Single-particle multi-phase component spherical ceramic powder for network communication and preparation method thereof

By adopting the chemical composite synthesis method of spherical ceramic powders with single-particle complex phase components in the field of network communication, the problem of mechanical performance reduction caused by poor powder matching and oil absorption characteristics is solved, and high-efficiency and low-cost thermally conductive ceramic powders are achieved. Production improves the mechanical properties and production efficiency of composite ceramic powders.

CN118724567BActive Publication Date: 2024-11-22SHANDONG RES & DESIGN ACADEMY OF IND CERAMICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411230882.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The thermally conductive filler powder in the existing network communication field is reduced due to poor powder matching and different oil absorption characteristics during the composite process. The composite ceramic powder is difficult, high production cost and low efficiency, and is prepared by physical and mechanical mixing method. The body has a problem of weakening performance during use.

Method used

Alumina/nitriding is formed by chemical complex synthesis method of spherical ceramic powders with single-particle complex phase components using raw materials such as soluble aluminum-based ionic salts, long-chain alkyl surfactants, reaction aids and nitrogen-based conversion agents. The aluminum composite ceramic powder avoids the influence of poor powder matching and oil absorption characteristics, and simplifies the compounding process.

Benefits of technology

It realizes low-cost and efficient production of high-thermal conductivity ceramic powder, avoids weakening of the intrinsic properties of the powder, improves the mechanical properties and production efficiency of composite ceramic powder, and meets the requirements of downstream high thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724567B_ABST
    Figure CN118724567B_ABST
Patent Text Reader

Abstract

The present invention provides a single-particle multi-phase component spherical ceramic powder for network communication and a preparation method, which belongs to the field of network communication ceramics. The single-particle multi-phase component spherical ceramic powder for network communication is prepared using the following raw materials: soluble aluminum-based ion salt, long-chain alkyl surfactant, reaction aid, nitrogen-based conversion agent, water; the nitrogen-based conversion agent is at least one of the following: 1,14-diazide-3,6,9,12-tetraoxa-tetradecane, nitrilotriacetic acid. The single-particle multi-phase component spherical ceramic powder for network communication of the present invention and the preparation method effectively overcome the problem that many factors need to be considered in the composite production of different powders to meet the downstream high thermal conductivity requirements, and the difficulty of compounding is large; it can effectively reduce the difficulty of compounding, improve production efficiency, reduce production costs, and avoid the problem of weakening the intrinsic properties of different powders in compounding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of network communication ceramics, and in particular to a single-particle multi-phase component spherical ceramic powder for network communication and a preparation method thereof. Background Art

[0002] In the prior art, the network communication field requires that the thermal conductivity of thermally conductive filler powders must reach 8W / (m·K) or above. Existing oxide / nitride composite ceramic powders used as thermally conductive filler powders are all made of two or more powders such as oxide powders and nitride powders as raw materials, and are made by simple physical and mechanical mixing; the composite ceramic powders have the problem of poor matching of different powders during subsequent use, which is mainly reflected in that after two or more powders are mixed, the thermal conductivity of the composite ceramic powder will be reflected through the composite of different types of powders, but at the same time, the intrinsic characteristics of each raw material powder are still reflected, so the expansion coefficient, hardness, dielectric properties, oil absorption value and powder appearance state of different powders are different, which directly affects the subsequent use performance of the composite ceramic powder, and during use, it can often only meet a certain performance requirement and weaken other performance.

[0003] Furthermore, during the subsequent use of the composite ceramic powder prepared by the aforementioned physical and mechanical mixing, the mechanical properties of the back-end product (composite ceramic powder thermal conductive material) will be adversely affected due to the different oil absorption characteristics of different powders in the composite ceramic powder. For example, nitride powder has the characteristics of high oil absorption value, high surface roughness, and high porosity. In order to prepare high thermal conductivity composite ceramic powder, it is necessary to increase the amount of nitride powder added; on the premise of ensuring sufficient addition of nitride powder, the high oil absorption value of nitride powder will cause the back-end product (composite ceramic powder thermal conductive material) to have mechanical weak points or stress concentration points, which will lead to reduced mechanical properties of the back-end product, and its comprehensive performance is difficult to be effectively guaranteed. In addition, the different oil absorption characteristics of different powders also lead to different addition ratios of thermal conductive glue that needs to be added.

