layer (PI-1) and layer (PI-3) (TPI layer, mPI layer and TPI layer) were laminated in this order. The thickness of the laminated film 3 was 46 μm, the thickness of the intermediate region between the layer (PI-2) and the layer (PI-1) was 2800 nm, the thickness of the layer (PI-2) and the layer (PI-3) was 3.6 μm each, and the thickness of the layer (PI-1) was 33.2 μm.
[0494] (4) Embodiment 4
[0495] It was left standing for 48 hours in an environment at 4°C, and otherwise, the operation was the same as in Example 1 to obtain a laminated film 4 laminated in the order of layer (PI-2) (copper foil layer side), layer (PI-1), and layer (PI-3) (TPI layer, mPI layer, and TPI layer). The thickness of this laminated film 4 was 50 μm, the thickness of the intermediate region between layer (PI-2) and layer (PI-1) was 2900 nm, the thicknesses of layer (PI-2) and layer (PI-3) were each 3.6 μm, and the thickness of layer (PI-1) was 37.1 μm.
[0496] (5) Comparative Example 1
[0497] As the upper layer / middle layer / lower layer, the PI-based resin precursor solution 2 / PI-based resin precursor solution 1 / PI-based resin precursor solution 2 was coated in such a manner that the dry thicknesses were 5 μm / 36 μm / 5 μm, respectively. Without leaving it standing in an environment at 4°C, heat treatment was immediately carried out at 320°C, and otherwise, the operation was the same as in Example 2 to obtain a laminated film 5 laminated in the order of layer (PI-2) (copper foil layer side), layer (PI-1), and layer (PI-3) (TPI layer, mPI layer, and TPI layer). The thickness of this laminated film 5 was 46 μm, the thickness of the intermediate region between layer (PI-2) and layer (PI-1) was 250 nm, the thicknesses of layer (PI-2) and layer (PI-3) were each 4.9 μm, and the thickness of layer (PI-1) was 35.8 μm.
[0498] <Film thickness measurement>
[0499] From the laminated films 1 to 5 obtained in the examples and comparative examples, arbitrary portions were cut out in 5 mm × 5 mm, embedded with resin, and thus samples for film thickness measurement were prepared. For the prepared samples for film thickness measurement, they were cut with a microtome to prepare a measurement cross-section, and the thickness of the laminated film was measured using a laser microscope under the following conditions.
[0500] Device: LEXT OLS4100 manufactured by Olympus Corporation
[0501] Observation magnification: 100 times
[0502] <Measurement of Df and Dk>
[0503] From the laminated films 1 to 5 obtained in the examples and comparative examples, measurement samples of 50 mm × 50 mm were cut out, and Df and Dk were measured under the following conditions. It should be noted that the measurement was carried out after conditioning the measurement samples at 23°C / 50% RH for 24 hours.
[0504] Device: Compact USB vector network analyzer manufactured by Anritsu Corporation (product name: MS46122B)
[0505] Cavity resonator manufactured by AET Inc. (TE mode 10 GHz type)
[0506] Measurement frequency: 10 GHz
[0507] Measurement atmosphere: 23℃ / 50%RH
[0508] <Determination of Coefficient of Thermal Expansion (CTE)>
[0509] The CTE of the laminated films 1 to 5 obtained in the examples and comparative examples was measured using a thermomechanical analyzer TMA under the following conditions, and the CTE at 50° C. to 100° C. was calculated.
[0510] Device: TMA / SS7100 manufactured by Hitachi High-Tech Science Corporation Load: 50.0 mN
[0511] Temperature program: from 20°C to 130°C at a rate of 5°C / min
[0512] Test piece: 40mm in length, 5mm in width
[0513] <Determination of Storage Elastic Modulus>
[0514] The storage elastic modulus of each PI-based resin formed from the PI-based resin precursor solutions 1 to 5 was determined by measuring a PI-based resin film produced by the following method under the following conditions.
[0515] Each PI-based resin precursor solution was cast on a glass substrate in a manner such that the dry thickness was 30 μm, thereby forming a coating film of the PI-based resin precursor solution. The coating film was heated at 120° C. for 30 minutes, and the obtained film was peeled off from the glass substrate and fixed to a metal frame. In an atmosphere with an oxygen concentration of 1%, the film fixed to the metal frame was heated from 30° C. to 320° C. over 10 minutes, and then maintained at 320° C. for 5 minutes to obtain a PI-based resin film.
