Indenofluorene derivative and electroluminescent device thereof

By designing indenofluorene derivatives as the main material of OLED display devices, the problems of insufficient luminous efficiency and lifetime of luminescent materials in the existing technology are solved, and efficient triplet energy level transfer and stable luminescent performance are achieved, which is suitable for OLEDs. Display device applications.

CN118724670APending Publication Date: 2024-10-01西安欧得光电材料有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410804292.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The luminescent materials of existing OLED display devices have shortcomings in luminous efficiency and lifetime. In particular, the host material is difficult to adapt to the changing characteristics of the guest material, resulting in poor triplet luminescence performance and affecting the overall performance of the device.

Method used

An indenofluorene derivative was designed as the host material. By substituting at the 9-position of fluorene to increase spatial rigidity, it was connected to the structure of a common fluorescent host material, and an indenofluorene structure with high triplet energy level was introduced. Improve luminous efficiency and stability.

Benefits of technology

It significantly improves the luminous efficiency of the luminescent layer and device lifetime, enhances the spatial configuration and film-forming properties of molecules, is suitable for existing fluorescent host material application scenarios, and improves the overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724670A_ABST
    Figure CN118724670A_ABST
Patent Text Reader

Abstract

The invention discloses an indenofluorene derivative and an electroluminescent device thereof, the indenofluorene derivative has a high glass transition temperature, and when the indenofluorene derivative is applied to an OLED (Organic Light Emitting Diode) device, the stability of the device is effectively ensured; meanwhile, the derivative has relatively high triplet excitation energy, and when the derivative is used as a host luminescent material, the derivative can transfer rich triplet exciton energy to a corresponding guest phosphorescent illuminant for luminescence, so that the overall luminous efficiency of a device is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic luminescent materials and semiconductors, and specifically relates to an indenofluorene derivative and an electroluminescent device thereof. Background Art

[0002] Display technology is becoming more and more inseparable from people's production and life, and people are constantly putting forward higher requirements for the effects and application scenarios of image display. As a new generation of information display trend technology, the speed of change and iteration of OLED technology is increasing day by day. The continuous iteration and change of technology has promoted the rapid development of display technology. At present, this emerging display technology is gradually becoming mature and stable. In the future, it will provide a variety of solutions for various electrical equipment, transportation, wearable devices, etc. to provide a friendly visualization experience of human-machine interface information interaction. As a rising star, the new OLED display technology has a good universal display technology to achieve many demanding engineering requirements such as thin, transparent, wearable, foldable, low energy consumption, wide viewing angle, and low temperature resistance. This technology is the most promising feasible technical path to provide an integrated solution to the above requirements. At present, commercial OLED display screens have begun to develop and promote from small display screens to large screens, bendable, ultra-thin and many other above-mentioned sub-segments. In the future, it is the most promising new generation of products that can completely replace existing display technologies in the display field. In order to promote the further application of this technology, industry practitioners are making a lot of R&D investment in many aspects, from device structure design, engineering technology innovation to new material design, and constantly working hard to meet people's demand for humanized multi-dimensional display as soon as possible. In addition, OLED technology is constantly exploring new application scenarios in the field of high-end lighting by taking advantage of its self-luminous characteristics and the ability to adjust the luminous color at will through materials.

[0003] As an important driving force for the innovation of display technology, new materials have always been one of the major tasks of scientific researchers in this field. Currently, most mature and mainstream OLED display devices are implemented using a sandwich multi-layer device structure, and the various functional layers in the device optimize the technical dimension parameters of the overall device through mutual synergy. The above-mentioned multi-layer device structure mainly includes an anode plate, a cathode plate, and functional materials located between the anode plate and the cathode plate; specifically, the hole injection layer, hole transport layer, light-emitting layer, electron transport layer, electron injection layer and other functional layer materials are filled in sequence from the anode plate to the cathode plate to achieve. In order to effectively improve the luminous efficiency of the light-emitting device, while reducing the power consumption of the device and extending the life of the device, the materials of each functional layer need to be continuously innovated and iterated to meet the latest market development needs of the device.