[0004] At the same time, the existing preparation method of thermal conductive filler powder is to use nitride powders such as aluminum nitride, composite alumina powder and other powder raw materials, set different powder addition ratios and different particle gradings of powders according to the requirements of thermal conductivity, and then perform physical and mechanical compounding; and the composite powder needs to be subjected to specific homogenization treatment during the compounding process. However, in order to meet the downstream high thermal conductivity requirements, there are many factors to consider in the composite production of different powders, and the compounding is difficult; there are problems such as high production cost, low production efficiency, and weakening of the intrinsic properties of different powders. For example, the production of thermal conductive powder fillers using spherical alumina powder and aluminum nitride powder as raw materials requires the downstream thermal conductivity requirements, according to the difference in the intrinsic characteristics of the two powders, and comprehensively considers the density, particle size, hardness, oil absorption value, expansion coefficient, dielectric properties and other factors of the two powders. After multiple mechanical mixing and homogenization tests in advance, large-scale production can be carried out; its compounding is difficult, the production efficiency is low, the production cost is high, and there is a problem of weakening the intrinsic properties of different powders. Summary of the invention

[0005] In order to solve the technical problems existing in the prior art, the present invention provides a single-particle multi-phase component spherical ceramic powder for network communication and a preparation method, which effectively overcomes the problem that many factors need to be considered in the composite production of different powders to meet the downstream high thermal conductivity requirements and the difficulty of compounding; it can effectively reduce the difficulty of compounding, improve production efficiency, reduce production costs, and avoid the problem of weakening the intrinsic properties of different powders in compounding; and effectively solves the problem that in the subsequent use of the existing composite ceramic powder prepared by physical and mechanical mixing, the different oil absorption characteristics of different powders in the composite ceramic powder have different effects on the mechanical properties of the back-end products.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a single-particle multi-phase component spherical ceramic powder for network communication, which is prepared by using the following raw materials: soluble aluminum-based ion salt, long-chain alkyl surfactant, reaction aid, nitrogen-based conversion agent, and water;

[0008] The soluble aluminum-based ion salt is at least one of the following: aluminum chloride, aluminum sulfate, and aluminum acetate;

[0009] The long-chain alkyl surfactant is at least one of the following: octadecyl trimethyl ammonium bromide, octadecyl dimethyl tertiary amine, octadecyl methyl dihydroxyethyl ammonium bromide;

[0010] The reaction aid is at least one of the following: ammonium oxalate, ammonium acetate, ammonium formate, ammonium citrate, and ammonium phosphate;

[0011] The nitrogen-based conversion agent is at least one of the following: 1,14-diazide-3,6,9,12-tetraoxatetradecane, nitrilotriacetic acid;

[0012] The water, without particular limitation, may be tap water or deionized water;

[0013] The method for preparing the single-particle multi-phase component spherical ceramic powder for network communication comprises the following steps:

[0014] Step S001, adding a long-chain alkyl surfactant into water, stirring evenly at a temperature of 60-85° C. to obtain a white foamy solution, and keeping it at 60-85° C. to obtain a transparent spherical micelle solution;

[0015] Step S002, adding a soluble aluminum-based ion salt to the transparent spherical micelle solution, stirring at a stirring speed of 300-800 r / min at room temperature, and then standing to obtain a white sol;

[0016] Step S003, adding a reaction aid to the white sol, mixing and stirring at room temperature for 0.5 h or more, to obtain a milky white high-viscosity sol;

[0017] Step S004, taking out 30-50% by weight of the milky white high-viscosity sol, adding a nitrogen-based conversion agent, and reacting in a sealed manner under a negative pressure environment at a temperature of 60-90° C. to obtain a white precipitation solution;

[0018] Step S005, mixing the remaining milky white high-viscosity sol of step S003 and the white precipitation solution of step S004 evenly, and spray drying to obtain white spherical powder;

[0019] Step S006, calcining the white spherical powder in an inert gas protective atmosphere to obtain a single-particle multi-phase component spherical ceramic powder for network communication.

[0020] Furthermore, the aluminum chloride salt is at least one of the following: crystalline aluminum chloride, polyaluminum chloride; the aluminum sulfate salt is at least one of the following: aluminum sulfate, hydrated aluminum sulfate, basic aluminum sulfate; the aluminum acetate salt is basic aluminum acetate. The soluble aluminum-based ion salt can effectively achieve ionic bonding during the reaction and spheroidization agglomeration process to form a single particle structure composite phase component.

[0021] The long-chain alkyl surfactant can form spherical micelles in water, and the polar bonds formed by it are long-chain structures, which effectively promote the multi-layer long-chain enrichment of aluminum ions, and further realize the multi-component composite of single spherical particle oxide-nitride. After the reaction aid is dissolved in water, under the action of ion reaction, the ammonium ions react with the aluminum ions and the negative ions to form Al-OH-NH bonds, effectively forming a precursor of spherical aluminum oxide.

[0022] Preferably, the mass ratio of the soluble aluminum-based ion salt to water is 15-35:65-85;

[0023] The dosage of the long-chain alkyl surfactant is 0.1-0.5% of the mass of the soluble aluminum-based ion salt;

[0024] The dosage of the reaction aid is 0.02-0.05% of the mass of the soluble aluminum-based ion salt;

[0025] The mass ratio of the nitrogen-based conversion agent to the soluble aluminum-based ion salt is 1:1.