[0516] The storage modulus (Storage modulus, E') was obtained by measuring the dynamic viscoelasticity using a dynamic viscoelasticity measuring apparatus (DVA-220 manufactured by IT Measurement Control Co., Ltd.) with the following samples and conditions.
[0517] Test piece: Rectangular block with a length of 40 mm, a width of 5 mm, and a thickness of 30 μm Experimental mode: Single frequency, constant heating rate
[0518] Experimental method: stretching
[0519] Sample clamping interval length: 15mm
[0520] Determination starting temperature: room temperature ~ 342℃
[0521] Heating rate: 5℃ / min
[0522] Frequency: 10Hz
[0523] Static / dynamic stress ratio: 1.8
[0524] The results of the measurement by the above method showed that the storage elastic modulus of the PI-based resin film formed from the PI-based resin precursor solution 1 at 40°C was 2.3×10 9 Pa, the storage elastic modulus at 300°C is 2.8×10 8 Pa, the storage elastic modulus of the PI-based resin film formed from the PI-based resin precursor solution 2 at 40°C is 2.4×10 9 Pa, the storage elastic modulus at 300°C is 1.1×10 7 Pa, the storage elastic modulus of the PI-based resin film formed from the PI-based resin precursor solution 3 at 40°C is 4.3×10 9 Pa, the storage elastic modulus at 300°C is 3.0×10 8 Pa, the storage elastic modulus of the PI-based resin film formed from the PI-based resin precursor solution 4 at 40°C is 7.5×10 9 Pa, the storage elastic modulus at 300°C is 4.8×10 8 Pa.
[0525] <Measurement of puncture strength>
[0526] The puncture strength of the laminated films 1 to 5 obtained in the examples and comparative examples was measured in an environment of 23°C and 50% relative humidity in accordance with JIS Z 1707 using a small tabletop tester EZ-LX manufactured by Shimadzu Corporation. Specifically, a test piece having a width of 50 mm and a length of 50 mm was used, and a pressure head having a semicircular needle with a diameter of 0.5 mm and a tip shape of Φ2.5 mm was used. The test was carried out under the conditions of a load sensor of 50 N and a test speed of 200 mm / min, and the breakpoint displacement was measured, and the maximum load at this time was taken as the puncture strength. It should be noted that the puncture strength was measured from the layer (PI-2) (TPI layer) side.
[0527] <Determination of the intermediate region and layers (PI-1) to (PI-3) and measurement of their thickness>
[0528] (Preparation of test pieces)
[0529] A portion of each of the laminated films 1 to 5 obtained in the examples and comparative examples was cut and resin-embedded in a manner that a cross section in the thickness direction was visible. Next, a glass knife was installed on an ultrathin slicer (manufactured by Leica, "Leica EMUC7"), and the blade was scanned in a vertical direction with respect to the surface of the laminated film. After reaching the surface of the film embedded in the resin, more than 100 μm was cut along the depth direction of the test piece (the plane direction relative to the laminated film). Then, a SYM knife (manufactured by SHINTECH, "SYM2045 Ultra") was installed, and more than 1 μm was further cut. The cross section obtained by cutting was used as the observation surface, and the obtained test piece (specimen) was set on SPM (manufactured by Bruker; Dimension Icon). It should be noted that the cross section (observation surface) obtained by cutting includes layer (PI-2) (T PI layer), layer (PI-1) (mPI layer) and layer (PI-3) (TPI layer).
[0530] (Obtaining elastic modulus images using SPM)
[0531] The mechanical properties of the sample cross section were evaluated under the following conditions, and the DMT elastic modulus (GPa) was calculated based on the DMT (De rjaguim-Muller-Toporov) theory to obtain a DMT elastic modulus image.
[0532] Specifically, first, the displacement of the piezoelectric scanner and the warping of the cantilever are measured during the contact between the cantilever probe and the sample, and a curve (force curve) showing the relationship between the load F and the sample deformation δ is obtained. At each measurement point, the pullback process of the obtained force curve (the process from the time when the cantilever probe is pressed into the sample to the preset maximum load point until the probe completely leaves the sample surface (such as Figure 3 The DMT modulus of elasticity is obtained by performing an analysis based on the DMT theoretical formula (the process from point C to point D to point E shown in the figure).