[0004] Among the above functional layer materials, the luminescent material is one of the main components of the device, and its luminescent performance efficiency and life reliability are undoubtedly the most important indicators. In order to achieve an efficient luminescence process, the device construction mode and technology that relies on a single luminescent layer for luminescence are gradually replaced by the current composite luminescent functional layer device construction technology. The composite luminescent layer is mainly composed of a host material and a guest material, and some devices will further dope sensitizer materials to further improve the luminescence efficiency of the luminescent layer. At present, phosphorescent materials have made great breakthroughs in guest materials due to their high luminescence efficiency. Various structures and luminescent specific phosphorescent materials are being developed. In order to cooperate with the above-mentioned iterative and innovative guest luminescent materials, the host material needs to be adjusted and optimized accordingly to adapt to the performance requirements of the above-mentioned guest materials. In order to fully exert the triplet luminescence performance of the phosphorescent material, it is necessary to adaptively adjust the triplet energy level of the host material to cope with the new characteristics of the material that is constantly changing. Therefore, it is very necessary and urgent to develop a host material with a higher triplet energy level, a larger scale range of spatially stable structure, and higher film-forming stability. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned deficiencies of the prior art and provide an indenofluorene derivative and an electroluminescent device thereof, wherein the indenofluorene derivative is used as a host material.

[0006] The technical solution of the present invention is: an indenofluorene derivative, the structural formula of the indenofluorene derivative is shown in the following general formula 1:

[0007]

[0008] in:

[0009] A is selected from C5~C 15 The aromatic condensed ring, A and the main structure are bonded by a single bond or a ring-joined bond;

[0010] B is selected from phenyl, naphthyl, anthracenyl, phenanthrenyl and C5~C 20 Aromatic fused ring or aromatic fused heterocyclic ring, B is bonded to the main structure by a single bond;

[0011] R1, R2, R3, and R4 are independently selected from H, deuterium, C1-C5 alkyl, C5-C 15 R5, R6 are independently selected from H, deuterium, C3~C 15 Alkyl, C6~C 20 Aryl, C5~C 20 The heterocyclic aromatic group.

[0012] Preferably, the general formula 1 includes general formulas 2-1, 2-2, 2-3, 2-4 and 2-5, and the specific structural formulas are as follows:

[0013]

[0014] in:

[0015] B is selected from phenyl, naphthyl, anthracenyl, phenanthrenyl and C5~C 20 Aromatic fused ring or aromatic fused heterocyclic ring, B is bonded to the main structure by a single bond;

[0016] R1, R2, R3, and R4 are independently selected from H, deuterium, C1-C5 alkyl, C5-C 15 R5, R6 are independently selected from H, deuterium, C3~C 15 Alkyl, C6~C 20 Aryl, C5~C 20 The heterocyclic aromatic group.

[0017] Preferably, an electroluminescent device comprises a first electrode, a second electrode and an organic layer located between the first electrode and the second electrode, wherein the organic layer comprises a combination of any one or more compounds of the indenofluorene derivative compounds 1 to 188.

[0018] Preferably, the organic layer comprises a hole transport layer, a light-emitting layer and an electron transport layer, wherein the light-emitting layer comprises a combination of one or more of compounds 1 to 188.

[0019] Preferably, the light-emitting layer is composed of a combination of a host material and a guest material, wherein the ratio of the host material to the guest material is 95:5 to 99:1.

[0020] Preferably, the ratio of the host material to the guest material is 98:2.

[0021] Preferably, the host material is selected from one or a combination of two of compounds 1 to 188, and the guest material is selected from

[0022] Compared with the prior art, the advantages of the present invention are:

[0023] (1) The indenofluorene structure designed in the present invention has a high structural stability. First, the 9-position (R1, R2 or R3, R4 substitution position) of fluorene is effectively substituted to increase the spatial rigidity of the entire molecule. Second, the main structure is effectively connected with a common fluorescent main material structure fragment (B). This not only effectively transforms the structure of the conventional fluorescent main material, but also retains the efficient fluorescent luminescence efficiency of the conventional fluorescent main structure, and further improves the stability of the traditional fluorescent main material in terms of spatial structure, thereby further extending the device life.