[0026] Preferably, in the soluble aluminum-based ion salt, the mass ratio of aluminum chloride salt, aluminum sulfate salt and aluminum acetate salt is 2:2:1.

[0027] Furthermore, the preparation method of the single-particle multi-phase component spherical ceramic powder for network communication is specifically as follows:

[0028] Step S001, adding a long-chain alkyl surfactant into water, stirring at a high speed of 1000 r / min or more for 0.5 h or more at a temperature of 60-85° C. to obtain a white foamy solution, and keeping the solution at 60-85° C. for 2 h or more to obtain a transparent spherical micelle solution with a micelle size of 10-30 nm;

[0029] Step S002, adding a soluble aluminum-based ion salt to the transparent spherical micelle solution, stirring at room temperature for 0.5 h or more at a stirring speed of 300-800 r / min, and standing for 1 h or more to obtain a white sol;

[0030] Step S003, adding a reaction aid to the white sol, mixing and stirring at room temperature for 0.5 h or more at a speed of 80-150 r / min, to obtain a milky white high-viscosity sol with a viscosity of 8000-13000 mPa·s;

[0031] Step S004, taking out 30-50% by weight of the milky white high-viscosity sol, adding a nitrogen-based conversion agent, and reacting in a sealed state for 2 hours or more at a temperature of 60-90° C. under a negative pressure of -0.1 MPa to obtain a white precipitate solution;

[0032] Step S005, mixing the remaining milky white high-viscosity sol of step S003 with the white precipitation solution of step S004, stirring for 3 hours or more at a rotation speed of 300 rpm or less, and spray drying to obtain white spherical powder; the white spherical powder is AlO / Al(OH) x (NH2) y -R powder, x is any number from 1 to 2, y is any number from 1 to 2, and R is octadecyl;

[0033] Step S006, calcining the white spherical powder in a nitrogen protective atmosphere, controlling the calcination temperature to 900-1380°C and the calcination time to 6 hours, to obtain a highly crystalline, high-purity, spherical alumina composite aluminum nitride powder, i.e., a single-particle multi-phase component spherical ceramic powder for network communication.

[0034] A single-particle multi-phase component spherical ceramic powder for network communication is prepared by the above-mentioned preparation method; the single-particle multi-phase component spherical ceramic powder for network communication has an aluminum oxide content of 50-70wt%, an aluminum nitride content of 30-50wt%, a sphericity of more than 95%, and a specific surface area of ​​less than 0.2m 2 / g.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The preparation method of the single-particle multi-phase component spherical ceramic powder for network communication of the present invention comprises the following steps: dissolving a soluble aluminum-based ion salt in water to form an ionic solution, and under the action of a surfactant, forming a spherical micelle powder agglomeration state in the aqueous solution; the soluble aluminum-based ion salt is enriched under the bonding action of a long-chain alkyl surfactant to form aluminum ion spherical micelles with non-polar bonds facing outward; part of the aluminum ion spherical micelles is converted into Al-(NH2) under the action of a nitrogen-based conversion agent. x -O y -R solution; the aluminum ion spherical micelle solution and Al-(NH2) x -O y After mixing the -R solution, an aluminum-based spherical precipitate is formed under the action of the reaction aid, and a spherical AlO / Al(OH) is obtained after drying. x (NH2) y-R powder; then, under a nitrogen protective atmosphere, calcined to obtain spherical alumina / aluminum nitride powder, that is, single-particle multi-phase component spherical ceramic powder for network communication, which can effectively overcome the problem of many factors to be considered in the composite production of different powders to meet the downstream high thermal conductivity requirements and the difficulty of compounding; it can effectively reduce the difficulty of compounding, improve production efficiency, reduce production costs, and avoid the problem of weakening the intrinsic properties of different powders in compounding; and effectively solve the problem that the existing composite ceramic powders prepared by physical and mechanical mixing have different oil absorption characteristics in the subsequent use process, which adversely affects the mechanical properties of the back-end products due to the different oil absorption characteristics of different powders in the composite ceramic powders.

[0037] (2) The preparation method of the single-particle multi-phase component spherical ceramic powder for network communication of the present invention adopts the method of integrated chemical multi-phase synthesis of oxide / nitride single particles to obtain aluminum oxide / aluminum nitride multi-phase ceramic powder, in which both oxide and nitride components are present in a single particle of the powder, thereby realizing effective multi-phase chemical combination of oxide and nitride. When the single-particle multi-phase component spherical ceramic powder for network communication is used, there is no need to match and compound with other powders, and there is no problem of poor matching of different powders, which affects the subsequent use performance of the composite ceramic powder. At the same time, there is no problem in the prior art that the composite ceramic powder prepared by physical and mechanical mixing will affect the mechanical properties of the back-end product during subsequent use due to different oil absorption characteristics.