[0533] In the analysis, the analysis software (NanoScope Analysis ver.2.00) was used to calculate the DMT elastic modulus by fitting the range of 0.05 to 0.7 when the values of the minimum to maximum values of the F value in the pullback process of the force curve were replaced with values of 0 to 1. The DMT elastic modulus was calculated at 512 points in the horizontal direction and 512 points in the vertical direction within the range of 10 μm × 10 μm of the sample cross section, and a DMT elastic modulus image storing the values was obtained.
[0534] The cantilever used was RTESPA300 (manufactured by Bruker; nominal spring constant: 40 N / m, nominal probe tip radius: 8 nm). The spring constant of the cantilever was calculated using the Sader method (Reference A) built into the SPM device. The probe tip radius of the cantilever was calculated using the reconstruction method (Reference B) built into the SPM device, at a position 2 nm above the tip. The force curve was obtained in Peak Force QNM (Quantitative Nanomechanical Mapping) mode as follows: Figure 4 The measurement sites were set so that the interface shown was located at the center, the layer (PI-2) was located above the center, and the layer (PI-1) was located below the center. The measurement conditions are shown below.
[0535] (Document A) Sader JE, Sanelli JA, Adamson BD, Monty JP, Wei X., Crawford SA, Rev. Sci. Instrum., 2012, Vol. 83, pp. 103705-1 to 103705-16
[0536] (Document B) ISO13095:2014
[0537] Device: Dimension Icon (Bruker)
[0538] Cantilever: RTESPA-300 (Bruker)
[0539] Measurement mode: Peak Force QNM
[0540] Measurement atmosphere: 24°C / atmosphere
[0541] Measurement range: 10 μm × 10 μm (including the layer (PI-2) (TPI layer) and layer (PI-1) (mPI layer) located on the copper foil side)
[0542] Resolution: 512×512pixel (19.53nm / pixel)
[0543] Cantilever moving speed: 0.4μm / s
[0544] Maximum load: 40nN
[0545] Peak Force Frequency: 1kHz
[0546] Peak Force Amplitude: 30nm
[0547] Feedback Gain: Auto
[0548] (Calculation of average elastic modulus of each layer based on SPM)
[0549] The upper left end of the obtained DMT elastic modulus image is (X, Y) = (0, 0), the lower left end is (X, Y) = (0, 511), the upper right end is (X, Y) = (511, 0), and the lower right end is (X, Y) = (511, 511). The average value of the DMT elastic modulus values of 512 × 100 points from (0, 0) to (511, 99) is taken as the average DMT elastic modulus of layer (PI-2) (average elastic modulus measured by SPM). The average of the DMT elastic modulus values of 512 × 100 points from (X, Y) = (0, 412) to (511, 511) is taken as the average DMT elastic modulus of layer (PI-1) (average elastic modulus measured by SPM).
[0550] (Calculation of the thickness of the intermediate region and the thickness of the layer (PI-2))
[0551] In the obtained DMT elastic modulus image, a DMT elastic modulus distribution graph corresponding to Y=0 to 511 is obtained at X=50, 150, 250, 350, and 450, respectively. Specifically, in the DMT elastic modulus image, the DMT elastic modulus at X=50 and Y=0 to 511 [(X, Y)=(50, 0) to (50, 511)] is plotted as the vertical axis and the corresponding Y (Y coordinate) is plotted as the horizontal axis, thereby obtaining a DMT elastic modulus distribution graph at X=50. This DMT elastic modulus distribution graph is also prepared for X=150, 250, 350, and 450.
[0552] Next, for the 5 DMT elastic modulus distribution graphs, the average value of the DMT elastic modulus is calculated separately for each Y value (0 to 511 of the Y coordinate) of each DMT elastic modulus image, and an average DMT elastic modulus distribution graph is made. Furthermore, in the average DMT elastic modulus distribution graph, when n is set to any value from 0 to 511 and Y = n is set, the average value of the DMT elastic modulus at 9 points from n - 4 to n + 4 is obtained as the DMT elastic modulus value when Y = n (4 < n < 508) (a 9-point moving average line of the average DMT elastic modulus distribution graph is made). On this line, the region where the average DMT elastic modulus of layer (PI-1) (average elastic modulus measured by SPM) continuously changes to the average DMT elastic modulus of layer (PI-2) (average elastic modulus measured by SPM) is taken as the intermediate region, and the width of the Y value of this region is taken as the thickness of the intermediate region. At this time, the width of the Y value (pixel) is divided by 19.53 pixel / nm, thereby converting from the pixel unit to the nm unit. In addition, the region from the surface of layer (PI-2) to the interface between layer (PI-2) and the intermediate region is taken as layer (PI-2), and their distance is calculated as the thickness (nm) of layer (PI-2).