[0024] (2) The present invention introduces an indenofluorene structure with a high triplet energy level, which can further improve the triplet energy level of the fluorescent main light emitter after being adapted to the traditional fluorescent main structure. When this type of material is used as a main material, it can more efficiently transfer and transfer the energy of its triplet excitons to the matching guest material, thereby greatly improving the luminous efficiency of the light-emitting layer;

[0025] (3) The indenofluorene derivatives designed by the present invention have a large spatial stereo configuration. In addition to having a high glass transition temperature, the molecules have a significant asymmetric configuration and excellent film-forming properties during molecular evaporation, which significantly improves the luminescence consistency, thereby effectively improving the device yield;

[0026] (4) The designed material of the present invention has good compatibility with the traditional high-efficiency fluorescent main body core structure, and has little impact on the application matching mode of the above-mentioned traditional main body core structure, which is conducive to the rapid application of the material to the existing mature fluorescent main body material application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 , a cross-sectional view of an electroluminescent device of the present invention;

[0028] Figure 2 , the NMR spectrum of compound 3 of the present invention;

[0029] Figure 3 , the NMR spectrum of compound 10 of the present invention;

[0030] Figure 4 , the NMR spectrum of compound 49 of the present invention;

[0031] Figure 5 , the NMR spectrum of compound 107 of the present invention;

[0032] Figure 6 , NMR spectrum of compound 112 of the present invention

[0033] Figure 7 , NMR spectrum of compound 151 of the present invention

[0034] Figure 8, the NMR spectrum of compound 187 of the present invention.

[0035] Attached Figure 1 Marking Description:

[0036] 1. Glass plate or polymer substrate, 2. Anode layer, 3. Hole injection layer, 4. Hole transport layer, 5. Electron blocking layer, 6. Light-emitting layer, 7. Hole blocking layer, 8. Electron transport layer, 9. Electron injection layer, 10. Cathode layer, 11. Covering layer. DETAILED DESCRIPTION

[0037] The specific implementation mode of the present invention is described below in conjunction with examples. The raw materials and reagents described in the present invention are all commercially available.

[0038] The present invention discloses an indenofluorene derivative, the general structural formula of the indenofluorene derivative is as follows:

[0039] As shown in formula 1:

[0040]

[0041] in:

[0042] A is selected from C5~C 15 The aromatic condensed ring, A and the main structure are bonded by a single bond or a ring-joined bond;

[0043] B is selected from phenyl, naphthyl, anthracenyl, phenanthrenyl and C5~C 20 Aromatic fused ring or aromatic fused heterocyclic ring, B is bonded to the main structure by a single bond;

[0044] R1, R2, R3, and R4 are independently selected from H, deuterium, C1-C5 alkyl, C5-C 15 R5, R6 are independently selected from H, deuterium, C3~C 15 Alkyl, C6~C 20 Aryl, C5~C 20 The heterocyclic aromatic group.

[0045] Preferably, the general formula 1 includes general formulas 2-1, 2-2, 2-3, 2-4 and 2-5, and the specific structural formulas are as follows:

[0046]

[0047] in:

[0048] B is selected from phenyl, naphthyl, anthracenyl, phenanthrenyl and C5~C 20 Aromatic fused ring or aromatic fused heterocyclic ring, B is bonded to the main structure by a single bond;

[0049] R1, R2, R3, and R4 are independently selected from H, deuterium, C1-C5 alkyl, C5-C 15 R5, R6 are independently selected from H, deuterium, C3~C 15 Alkyl, C6~C 20 Aryl, C5~C 20 The heterocyclic aromatic group.

[0050] Preferably, the indenofluorene derivatives include compounds 1 to 188, and the specific structural formulas are as follows:

[0051]

[0052]

[0053]

[0054]

[0055]

[0056]

[0057]

[0058] Preferably, an electroluminescent device comprises a first electrode, a second electrode and an organic layer located between the first electrode and the second electrode, wherein the organic layer comprises a combination of any one or more compounds of the indenofluorene derivative compounds 1 to 188.

[0059] Preferably, the organic layer comprises a hole transport layer, a light-emitting layer and an electron transport layer, wherein the light-emitting layer comprises a combination of one or more of compounds 1 to 188.

[0060] Preferably, the light-emitting layer is composed of a combination of a host material and a guest material, wherein the ratio of the host material to the guest material is 95:5 to 99:1.