[0038] (3) In the process of preparing thermal conductive filler using the single-particle multi-phase component spherical ceramic powder for network communication of the present invention, there is no need to set different powder addition ratios and different particle gradings of powders according to different powder properties. The compounding difficulty is low, the production efficiency is effectively improved, and the production cost is reduced; and the problem of weakening the intrinsic properties of different powders during compounding is avoided.

[0039] (4) The single-particle multi-phase component spherical ceramic powder for network communication of the present invention has an aluminum oxide content of 50-70wt%, an aluminum nitride content of 30-50wt%, a sphericity of more than 95%, and a specific surface area of ​​less than 0.2m 2 / g, according to the requirements of high thermal conductivity fillers for spherical ceramic powders, powders with appropriate alumina / aluminum nitride ratios can be selected to effectively realize the application of single-particle multiphase component spherical ceramic powders for network communications in the field of high thermal conductivity.

[0040] (5) During the preparation process of the single-particle multi-phase component spherical ceramic powder for network communication of the present invention, the sintering temperature is 900-1380°C, which is lower than the sintering temperature required for the preparation of single alumina powder and aluminum nitride powder, and can further reduce production energy consumption and significantly reduce production costs; and effectively reduce the labor cost and fuel cost caused by the back-end alumina / aluminum nitride multi-phase powder compounding. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is an electron microscope photograph of the single-particle multi-phase component spherical ceramic powder for network communication in Example 1. DETAILED DESCRIPTION

[0042] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0043] Example 1

[0044] like Figure 1 As shown, this embodiment provides a single-particle multi-phase component spherical ceramic powder for network communication, which has a nearly spherical structure. The specific specifications of the single-particle multi-phase component spherical ceramic powder for network communication are shown in Table 1:

[0045] Table 1 Specifications of single-particle multi-phase component spherical ceramic powder for network communication in Example 1

[0046]

[0047] The single-particle multi-phase component spherical ceramic powder for network communication is prepared from the following raw materials: soluble aluminum-based ion salt, long-chain alkyl surfactant, reaction aid, nitrogen-based conversion agent and water.

[0048] The soluble aluminum-based ion salt is a combination of crystalline aluminum chloride, aluminum sulfate, and basic aluminum acetate; the mass ratio of the crystalline aluminum chloride, aluminum sulfate, and basic aluminum acetate is 2:2:1.

[0049] The long-chain alkyl surfactant is octadecyltrimethylammonium bromide.

[0050] The reaction aid is ammonium oxalate.

[0051] The nitrogen-based conversion agent is 1,14-diazide-3,6,9,12-tetraoxatetradecane.

[0052] The specific weight portions of the above-mentioned raw materials are as follows:

[0053] 10 parts of crystalline aluminum chloride;

[0054] 10 parts of aluminum sulfate;

[0055] 5 parts of basic aluminum acetate;

[0056] 75 parts water;

[0057] 0.05 parts of octadecyltrimethylammonium bromide;

[0058] 0.0075 parts of ammonium oxalate;

[0059] 1,14-diazide-3,6,9,12-tetraoxatetradecane 25 parts.

[0060] This embodiment also provides a method for preparing the single-particle multi-phase component spherical ceramic powder for network communication. A soluble aluminum-based ion salt is dissolved in water to form an ionic solution. Under the action of a surfactant, a spherical micelle powder agglomeration state is formed in the aqueous solution. The soluble aluminum-based ion salt is enriched under the bonding action of a long-chain alkyl surfactant to form aluminum ion spherical micelles with non-polar bonds facing outward. Under the action of a nitrogen-based conversion agent, part of the aluminum ion spherical micelles form Al-(NH2) x -O y -R solution; the aluminum ion spherical micelle solution and Al-(NH2) x -O y After mixing the -R solution, an aluminum-based spherical precipitate is formed under the action of the reaction aid, and a spherical AlO / Al(OH) is obtained after drying. x (NH2) y -R powder; and then calcined in a nitrogen protective atmosphere to obtain spherical alumina / aluminum nitride powder, that is, a single-particle multi-phase component spherical ceramic powder for network communication.

[0061] Among them, spherical AlO / Al(OH) x (NH2) y In -R powder, x=1, y=1, and R is octadecyl.