[0553] (Calculation of the thickness of layer (PI-1))
[0554] In the laminated films obtained in the examples and comparative examples, the thickness of the intermediate region between layer (PI-3) (another TPI layer) and layer (PI-1) (mPI layer) and the thickness of layer (PI-3) are calculated by the same analysis as above. The thickness of layer (PI-1) (mPI layer) is calculated by subtracting the thicknesses of layer (PI-2), layer (PI-3), and the two intermediate regions from the thickness (total thickness) of the laminated film obtained by the laser microscope above.
[0555] (Calculation of the orientation degree parameter based on laser Raman spectroscopy)
[0556] A portion of each of the laminated films 1 to 5 obtained in the examples and comparative examples was cut and resin-embedded in a manner that a cross section in the thickness direction was visible. Next, a glass knife was installed on an ultrathin slicer (manufactured by Leica, "Leica EMUC7"), and the blade was scanned perpendicular to the surface of the laminated film and along the in-plane direction (TD direction) of the laminated film. After reaching the surface of the film embedded in the resin, more than 100 μm was cut along the depth direction of the test piece. Then, a SYM knife (manufactured by SHINTECH, "SYM2045 Ultra") was installed, and more than 1 μm was further cut. The cross section obtained by cutting was used as the observation surface, and the obtained test piece (sample) was set in a microscopic Raman device (manufactured by JASCO: NRS-5000). It should be noted that the cross section (observation surface) obtained by cutting includes layer (PI-2) (TPI layer), layer (PI-1) (mPI layer) and layer (PI-3) (TPI layer).
[0557] (Device details)
[0558] Device: NRS-5000 (JASCO)
[0559] Excitation wavelength: 785nm
[0560] Objective lens: 100 times
[0561] Grating: L600 / B500nm
[0562] Slit width: 200×1000μm
[0563] Aperture: φ20μm
[0564] Laser intensity: 11.4mW
[0565] Optical attenuator: 100% (open)
[0566] Exposure time: 120 seconds
[0567] Cumulative times: 2 times
[0568] Polarizer: Not used
[0569] Under the above conditions, the 1 / 2 wavelength plate was set at 90°, and the angle of the sample was set so that the vibration direction of the laser polarization light was parallel to the in-plane direction (TD direction) of the sample. The obtained Raman spectrum was smoothed using the 13-point moving average method. Then, fluorescence removal was performed under the following conditions.
[0570] Method: Rolling Ball Algorithm
[0571] Model shape: round
[0572] Circle Radius: 500
[0573] Judgment interval: 10cm -1
[0574] Furthermore, in the obtained Raman spectrum, the 725 cm -1 The intensity of the peak near 1615 cm (attributable to the peak from the CH angle vibration of the aromatic ring) and -1 The intensity of the peak near (attributable to the peak from the stretching vibration of the aromatic ring C=C) was obtained. IP [(1615cm in polarization configuration consistent with the in-plane direction of the laminated film -1 Peak intensity near 725 cm) / (725 cm in a polarization configuration consistent with the in-plane direction of the laminated film -1 It should be noted that the peak intensity is the height of the peak.
[0575] Next, the 1 / 2 wavelength plate was changed to 0°, and the vibration direction of the laser polarization light was set to be parallel to the thickness direction (ND direction) of the sample. The Raman spectrum obtained under this setting was subjected to the same spectrum processing as above to obtain I ND [(1615cm in polarization configuration aligned with the thickness direction of the laminated film -1 Peak intensity near) / (725cm in polarization configuration aligned with the thickness direction of the laminated film -1 The peak intensity near
[0576] The obtained I IP / I ND The value of is taken as the orientation parameter P of the measurement point.
[0577] <P1、P1 C 、Calculation of P2>
[0578] Based on the thickness of the intermediate area and layer (PI-2) obtained by the method described above, the center position of layer (PI-2) is inferred, and the average value of the above-mentioned P obtained at the center of the thickness and three points within ±0.5μm in the thickness direction from the center is taken as P2.
