Confined-range driven patterned chiral assembly and preparation method and application thereof
The assembly method of two-dimensional bubble arrays generated by template confinement and specific assembly inks solves the problem of difficult patterning of traditional interface assembly and achieves efficient and orderly preparation of chiral assemblies, which is suitable for a variety of optoelectronic devices.
Patent Information
- Application Number
- CN202410795438.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional interfacial assembly methods are difficult to achieve patterned chiral assembly, and the competition between interfacial chiral assembly and bulk achiral assembly limits the preparation efficiency, making it difficult to be compatible with patterning and kinetic optimization.
The two-dimensional bubble array generated through template confinement provides a confined gas-liquid interface, inducing interfacial adsorption and orderly assembly of amphiphilic chiral assembly molecules, forming patterned chiral assemblies with high asymmetry factors, and utilizing functional stacking groups. The groups are connected to chiral groups, combined with specific assembly inks and template designs, to achieve rapid foaming and orderly assembly.
It achieves a chiral assembly structure with a high asymmetry factor, improves the patterning characteristics and preparation efficiency of the assembly, and is suitable for electron spin filters, circularly polarized photodetectors and circularly polarized light-emitting devices.
Smart Images

Figure CN118723915A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of chiral optoelectronic devices and their preparation, and specifically, relates to a confined-drive patterned chiral assembly and a preparation method and application thereof. Background Art
[0002] Chiral characteristics break the structural symmetry of functional materials and have broad application prospects in the field of spin optoelectronic devices, such as spin light-emitting devices, spin optoelectronic logic devices and memory devices. In the preparation of chiral structures, traditional inorganic material systems obtain chiral characteristics through photolithography or electron beam etching, and the process is cumbersome and complicated. In addition, traditional inorganic materials often only have passive optical properties, and face the problem of lattice mismatch during the processing of integrating active layers, which poses a challenge to the preparation of spin optoelectronic devices. Unlike inorganic materials, organic functional molecules can introduce chiral characteristics at the molecular level through reasonable molecular design. During the assembly process, chiral characteristics are transmitted across spatial scales through intermolecular interactions, and finally form a multi-level chiral assembly structure. By introducing suitable functional molecular fragments, the assembly can have various optoelectronic properties. At the same time, organic molecules are compatible with solution processing technology, which is low-cost and simple.
[0003] In the design of chiral assembly strategies, the most important consideration is how to make the assembly have a high chiral asymmetry factor. The fluid / fluid interface assembly strategy is considered to be an excellent chiral assembly method. Molecules are aligned on the interface driven by amphiphilic compounds, which is conducive to the orderly assembly process driven by intermolecular interactions. At the same time, the two-dimensional interface provides a confined assembly environment with symmetry breaking for the assembly, which is conducive to the cross-level transmission of chirality during the assembly process.
[0004] However, conventional interfacial assembly methods are difficult to adapt to patterning, and the assembly morphology is often disordered fibers, which limits the application of interfacial assembly methods in the actual industrial manufacturing of chiral device arrays. In addition, the competition between interfacial chiral assembly and bulk achiral assembly also limits the preparation efficiency of interfacial assembly methods. Therefore, how to be compatible with patterning and make the interfacial chiral assembly pathway kinetically dominant is a key issue in the preparation of chiral functional device arrays. Summary of the invention
[0005] In order to improve the above technical problems, the present invention provides a method for preparing a patterned chiral assembly with a high asymmetry factor formed by assembling amphiphilic chiral assembly molecules under confinement driving, a chiral assembly based on the method and its application. Specifically, the present invention provides the following technical solutions:
[0006] A method for preparing a chiral assembly, the method is based on a two-dimensional bubble array generated by template restriction, the two-dimensional bubble array provides a confined gas-liquid interface, induces amphiphilic chiral assembly molecules to undergo interfacial adsorption, and then, under the induction of evaporation, the amphiphilic chiral assembly molecules undergo orderly interfacial assembly to form a chiral assembly;
[0007] The amphiphilic chiral assembly molecule comprises a chiral group and a functional stacking group, wherein one functional stacking group connects 1 to 4 chiral groups; corresponding to the connection of 1, 2, 3 or 4 chiral groups, the amphiphilic chiral assembly molecule exhibits C1 symmetry, C2 symmetry, C3 symmetry or C4 symmetry respectively.
[0008] According to an embodiment of the present invention, the molecular configuration of the amphiphilic chiral assembly molecule is as follows Figure 1 shown.
[0009] According to an embodiment of the present invention, when one functional stacking group is connected to at least two chiral groups, the chiral groups are the same or different.