[0062] The method for preparing the single-particle multi-phase component spherical ceramic powder for network communication is specifically as follows:

[0063] Step S001, adding a long-chain alkyl surfactant into water, stirring at 80°C and 1000 r / min for 0.5 h to obtain a white foamy solution, and keeping at 80°C for 2 h to obtain a transparent spherical micelle solution with a micelle size of 15 nm;

[0064] Step S002, adding a soluble aluminum-based ion salt to the transparent spherical micelle solution, stirring at a stirring speed of 700 r / min at room temperature for 0.5 h, and standing for 1 h to obtain a white sol.

[0065] Step S003, adding a reaction aid to the white sol, mixing and stirring at room temperature at a speed of 100 r / min for 0.5 h, to obtain a milky white high-viscosity sol (i.e., aluminum ion spherical micelles) with a viscosity of 8950 mPa·s.

[0066] Step S004, taking out 35% by weight of the milky white high-viscosity sol of step S003, adding a nitrogen-based conversion agent, and reacting for 2 hours under a temperature of 80° C. and a negative pressure of -0.1 MPa to obtain a white precipitate solution.

[0067] Step S005, mixing the remaining milky white high-viscosity sol of step S003 with the white precipitation solution of step S004, stirring the mixture at 300 rpm for 3 hours, and spray drying the mixture to obtain white spherical powder.

[0068] Step S006, calcining the white spherical powder in a nitrogen protective atmosphere, controlling the calcination temperature to 960°C and the calcination time to 6 hours, to obtain a highly crystalline, high-purity, spherical alumina composite aluminum nitride powder, that is, a single-particle multi-phase component spherical ceramic powder for network communication.

[0069] Example 2

[0070] This embodiment provides a single-particle multi-phase component spherical ceramic powder for network communication, which has a nearly spherical structure. The specific specifications of the single-particle multi-phase component spherical ceramic powder for network communication are shown in Table 2:

[0071] Table 2 Specifications of single-particle multi-phase component spherical ceramic powder for network communication in Example 2

[0072]

[0073] The single-particle multi-phase component spherical ceramic powder for network communication is prepared from the following raw materials: soluble aluminum-based ion salt, long-chain alkyl surfactant, reaction aid, nitrogen-based conversion agent and water.

[0074] The soluble aluminum-based ion salt is a combination of polyaluminum chloride, crystalline aluminum chloride, hydrated aluminum sulfate, and basic aluminum acetate; the mass ratio of the polyaluminum chloride, crystalline aluminum chloride, hydrated aluminum sulfate, and basic aluminum acetate is 1:1:2:1.

[0075] The long-chain alkyl surfactant is octadecylmethyl dihydroxyethyl ammonium bromide.

[0076] The reaction aid is ammonium phosphate.

[0077] The nitrogen-based conversion agent is nitrilotriacetic acid.

[0078] The specific weight portions of the above-mentioned raw materials are as follows:

[0079] 6 parts of polyaluminium chloride;

[0080] 6 parts of crystalline aluminum chloride;

[0081] 12 parts of hydrated aluminum sulfate;

[0082] 6 parts of basic aluminum acetate;

[0083] 70 parts water;

[0084] 0.06 parts of octadecylmethyl dihydroxyethyl ammonium bromide;

[0085] 0.006 parts of ammonium phosphate;

[0086] 30 parts of nitrilotriacetic acid.

[0087] This embodiment also provides a method for preparing the single-particle multi-phase component spherical ceramic powder for network communication. A soluble aluminum-based ion salt is dissolved in water to form an ionic solution. Under the action of a surfactant, a spherical micelle powder agglomeration state is formed in the aqueous solution. The soluble aluminum-based ion salt is enriched under the bonding action of a long-chain alkyl surfactant to form aluminum ion spherical micelles with non-polar bonds facing outward. Under the action of a nitrogen-based conversion agent, part of the aluminum ion spherical micelles form Al-(NH2) x -O y -R solution; the aluminum ion spherical micelle solution and Al-(NH2) x -O y After mixing the -R solution, an aluminum-based spherical precipitate is formed under the action of the reaction aid, and a spherical AlO / Al(OH) is obtained after drying. x (NH2) y -R powder; and then calcined in a nitrogen protective atmosphere to obtain spherical alumina / aluminum nitride powder, that is, a single-particle multi-phase component spherical ceramic powder for network communication.

[0088] Among them, spherical AlO / Al(OH) x (NH2) y In -R powder, x=2, y=1, and R is octadecyl.

[0089] The method for preparing the single-particle multi-phase component spherical ceramic powder for network communication is specifically as follows:

[0090] Step S001, adding a long-chain alkyl surfactant into water, stirring at 85°C and 1100 r / min for 0.75 h to obtain a white foamy solution, and keeping at 85°C for 2.5 h to obtain a transparent spherical micelle solution with a micelle size of 23 nm;

[0091] Step S002, adding a soluble aluminum-based ion salt to the transparent spherical micelle solution, stirring at room temperature for 0.5 h at a stirring speed of 750 r / min, and standing for 2 h to obtain a white sol.