[0579] In addition, based on the intermediate region obtained by the method described above, the position of the end of layer (PI-1) on the layer (PI-2) side (i.e., the interface between layer (PI-1) and the intermediate region) is inferred, and measurements are performed at intervals of 0.5 μm in the range from 1.5 μm to 6.5 μm in the thickness direction starting from the end, and the average value of P at the 11 points obtained is taken as P1.
[0580] Furthermore, based on the thickness of the intermediate region and layer (PI-1) obtained by the method described above, the center position of layer (PI-1) was estimated, and the center of the thickness and the range of ±2.5 μm in the thickness direction from the center were measured at intervals of 0.5 μm, and the average value of P at the obtained 11 points was taken as P1. C .
[0581] From P1 and P1 obtained as described above C The value of (P1 / P2) / (|P1-P2|) and the value of P1c / P1 are obtained from the value of P2.
[0582] <Measurement of Burr Height at Punched Hole Part>
[0583] A 3 cm × 5 cm test piece was cut out from the laminated film obtained in Examples 1 to 3, and the test piece was firmly fixed to a polystyrene foam plate with the layer (PI-2) (TPI layer) facing upward using an adhesive tape. A drill blade with a diameter of 1 mm was attached to a drill bit (GBM 13RE) manufactured by BOSCH Co., Ltd., and the drill was drilled at a rotation speed of 2,600 min. -1 Under the conditions of , a through hole is opened from directly above the laminated film.
[0584] On the layer (PI-2) (TPI layer) side of the laminated film, a through hole opened with a drill was observed under the following conditions using a laser microscope (LEXTOLS4100 manufactured by Olympus Co., Ltd.), and the height of the burr around the through hole (height from the laminated film surface) was determined at 5 locations in each sample, and the average value was calculated. The burr height was measured using the line roughness measurement function of OLS4100.
[0585] The heights of the burrs in Examples 1 to 3 were 204 μm, 174 μm, and 197 μm, respectively.
[0586] Observation magnification: 5 times
[0587] Cut-off: λc: 80μm
[0588] Filter: Gaussian filter
[0589] The results obtained by performing the above measurements are shown in Table 1. In Table 1, the puncture strength is the value when the thickness of the laminated film is converted to 50 μm. It should be noted that in Table 1, PI-1, PI-2 and PI-3 represent layer (PI-1), layer (PI-2) and layer (PI-3), respectively, and layer (I) and layer (II) represent layer (PI-1) and layer (PI-2), respectively.
[0590] [Table 1]
[0591]
[0592] As shown in Table 1, it was confirmed that the laminated films obtained in Examples 1 to 4 had higher puncture strength than the laminated film of Comparative Example 1.
Claims
1. A laminated film comprising a layer (PI-1) containing a polyimide resin and a layer (PI-2) containing a polyimide resin, The thickness of the layer (PI-1) is 10 μm or more, the thickness of the layer (PI-2) is 2 μm or more, The average orientation parameter of each layer obtained by linear analysis of a cross section along the thickness direction of the laminated film using a laser Raman spectrometer satisfies the relationship of formula (I), (P1 / P2) / (|P1-P2|)≥0.70(I) In formula (I), P1 represents the average orientation parameter of the layer (PI-1) within the range of 1.5 μm to 6.5 μm in the thickness direction from the end of the layer (PI-1) on the layer (PI-2) side, and P2 represents the average orientation parameter of the layer (PI-2) within the range of ±0.5 μm in the thickness direction from the center of the layer (PI-2), and the average orientation parameter is obtained by (1615 cm in a polarization configuration consistent with the in-plane direction of the laminated film) -1 Peak intensity near 725 cm / 725 cm in a polarization configuration consistent with the in-plane direction of the laminated film -1 The peak intensity near the layer) / (1615cm in the polarization configuration consistent with the thickness direction of the laminated film -1 Peak intensity near 725 cm / 725 cm in a polarization configuration aligned with the thickness direction of the laminated film -1 The average value of the orientation parameter represented by the peak intensity near .