[0010] In the present invention, the amphiphilic chiral assembly molecule is amphiphilic, the chiral group is hydrophilic and the functional stacking group is hydrophobic, or the chiral group is hydrophobic and the functional stacking group is hydrophilic.
[0011] According to an embodiment of the present invention, the functional stacking group is selected from a conjugated group; illustratively, the conjugated group includes but is not limited to one of a perylenyl group, a pyrene group, a phenanthrenyl group, anthracene group, a polyphenylvinyl group (e.g., a tetraphenylvinyl group), an azophenyl group, a porphyrinyl group or related derivatives.
[0012] According to an embodiment of the present invention, the chiral group is selected from alanine, valine, leucine, isoleucine, methionine, phenylalanine, tryptophan, proline, serine, threonine, asparagine, glutamine, tyrosine, cysteine, aspartic acid, glutamic acid, lysine, arginine, histidine, glucose, fructose, galactose, mannose, ribose, deoxyribose and an alkyl chain with a chiral center (e.g., 2,6-dimethyloctane), etc.
[0013] In the present invention, the two-dimensional bubble array contains a plurality of micrometer-sized bubbles, and the micrometer-sized bubbles provide abundant confined gas-liquid interfaces.
[0014] According to an embodiment of the present invention, the two-dimensional bubble array is produced by depositing a metal catalyst or a borohydride catalyst on a template and causing a chemical reaction after the catalyst is brought into contact with an assembly ink containing a foaming agent and the amphiphilic chiral assembly molecules on a substrate.
[0015] According to an embodiment of the present invention, the template surface has a patterned structure. Further, the template surface has a patterned structure, and the metal catalyst or borohydride catalyst is deposited on the template.
[0016] According to the embodiment of the present invention, under the restriction of the patterned structure on the template, the bubbles rapidly develop into micrometer-scale two-dimensional bubbles of uniform size, and drive the solution to be pinned in the patterned structure to form a liquid bridge network.
[0017] According to an embodiment of the present invention, the assembly ink comprises the following components: amphiphilic chiral assembly molecules, a foaming agent and water. Preferably, an acidic compound, a basic compound or an organic solvent miscible with water may also be added to the assembly ink, and its function is to provide a suitable solvent environment for promoting the dissolution of the amphiphilic chiral assembly molecules. The basic compound includes but is not limited to sodium hydroxide, potassium hydroxide and ammonia water, the acidic compound includes but is not limited to hydrochloric acid, sulfuric acid and glacial acetic acid, and the organic solvent includes but is not limited to tetrahydrofuran, 1,4-dioxane and dimethyl sulfoxide.
[0018] According to an embodiment of the present invention, in the assembly ink, the foaming agent is selected from:
[0019] a1) hydrogen ions, wherein the hydrogen ion concentration ranges from 0.0001 to 0.5 mol / L, preferably from 0.01 to 0.1 mol / L; the hydrogen ions are derived from, for example, hydrogen ions in hydrochloric acid;
[0020] a2) peroxide, the peroxide is selected from hydrogen peroxide, urea peroxide and peracetic acid, etc. The volume of the peroxide is 1-7% by volume of the alkaline compound solution of the assembled molecules, preferably 5% by volume.
[0021] According to an embodiment of the present invention, in the assembly ink, the amphiphilic chiral assembly molecules are first dissolved in an alkaline compound solution; specifically, the concentration of the amphiphilic chiral assembly molecules in the alkaline compound solution is 10-200 mg / mL, preferably 30-100 mg / mL.
[0022] According to an embodiment of the present invention, the metal catalyst or borohydride catalyst required for the foaming reaction deposited on the template is selected from:
[0023] b1) borohydrides, such as sodium borohydride, potassium borohydride and calcium borohydride;
[0024] The borohydride is deposited on the template by drop casting of an ethanol solution; the concentration of the borohydride ethanol solution is in the range of 0.001 to 0.01 wt %, preferably 0.0025 wt %;
[0025] b2) Metal catalysts, such as silver, platinum, palladium and gold, etc.; deposited by vacuum evaporation or magnetron sputtering, with a thickness ranging from 1 to 50 nanometers, preferably 3 to 20 nanometers.
[0026] According to the embodiments of the present invention, the materials of the template and / or substrate include but are not limited to: common hard substrates such as glass, silicon wafers, silicon dioxide wafers, quartz, metals, polysiloxanes, polyolefins, polyamides, natural rubber and synthetic rubber.