[0092] Step S003, adding a reaction aid to the white sol, mixing and stirring at room temperature for 1.5 hours at a rotation speed of 120 r / min, to obtain a milky white high-viscosity sol (i.e., aluminum ion spherical micelles) with a viscosity of 9500 mPa·s.

[0093] Step S004, taking out 33% by weight of the milky white high-viscosity sol of step S003, adding a nitrogen-based conversion agent, and reacting for 2.5 hours in a sealed state at a temperature of 85° C. and a negative pressure of −0.1 MPa to obtain a white precipitate solution.

[0094] Step S005, mixing the remaining milky white high-viscosity sol of step S003 with the white precipitation solution of step S004, stirring the mixture at a rotation speed of 250 rpm for 3 hours, and spray drying to obtain white spherical powder.

[0095] Step S006, calcining the white spherical powder in a nitrogen protective atmosphere, controlling the calcination temperature to 1380°C and the calcination time to 6 hours, to obtain a highly crystalline, high-purity, spherical alumina composite aluminum nitride powder, that is, a single-particle multi-phase component spherical ceramic powder for network communication.

[0096] Example 3

[0097] This embodiment provides a single-particle multi-phase component spherical ceramic powder for network communication, which has a nearly spherical structure. The specific specifications of the single-particle multi-phase component spherical ceramic powder for network communication are shown in Table 3:

[0098] Table 3 Specifications of single-particle multi-phase component spherical ceramic powder for network communication in Example 3

[0099]

[0100] The single-particle multi-phase component spherical ceramic powder for network communication is prepared from the following raw materials: soluble aluminum-based ion salt, long-chain alkyl surfactant, reaction aid, nitrogen-based conversion agent and water.

[0101] The soluble aluminum-based ion salt is a combination of polyaluminum chloride, aluminum sulfate, and basic aluminum acetate; the mass ratio of the polyaluminum chloride, aluminum sulfate, and basic aluminum acetate is 2:2:1.

[0102] The long-chain alkyl surfactant is octadecyl dimethyl tertiary amine.

[0103] The reaction aid is ammonium formate.

[0104] The nitrogen-based conversion agent is nitrilotriacetic acid.

[0105] The specific weight portions of the above-mentioned raw materials are as follows:

[0106] 12 parts of polyaluminium chloride;

[0107] Aluminum sulfate 12 parts;

[0108] 6 parts of basic aluminum acetate;

[0109] 70 parts of water;

[0110] 0.03 parts of octadecyl dimethyl tertiary amine;

[0111] 0.006 parts of ammonium formate;

[0112] 30 parts of nitrilotriacetic acid.

[0113] This embodiment also provides a method for preparing the single-particle multi-phase component spherical ceramic powder for network communication. A soluble aluminum-based ion salt is dissolved in water to form an ionic solution. Under the action of a surfactant, a spherical micelle powder agglomeration state is formed in the aqueous solution. The soluble aluminum-based ion salt is enriched under the bonding action of a long-chain alkyl surfactant to form aluminum ion spherical micelles with non-polar bonds facing outward. Under the action of a nitrogen-based conversion agent, part of the aluminum ion spherical micelles form Al-(NH2) x -O y -R solution; the aluminum ion spherical micelle solution and Al-(NH2) x -O y After mixing the -R solution, an aluminum-based spherical precipitate is formed under the action of the reaction aid, and a spherical AlO / Al(OH) is obtained after drying. x (NH2) y -R powder; and then calcined in a nitrogen protective atmosphere to obtain spherical alumina / aluminum nitride powder, that is, a single-particle multi-phase component spherical ceramic powder for network communication.

[0114] Among them, spherical AlO / Al(OH) x (NH2) y In -R powder, x=1, y=2, and R is octadecyl.

[0115] The method for preparing the single-particle multi-phase component spherical ceramic powder for network communication is specifically as follows:

[0116] Step S001, adding a long-chain alkyl surfactant into water, stirring at 1200 r / min for 1 hour at 70° C. to obtain a white foamy solution, and keeping at 70° C. for 2 hours to obtain a transparent spherical micelle solution with a micelle size of 20 nm;

[0117] Step S002, adding a soluble aluminum-based ion salt to the transparent spherical micelle solution, stirring at a stirring speed of 700 r / min at room temperature for 1 hour, and standing for 2 hours to obtain a white sol.

[0118] Step S003, adding a reaction aid to the white sol, mixing and stirring at room temperature at a speed of 130 r / min for 1.5 hours, to obtain a milky white high-viscosity sol (i.e., aluminum ion spherical micelles) with a viscosity of 7500 mPa·s.