[0061] Preferably, the ratio of the host material to the guest material is 98:2.

[0062] Preferably, the host material is selected from one or a combination of two of compounds 1 to 188, and the guest material is selected from

[0063] The synthesis process of compounds 1 to 188 is described as follows:

[0064] The implementation process of the key intermediate synthesis process is as follows:

[0065] 1. Synthesis steps of key intermediate M1:

[0066]

[0067] Step 1:

[0068]

[0069] Operation process: under argon protection, add 238g (1.0mol) of 9,9-dimethyl-4-boric acid fluorene, 249g (1.0mol) of methyl 2-bromo-5-chlorobenzoate, 276g (2.0mol) of potassium carbonate, 1.9L of ethanol, and 450mL of deionized water into a 5L three-necked flask in sequence, start stirring, stir evenly, add 11.5g of tetrakistriphenylphosphine palladium into the reaction flask, and then heat the reaction system to reflux for insulation reaction, and inert gas protection is done during the whole process. Insulate the reaction for 8 to 10 hours until the raw materials react completely and then treat. Add water to the reaction solution, extract with ethyl acetate and combine the organic phases, then concentrate under reduced pressure to obtain the crude product of M1-1; the crude product is purified by column chromatography and crystallization from petroleum ether to obtain an off-white solid weighing 265g, with a GC content of 97%, a yield of 73%, and a molecular weight of 362.11 shown by GC-MS.

[0070] Step 2:

[0071]

[0072] Operation process: Under argon protection, add M1-1: 200g (0.55mol), THF1.5L to a 3L three-necked flask in sequence, slowly raise the system temperature to 40-45°C, then drop 0.825L of methylmagnesium bromide solution (2mol / L) into the system, control the temperature between 40-45°C, and continue to keep warm for 2h until the reaction is complete. After the reaction solution is cooled to room temperature, slowly pour ammonium chloride (1.0mol / L) aqueous solution under stirring to quench the reaction, then extract with ethyl acetate, wash the organic phase with water, separate the liquids, dry it, and then concentrate it under reduced pressure to obtain the crude product of M1-2. The crude product is solidified with petroleum ether and filtered and dried to obtain 134g of white solid, HPLC

[0073] The content was 98%, the yield was 67%, and the molecular weight was 363.10 as shown by LC-MS.

[0074] Step 3:

[0075]

[0076] Operation process: Under an inert atmosphere, add 134g (0.37mol) of M1-2, 0.7L of toluene, and 70g of p-toluenesulfonic acid monohydrate into a 2L three-necked flask in sequence, start stirring, heat to reflux for water separation reaction, and stop the reaction until no water is separated from the system. The reaction solution is cooled to room temperature and then separated. The organic phase is washed with water and then subjected to column chromatography, and then concentrated under reduced pressure to obtain a solid crude product; the crude product is refluxed with ethanol and then cooled to room temperature for filtration and drying to obtain 103g of white solid, GC content 99%, yield 81%, GC-MS shows a molecular weight of 344.12.

[0077] 2. Synthesis steps of M2:

[0078] Step 1:

[0079]

[0080] Operation process: The feeding process refers to the synthesis process of M1-1, 362g (1.0mol) of 9,9-diphenyl-4-boric acid fluorene is added, and 336g of white solid M2-1 is produced, with HPLC content of 97%, yield of 69%, and LC-MS molecular weight of 487.11.

[0081] Step 2:

[0082]

[0083] Operation process: The feeding process refers to the synthesis process of M1-2. The reaction feed M2-1 is 300g, and the output white solid M2-2: 192g, HPLC content 99%, yield 64%; LC-MS molecular weight 487.14.

[0084] Step 3:

[0085]

[0086] Operation process: The synthesis process refers to the synthesis process of M1, and 192 g of M2-2 is added to produce a white solid M2. Heavy off-white solid M2 weighs 155 g, HPLC content is 98%, yield is 84%; LC-MS molecular weight is 469.14.