[0027] According to an embodiment of the present invention, the preparation method specifically comprises the following steps:
[0028] (1) preparing an assembly ink; preparing a substrate with suitable hydrophilicity and a flat surface; preparing a template with suitable hydrophilicity and a patterned surface structure, and depositing a metal catalyst or a borohydride catalyst required for a foaming reaction on the template;
[0029] Wherein, the assembly ink comprises the following components: the amphiphilic chiral assembly molecules, a foaming agent and water;
[0030] (2) dropping the assembly ink onto the substrate and combining it with the template to form a sandwich structure assembly system, foaming and assembling the system, so that the amphiphilic chiral assembly molecules can self-assemble to obtain a chiral assembly.
[0031] According to an embodiment of the present invention, in step (1), the preparation of a template with suitable hydrophilicity and hydrophobicity and a patterned structure on the surface specifically includes but is not limited to one or more of the following technologies: photolithography technology, etching technology, imprinting technology, replica technology, 3D printing technology; preferably, a combination of photolithography technology and etching technology.
[0032] According to an embodiment of the present invention, the patterned structure of the template in step (1) can be a geometric pattern of any densely packed structure, or a circuit or optical path structure of a specific design; the densely packed geometric pattern is preferably a hexagon, a triangle or a quadrilateral; the side length of the densely packed geometric pattern is preferably 10 to 1000 microns.
[0033] Preferably, in step (1), the template with suitable hydrophilicity and hydrophobicity and a patterned structure on the surface is prepared by combining photolithography and etching technology. Preferably, the template is a silicon micro-column template with a hexagonal pattern, preferably, the diameter of the silicon micro-column template is 10 μm, the height is 20 μm, the column spacing is 20 μm, and the hexagon side length is 60 μm.
[0034] According to an embodiment of the present invention, in step (1), preparing a substrate with suitable hydrophilicity and hydrophobicity and a smooth surface specifically comprises:
[0035] Perfluorooctane sulfonic acid is coated on the surface of a quartz substrate, heated at 70-90°C for a certain period of time, and subjected to plasma treatment, so that the contact angle of the surface of the substrate with suitable hydrophilicity and flat surface is 10-90 degrees, for example, 40-60 degrees. For example, perfluorooctane sulfonic acid is coated on the surface of a quartz substrate, heated at 80°C for 3h, and subjected to plasma treatment, so that the contact angle of the surface of the substrate with suitable hydrophilicity and flat surface is 50 degrees.
[0036] According to an embodiment of the present invention, step (1) further includes regulating the wettability of the template and / or substrate, and the regulating methods include but are not limited to plasma cleaning, special solution treatment, group modification or ultraviolet radiation treatment; wherein the contact angle of the template ranges from 10 to 40 degrees, preferably 20 degrees; the contact angle of the substrate ranges from 10 to 90 degrees, preferably 40 to 60 degrees.
[0037] According to an embodiment of the present invention, the assembly process in step (2) is controlled by temperature and humidity: the temperature control range is 18-60°C, preferably 25-40°C; the humidity control range is RH 10-60%, preferably RH 10-40%, and preferably not more than 20%. A suitable drying environment is very important for depositing ordered chiral assemblies.
[0038] The present invention also provides a chiral assembly, which is an amphiphilic chiral assembly molecule assembly, which has a patterned structure and is asymmetric; the assembly ink forming the chiral assembly includes the following components: amphiphilic chiral assembly molecules, a foaming agent and water.
[0039] Preferably, the assembly is prepared by the above method.
[0040] The present invention also provides the application of the chiral assembly in an electron spin filter, a circularly polarized photodetector and a circularly polarized light emitting device.
[0041] Beneficial effects of the present invention:
[0042] The present invention provides a method for preparing a chiral assembly, wherein the method uses a multi-dimensional interlaced and interconnected confined gas-liquid interface formed by rapid foaming to provide a kinetic advantage for the interface chiral assembly behavior and patterning of amphiphilic chiral assembly molecules, so that they occupy a dominant position in the competition with bulk non-chiral assembly, thereby obtaining a chiral assembly structure with a high asymmetry factor. In addition, the present invention obtains a specific bubble pattern by designing a template pattern, thereby further obtaining a specific assembly pattern. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a molecular configuration diagram of the assembly of the present invention.
[0044] Figure 2 This is a microscopic picture of the chiral assembly of Example 1.
[0045] Figure 3 It is the CD spectra of different components in Example 1 and Comparative Examples 1-3.
[0046] Figure 4 This is the IV curve of Example 1 tested using a magnetic permeability microscope.