2. The laminated film according to claim 1, wherein In the formula (I), the P1 is 5.70 or less.
3. The laminated film according to claim 1 or 2, wherein: When the average orientation parameter of the layer (PI-1) within a range of ±2.5 μm in the thickness direction of the laminated film from the center of the layer (PI-1) containing the polyimide resin is defined as P1c, the relationship of formula (II) is satisfied, P1c / P1>0.84(II).
4. The laminated film according to claim 1 or 2, wherein There is an intermediate region between the polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2), The intermediate region is a region where, when the elastic modulus of a cross section in the thickness direction of the laminated film is continuously measured along the thickness direction using a scanning probe microscope, the elastic modulus continuously changes from the average elastic modulus (1) of the layer (PI-1) to the average elastic modulus (2) of the layer (PI-2), The thickness of the intermediate region is greater than 50 nm.
5. The laminated film according to claim 1 or 2, wherein The thickness of the polyimide resin-containing layer (PI-2) is 0.05 to 0.3 times the thickness of the polyimide resin-containing layer (PI-1). The laminated film according to claim 1 or 2, further comprising a layer (PI-3) containing a polyimide resin.
7. The laminated film according to claim 1 or 2, wherein: At least one of the polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2) comprises a polyimide resin having a structural unit (A) derived from a tetracarboxylic anhydride, The structural unit (A) includes a structural unit (A1) derived from a tetracarboxylic anhydride represented by the formula (A1) and / or a structural unit (A2) derived from a tetracarboxylic anhydride represented by the formula (A2). In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, k represents an integer from 0 to 2, In formula (A2), R a2 Each of them independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom, and each of them independently represents an integer of 0 to 3.
8. The laminated film according to claim 1 or 2, wherein At least one of the polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2) comprises a polyimide resin having a structural unit (B) derived from a diamine, The structural unit (B) comprises a structural unit (B1) derived from a diamine represented by formula (B1), In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, W independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the divalent linking group), R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted by a halogen atom, m represents an integer from 1 to 4, q represents an integer of 0 to 4 independently of each other.
9. The laminated film according to claim 1 or 2, wherein: The polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2) include a polyimide resin having a structural unit (A) derived from a tetracarboxylic anhydride and a structural unit (B) derived from a diamine, The structural unit (A) includes a structural unit (A1) derived from a tetracarboxylic anhydride represented by the formula (A1) and / or a structural unit (A2) derived from a tetracarboxylic anhydride represented by the formula (A2). The structural unit (B) comprises a structural unit (B1) derived from a diamine represented by formula (B1), In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, k represents an integer from 0 to 2, In formula (A2), R a2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, and each independently represents an integer of 0 to 3, In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, W independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the divalent linking group), R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted by a halogen atom, m represents an integer from 1 to 4, q represents an integer of 0 to 4 independently of each other.
10. The laminated film according to claim 1 or 2, wherein: The polyimide resin contained in the polyimide resin-containing layer (PI-1) and the polyimide resin contained in the polyimide resin-containing layer (PI-2) are different resins.
11. The laminated film according to claim 1 or 2, wherein The polyimide resin-containing layer (PI-1) and the polyimide resin-containing layer (PI-2) each contain a polyimide resin having at least two types of structural units (A) derived from tetracarboxylic anhydride.
12. The laminated film according to claim 1 or 2, wherein: At least the polyimide resin-containing layer (PI-1) contains a polyimide resin having a structural unit (A) derived from tetracarboxylic anhydride, The structural unit (A) comprises a structural unit (A3) derived from a tetracarboxylic anhydride having an ester bond represented by the formula (A3), In formula (A3), Z represents a divalent organic group, R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, s represents an integer of 0 to 3 independently of each other.
13. The laminated film according to claim 9, wherein At least the polyimide resin-containing layer (PI-1) comprises a polyimide resin having a structural unit (A) derived from a tetracarboxylic anhydride, wherein the structural unit (A) further comprises a structural unit (A3) derived from an ester bond-containing tetracarboxylic anhydride represented by the formula (A3) in an amount of 45 mol% or less based on the total amount of the structural unit (A), In formula (A3), Z represents a divalent organic group, R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group or an aryloxy group which may have a halogen atom, s represents an integer of 0 to 3 independently of each other. 14 . A laminated sheet comprising a metal layer on one or both sides of the laminated film according to claim 1 or 2.
15. A flexible printed circuit substrate comprising the laminated sheet according to claim 14.