[0087] 3. Synthesis steps of M3:

[0088]

[0089] Operation procedure: Add 330g (2.1mol / L) of bromobenzene and 2.0L of THF to a 5L three-necked flask under argon protection, cool down to -85--80°C while stirring, then drip 0.84L of n-butyl lithium solution (2.5mol / L), control the reaction temperature between -85--80°C and continue to keep warm for 1h, then drip 500mL of 1-1THF solution containing 254g into the reaction system, then naturally warm up to room temperature, and the reaction is complete. After adding 20mL of water to quench the reaction, the reaction solution is concentrated under reduced pressure, and ethyl acetate is added to dissolve after concentration, and then the organic phase is washed with water and dried, and the dried organic phase is re-concentrated under reduced pressure and then n-heptane is added for crystallization, filtered, and dried to obtain 249g of a slightly yellow solid, with a main content of 98% by LC, and a molecular weight of 487.15 by LC-MS.

[0090] Synthesis of M3:

[0091]

[0092] Operation procedure: refer to the synthesis process of M1, add a total of 249 g of M3-1, and output 187 g of M3, with a yield of 78%; LC-MS molecular weight 469.12.

[0093] 4. Synthesis steps of M4:

[0094] Step 1:

[0095]

[0096] Operating procedures: Add 334g (1.0mol) of methyl 3-(trifluoromethylsulfonyloxy)-2-naphthoate, 157g (1.0mol) of o-chlorophenylboric acid, 276g of potassium carbonate, 1L of toluene, 300mL of ethanol, and 300mL of deionized water to a 3L three-necked flask under argon protection, start stirring until the system is dissolved and cleaned, then add 11.5g of tetrakistriphenylphosphine palladium, continue to heat to 70-74°C for reaction, and the reaction is completed after 5h of reaction. The reaction solution is cooled to room temperature and separated, the aqueous phase is extracted with toluene and then the organic phase is combined; the organic phase is further washed with water, dried, and then passed through a chromatography column, and the column liquid is concentrated under reduced pressure to obtain a crude product of M4-1, which is crystallized and solidified by petroleum ether and filtered to obtain 229g of an off-white solid with a GC content of 97%. GC-MS shows a molecular weight of 296.06.

[0097] Step 2:

[0098]

[0099] Operation procedure: refer to the synthesis process of M3-1, add 200g of M4-1 in total, and produce 207g of M4-2.

[0100] Yield: 73%; LC-MS molecular weight: 421.11.

[0101] Step 3:

[0102]

[0103] Operation procedure: refer to the synthesis process of M1, add a total of 207 g of M4-2, and produce 160 g of M4-3, with a yield of 81%; LC-MS shows a molecular weight of 403.10.

[0104] Step 4:

[0105]

[0106] Operation procedure: 150g (0.37mol) of M4-3, 104g (0.41mol) of bipyralidin, 72g of potassium acetate, and 1.2L of 1,4-dioxane were added to a 3L three-necked flask under argon protection. After stirring evenly, 33.4g of Pd2(dba) and 3.5g of X-Phos were added to the reaction flask, and then the system was heated to 95-100°C for insulation reaction. The reaction was completed in 4-5h. After the reaction solution was cooled to room temperature, a small amount of water was added and then separated. The aqueous phase was extracted with ethyl acetate and then the organic phase was combined. The organic phase was concentrated under reduced pressure and toluene was added again to dissolve, and then the organic phase was further washed with water. After the organic phase was dried, it was concentrated to dryness under reduced pressure through a chromatography column, and then ethanol was added for crystallization. The solid was filtered to obtain 144g of light gray solid, with a yield of 78%. LC-MS showed a molecular weight of 495.24.

[0107] Step 5:

[0108]

[0109] Operation procedure: refer to the feeding process of M1-1, feed M4-4 75g, output M4-5 60g, yield 74%, LC-MS shows the molecular weight is 537.12.

[0110] Step 6:

[0111]

[0112] Operation procedure: refer to the synthesis process of M1-2, add 50 g of M4-5, output M4-6 31 g, yield 62%; LC-MS molecular weight 537.16.

[0113] Step 7:

[0114]

[0115] Operation procedure: refer to the synthesis process of M1, feed M4-6 30g, output M4 22g, yield 76%; LC-MS molecular weight 519.15.