[0119] Step S004, taking out 43% by weight of the milky white high-viscosity sol of step S003, adding a nitrogen-based conversion agent, and reacting for 2 hours under a temperature of 85° C. and a negative pressure of -0.1 MPa to obtain a white precipitate solution.

[0120] Step S005, mixing the remaining milky white high-viscosity sol of step S003 with the white precipitation solution of step S004, stirring the mixture at a rotation speed of 250 rpm for 3 hours, and spray drying to obtain white spherical powder.

[0121] Step S006, calcining the white spherical powder in a nitrogen protective atmosphere, controlling the calcination temperature to 1250°C and the calcination time to 6 hours, to obtain a high-crystalline, high-purity, spherical alumina composite aluminum nitride powder, that is, a single-particle multi-phase component spherical ceramic powder for network communication.

[0122] Comparative Example 1

[0123] Comparative Example 1 adopts the technical solution of Example 1, except that: 1) sodium hydroxide is used instead of ammonium oxalate as a reaction aid; 2) the addition of the nitrogen-based conversion agent (1,14-diazide-3,6,9,12-tetraoxatetradecane) and its related use steps are omitted.

[0124] Specifically, in the preparation method of the spherical ceramic powder of Comparative Example 1, spherical Al(OH)2-R powder is obtained by drying; and then spherical ceramic powder is obtained by calcining under a nitrogen protective atmosphere.

[0125] Among them, in the spherical Al(OH)2-R powder, R is octadecyl.

[0126] The preparation method of the spherical ceramic powder of Comparative Example 1 is specifically as follows:

[0127] Step S001, adding a long-chain alkyl surfactant into water, stirring at 80°C and 1000 r / min for 0.5 h to obtain a white foamy solution, and keeping at 80°C for 2 h to obtain a transparent spherical micelle solution with a micelle size of 15 nm;

[0128] Step S002, adding a soluble aluminum-based ion salt to the transparent spherical micelle solution, stirring at a stirring speed of 700 r / min at room temperature for 0.5 h, and standing for 1 h to obtain a white sol.

[0129] Step S003, adding a reaction aid to the white sol, mixing and stirring at room temperature at a speed of 100 r / min for 0.5 h, to obtain a milky white high-viscosity sol with a viscosity of 15500 mPa·s.

[0130] Step S004, spray drying the milky white high-viscosity sol to obtain white spherical powder.

[0131] Step S006, calcining the white spherical powder in a nitrogen protective atmosphere, controlling the calcination temperature to 960° C. and the calcination time to 6 hours, to obtain spherical ceramic powder.

[0132] The specific specifications of the spherical ceramic powder of Comparative Example 1 are shown in Table 4:

[0133] Table 4 Specifications of spherical ceramic powder of Comparative Example 1

[0134]

[0135] It can be seen that the spherical ceramic powder obtained in comparative example 1 has a relatively low alumina content, does not contain aluminum nitride components, and has a high specific surface area; in the subsequent preparation of high thermal conductivity fillers, it is necessary to conduct secondary mechanical mixing with aluminum nitride powder, and the mechanical mixing preparation inevitably has the problem of poor matching of the two powders; and due to the different oil absorption characteristics of the two powders, the back-end product (composite ceramic powder thermal conductive material) will have mechanical weak points or stress concentration points, affecting the mechanical properties of the back-end product. Furthermore, in the process of preparing high thermal conductivity fillers by mixing the two powders, in order to meet the requirements of high thermal conductivity performance, the composite of the two powders needs to consider many factors, and the compounding is difficult; there are problems of high production cost, low production efficiency, and weakening of the intrinsic properties of different powders.

[0136] In summary, the preparation method of the single-particle multi-phase component spherical ceramic powder for network communication of the present invention comprises the following steps: dissolving a soluble aluminum-based ion salt in water to form an ionic solution, and under the action of a surfactant, forming a spherical micelle powder agglomeration state in the aqueous solution; the soluble aluminum-based ion salt is enriched under the bonding action of a long-chain alkyl surfactant to form aluminum ion spherical micelles with non-polar bonds facing outward; part of the aluminum ion spherical micelles is converted into Al-(NH2) under the action of a nitrogen-based conversion agent. x -O y -R solution; the aluminum ion spherical micelle solution and Al-(NH2) x -O y After mixing the -R solution, an aluminum-based spherical precipitate is formed under the action of the reaction aid, and a spherical AlO / Al(OH) is obtained after drying. x (NH2) y-R powder; then, under a nitrogen protective atmosphere, calcined to obtain spherical alumina / aluminum nitride powder, that is, single-particle multi-phase component spherical ceramic powder for network communication, which can effectively overcome the problem of many factors to be considered in the composite production of different powders to meet the downstream high thermal conductivity requirements and the difficulty of compounding; it can effectively reduce the difficulty of compounding, improve production efficiency, reduce production costs, and avoid the problem of weakening the intrinsic properties of different powders in compounding; and effectively solve the problem that the existing composite ceramic powders prepared by physical and mechanical mixing have different oil absorption characteristics in the subsequent use process, which adversely affects the mechanical properties of the back-end products due to the different oil absorption characteristics of different powders in the composite ceramic powders.