[0047] Figure 5 It is a schematic diagram of the assembly of a chiral assembly. DETAILED DESCRIPTION
[0048] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0049] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0050] Example 1
[0051] a. Preparation and assembly of ink
[0052] The amphiphilic chiral molecule azo-glu obtained by coupling azobenzene and glutamic acid was dissolved in a NaOH solution at a concentration of 50 mg / mL, and ultrasonic and heated to accelerate the dissolution (ultrasound: 200 mW, 15 min; heating: 60°C for 15 min). The foaming agent H 2 O 2 (10wt%), wherein the volume of the foaming agent is 5v% of the mixed liquid.
[0053] b. Treat the substrate: coat the surface of the quartz substrate with perfluorooctane trimethoxysilane, heat it at 80° C. for 3 h, and perform plasma treatment on it to obtain a substrate with suitable hydrophilicity and flat surface, and its surface contact angle is 50 degrees.
[0054] c. Processing the template, the patterned structure of the template is prepared by combining photolithography and etching technology. The template is a silicon micro-pillar template with a hexagonal pattern, the diameter of the silicon micro-pillar template is 10 μm, the height is 20 μm, the column spacing is 20 μm, and the hexagon side length is 60 μm. A 5 nm Pt film is deposited on the surface by thermal evaporation.
[0055] d. Assembly
[0056] 2 μL of the assembly ink was dropped onto a quartz substrate, and then the microcolumn template was placed on the substrate. Under the catalysis of the Pt film, H 2 O 2 The decomposition of 20% MgO rapidly generates oxygen. The entire assembly process is carried out in the dark. To control the temperature, the assembly is carried out on a hot stage. The typical assembly temperature is 25°C. To control the humidity to less than RH 20%, conventional assembly is carried out in an electronic drying room.
[0057] Figure 2 This is a microscopic picture of the chiral assembly of Example 1.
[0058] Comparative Example 1
[0059] The difference between Comparative Example 1 and Example 1 is that no foaming agent H is added in step a. 2 O 2 , compared with Example 1, the rate of formation of the gas-liquid interface and the liquid bridge confined space is smaller.
[0060] Comparative Example 2
[0061] The difference between Comparative Example 2 and Example 1 is that in step d, a quartz slide smaller than the substrate (i.e., no catalyst is deposited on the slide) is used instead of the template. Compared with Example 1 and Comparative Example 1, no one-dimensional liquid bridge confined space is formed, only a two-dimensional capillary plate confined space is formed.
[0062] Comparative Example 3
[0063] The difference between Comparative Example 3 and Example 1 is that the template in step b is not added.
[0064] Figure 3 is the circular dichroism spectra (CD) of different components in Example 1 and Comparative Examples 1-3; wherein Bubble represents Example 1, No Bubble represents Comparative Example 1, Plate represents Comparative Example 2, and Droplet represents Comparative Example 3. Figure 3 It can be seen that the bubble assembly of Example 1 gives a strong dual-signal CD band, which represents the spiral stacking of adjacent azobenzenes and the Davydov splitting of excitons. The droplet assembly of Comparative Example 3 only shows a weak normal CD band of azobenzene at 385nm. The CD spectra of the bubble-free assembly of Comparative Example 1 and the plate assembly of Comparative Example 2 show a mixture of the above CD spectra, wherein the CD spectrum of the bubble-free assembly of Comparative Example 1 is close to the bubble assembly of Example 1, while the CD spectrum of the plate assembly of Comparative Example 2 is more similar to the droplet assembly of Comparative Example 3. In the assembly conditions of different confinement conditions, Example 1 has a significantly larger absorption asymmetry factor, which proves the application of the bubble method of the present invention in the patterned preparation of high asymmetry factor chiral structures.
[0065] Figure 4The IV curve of the assembly tested by the magnetic permeability microscope in Example 1 shows that after applying magnetic fields of different directions to the assembly, the magnetic needle tip will generate electron injections with different spin polarization directions. It can be found that under different magnetic fields, the same voltage will correspond to different currents, which means that the chiral molecules have a filtering effect in the transport of electrons with different spin directions. Therefore, the method of the present invention has an application scenario in the patterned preparation of spin electronics devices.
[0066] Example 2
[0067] The difference between Example 2 and Example 1 is that the amphiphilic chiral molecule in Example 2 is TPE-His obtained by coupling tetraphenylethylene and histidine.
[0068] Comparative Example 4
[0069] The difference between Comparative Example 4 and Example 2 is that no foaming agent H is added in step a. 2 O 2 , compared with Example 2, the rate of formation of the gas-liquid interface and the liquid bridge confined space is smaller.
[0070] Comparative Example 5
[0071] The difference between Comparative Example 5 and Example 2 is that in step b, a quartz slide smaller than the substrate is used instead of the template. Compared with Example 2 and Comparative Example 4, no one-dimensional liquid bridge confined space is formed, and only a two-dimensional capillary plate confined space is formed.