[0137] Unless otherwise specified, all percentages used in the present invention are by mass.

[0138] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a single-particle multi-phase component spherical ceramic powder for network communication, characterized in that: The preparation is carried out using the following raw materials: soluble aluminum-based ion salt, long-chain alkyl surfactant, reaction aid, nitrogen-based conversion agent and water; The soluble aluminum-based ion salt is at least one of the following: aluminum chloride, aluminum sulfate, and aluminum acetate; The long-chain alkyl surfactant is at least one of the following: octadecyl trimethyl ammonium bromide, octadecyl dimethyl tertiary amine, octadecyl methyl dihydroxyethyl ammonium bromide; The reaction aid is at least one of the following: ammonium oxalate, ammonium acetate, ammonium formate, ammonium citrate, and ammonium phosphate; The nitrogen-based conversion agent is at least one of the following: 1,14-diazide-3,6,9,12-tetraoxatetradecane, nitrilotriacetic acid; The method for preparing the single-particle multi-phase component spherical ceramic powder for network communication comprises the following steps: Step S001, adding a long-chain alkyl surfactant into water, stirring evenly at a temperature of 60-85° C. to obtain a white foamy solution, and keeping it at 60-85° C. to obtain a transparent spherical micelle solution; Step S002, adding a soluble aluminum-based ion salt to the transparent spherical micelle solution, stirring at a stirring speed of 300-800 r / min at room temperature, and then standing to obtain a white sol; Step S003, adding a reaction aid to the white sol, mixing and stirring at room temperature for more than 0.5 h to obtain a milky white high-viscosity sol; Step S004, taking out 30-50% by weight of the milky white high-viscosity sol, adding a nitrogen-based conversion agent, and reacting in a sealed manner under a negative pressure environment at a temperature of 60-90° C. to obtain a white precipitation solution; Step S005, mixing the remaining milky white high-viscosity sol of step S003 and the white precipitation solution of step S004 evenly, and spray drying to obtain white spherical powder; The white spherical powder is AlO / Al(OH) x (NH2) y -R powder, x is any number from 1 to 2, y is any number from 1 to 2, and R is octadecyl; Step S006, calcining the white spherical powder in an inert gas protective atmosphere, controlling the calcination temperature to 900-1380°C and the calcination time to more than 6 hours, to obtain a highly crystalline, high-purity, spherical alumina composite aluminum nitride powder, i.e., a single-particle multi-phase component spherical ceramic powder for network communication.

2. The method for preparing a single-particle multi-phase component spherical ceramic powder for network communication according to claim 1, characterized in that: The aluminum chloride salt is at least one of the following: crystalline aluminum chloride, polyaluminum chloride; The aluminum sulfate salt is at least one of the following: hydrated aluminum sulfate, basic aluminum sulfate; The aluminum acetate is basic aluminum acetate.

3. The method for preparing a single-particle multi-phase component spherical ceramic powder for network communication according to claim 1, characterized in that: The mass ratio of the soluble aluminum-based ion salt to water is 15-35:65-85; The mass ratio of the nitrogen-based conversion agent to the soluble aluminum-based ion salt is 1:

1.

4. The method for preparing a single-particle multi-phase component spherical ceramic powder for network communication according to claim 1, characterized in that: The amount of the long-chain alkyl surfactant is 0.1-0.5% of the mass of the soluble aluminum-based ion salt; The dosage of the reaction aid is 0.02-0.05% of the mass of the soluble aluminum-based ion salt.

5. The method for preparing a single-particle multi-phase component spherical ceramic powder for network communication according to claim 1, characterized in that: In the soluble aluminum-based ion salt, the mass ratio of aluminum chloride salt, aluminum sulfate salt and aluminum acetate salt is 2:2:

1.

6. The method for preparing a single-particle multi-phase component spherical ceramic powder for network communication according to claim 1, characterized in that: In the step S001, the micelle particle size of the transparent spherical micelle solution is 10-30 nm; In the step S003, the viscosity of the milky white high-viscosity sol is 8000-13000 mPa·s.

7. A single-particle multi-phase component spherical ceramic powder for network communication, characterized in that: The single-particle multi-phase component spherical ceramic powder for network communication has an aluminum oxide content of 50-70wt%, an aluminum nitride content of 30-50wt%, a sphericity of more than 95%, and a specific surface area of ​​less than 0.2m 2 / g.