[0072] Comparative Example 6
[0073] The difference between Comparative Example 6 and Example 2 is that the template in step b is not added.
[0074] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a chiral assembly, characterized in that: The method is based on a two-dimensional bubble array generated by template restriction, wherein the two-dimensional bubble array provides a confined gas-liquid interface to induce the amphiphilic chiral assembly molecules to undergo interfacial adsorption, and then, under the induction of evaporation, the amphiphilic chiral assembly molecules undergo orderly interfacial assembly to form a chiral assembly; The amphiphilic chiral assembly molecule comprises a chiral group and a functional stacking group, wherein one functional stacking group connects 1 to 4 chiral groups; corresponding to the connection of 1, 2, 3 or 4 chiral groups, the amphiphilic chiral assembly molecule exhibits C1 symmetry, C2 symmetry, C3 symmetry or C4 symmetry respectively.
2. The method according to claim 1, characterized in that When a functional stacking group is connected to at least two chiral groups, the chiral groups are the same or different. Preferably, the functional stacking group is selected from a conjugated group; illustratively, the conjugated group is selected from one of a perylene group, a pyrene group, a phenanthryl group, anthracene group, a polyphenylvinyl group, an azophenyl group, a porphyrin group or related derivatives.
3. The method according to claim 1 or 2, characterized in that: The chiral group is selected from alanine, valine, leucine, isoleucine, methionine, phenylalanine, tryptophan, proline, serine, threonine, asparagine, glutamine, tyrosine, cysteine, aspartic acid, glutamic acid, lysine, arginine, histidine, glucose, fructose, galactose, mannose, ribose, deoxyribose and an alkyl chain with a chiral center (e.g., 2,6-dimethyloctane).
4. The method according to any one of claims 1 to 3, characterized in that: The two-dimensional bubble array is produced by depositing a metal catalyst or a borohydride catalyst on a template and causing a chemical reaction after the catalyst is in contact with an assembly ink containing a foaming agent and the amphiphilic chiral assembly molecules on a substrate. Preferably, the assembly ink comprises the following components: amphiphilic chiral assembly molecules, a foaming agent and water.
5. The method according to claim 4, characterized in that In the assembly ink, the foaming agent is selected from: a1) hydrogen ions, wherein the hydrogen ion concentration ranges from 0.0001 to 0.5 mol / L; the hydrogen ions are derived from hydrogen ions in hydrochloric acid; a2) peroxide, the peroxide is selected from hydrogen peroxide, urea peroxide or peracetic acid, and the volume of the peroxide is 1-7v% of the volume of the alkaline compound solution of the assembled molecules.
6. The method according to claim 4, characterized in that The metal catalyst or borohydride catalyst required for the foaming reaction deposited on the template is selected from: b1) borohydrides, for example sodium borohydride, potassium borohydride or calcium borohydride; The borohydride is deposited on the template by drop casting of an ethanol solution; the concentration of the borohydride ethanol solution ranges from 0.001 to 0.01 wt %; b2) Metal catalysts, such as silver, platinum, palladium or gold; deposited by vacuum evaporation or magnetron sputtering, with a thickness ranging from 1 to 50 nanometers.
7. The method according to any one of claims 1 to 6, characterized in that: The method specifically comprises the following steps: (1) preparing an assembly ink; preparing a substrate with suitable hydrophilicity and a flat surface; preparing a template with suitable hydrophilicity and a patterned surface structure, and depositing a metal catalyst or a borohydride catalyst required for a foaming reaction on the template; Wherein, the assembly ink comprises the following components: the amphiphilic chiral assembly molecules, a foaming agent and water; (2) dropping the assembly ink onto the substrate and combining it with the template to form a sandwich structure assembly system, foaming and assembling the system, so that the amphiphilic chiral assembly molecules can self-assemble to obtain a chiral assembly.
8. The method according to claim 7, characterized in that The assembly process in step (2) is controlled by temperature and humidity: the temperature control range is 18-60° C.; the humidity control range is RH 10-60%.
9. A chiral assembly, characterized in that: The invention relates to an amphiphilic chiral assembly molecule assembly, which has a patterned structure and is asymmetric; the assembly ink forming the chiral assembly comprises the following components: amphiphilic chiral assembly molecules, a foaming agent and water. Preferably, the assembly is prepared by the method according to any one of claims 1 to 8.
10. Use of the chiral assembly according to claim 9 in an electron spin filter, a circularly polarized photodetector or a circularly polarized light emitting device.
Citation Information
Cited By
Gold nano-catalyst with two-dimensional ordered self-assembly structure as well as preparation method and application of gold nano-catalyst
CN122538812A