[0116] Through the above-mentioned similar synthesis methods, some important intermediates were prepared and synthesized, as shown in Table 1:

[0117]

[0118]

[0119] The above key intermediates were used to synthesize Compound 3, Compound 10, Compound 49, Compound 107, Compound 112, Compound 151 and Compound 187. The implementation process is as follows:

[0120] Synthesis of compound 3:

[0121] first step:

[0122]

[0123] Operation process: under argon protection, add 40.0g of M2, 23.8g of biboric acid pinacol ester, 16.4g of potassium acetate, and 400mL of 1,4-dioxane to a 1L three-necked reaction bottle, start stirring, stir the system evenly, then add 30.78g of Pd2(dba) and 0.81g of X-Phos to the system, then heat the system to 100-102°C for insulation reaction, and the reaction time is 10-12h until the reaction is complete. After the reaction liquid is naturally cooled to room temperature, the reaction system is directly passed through a diatomaceous earth funnel, the filter cake is rinsed with ethyl acetate, the filtrate is collected, the filtrate is concentrated under reduced pressure, and toluene is added again to dissolve and become clear, the organic phase is further washed with water, and after completion, the organic phase is dried and column chromatographed, and the column liquid is concentrated under reduced pressure to obtain a crude product of 3-1. The crude product was recrystallized from a mixed solvent of ethyl acetate and n-heptane to obtain 37.8 g of white solid 3-1 with a yield of 79%. LC showed a purity of 99% and LC-MS showed a molecular weight of 561.27.

[0124] Step 2:

[0125]

[0126] Operation process: Add 10.0g of 3-1, 5.95g of 9-phenyl-10-anthraceneboronic acid, 4.92g of potassium carbonate, 200mL of 1,4-dioxane, and 20mL of deionized water to a 500mL flask under argon protection, start stirring, and add 30.31g of catalyst Pd2 (dba) after the system is stirred and mixed evenly, and then continue to heat to 80-85℃ for insulation reaction until the raw material tracking 3-1 reacts completely and then stops the reaction. After the reaction liquid is cooled naturally to room temperature, it is poured into 1L of water with stirring to precipitate a solid crude product, and the crude product is filtered to obtain a light gray solid. After the solid crude product is dried, it is redissolved in toluene and purified by column chromatography, and then further recrystallized from xylene to obtain 9.3g of solid, LC purity 99.8%, LC-MS molecular weight 687.30.

[0127] Synthesis of compound 10:

[0128] first step:

[0129]

[0130] Operation process: The synthesis process refers to the synthesis process of compound 3-1, 15 g of M1 was added, and 12.5 g of 10-1 crude product was produced; the crude product was further crystallized from ethanol to obtain 10-1, 10.5 g, with a content of 99% and a yield of 66%. LC-MS showed a molecular weight of 437.25.

[0131] Step 2:

[0132]

[0133] Operation process: refer to the synthesis process of compound 3, input 10-1 (10 g), output compound 10 (10.7 g), yield 73%, LC-MS shows molecular weight 613.22.

[0134] Synthesis of compound 49:

[0135] first step:

[0136]

[0137] Operation process: The synthesis process refers to the synthesis process of compound 3-1, 10 g of M19 was added, 8.3 g of 49-1 was produced, the content was 99%, the yield was 68%, and LC-MS showed a molecular weight of 513.25.

[0138] Step 2:

[0139]

[0140] Operation process: refer to the synthesis process of compound 3 for synthesis, input 49-1 (8 g), output compound 49 (8.2 g), yield 76%, LC-MS shows molecular weight 689.31.

[0141] Synthesis of compound 107:

[0142] first step:

[0143]

[0144] Operation process: refer to the synthesis process of compound 3-1 for synthesis, feed M4 is 15 g, output 107-1 is 14.3 g, HPLC content is 99%, yield is 81%, LC-MS shows molecular weight is 611.30.

[0145] Step 2:

[0146]

[0147] Operation process: refer to the synthesis process of compound 3 for synthesis, feed 107-1 (10 g), output 107 (8.0 g), HPLC 99.9%, yield 71%, LC-MS showed molecular weight 685.24.

[0148] Synthesis of compound 112:

[0149]

[0150] Operation process: add 10g of M4, 7.2g of 4-phenyl-6-boronic acid pinacol ester-dibenzofuran, 2.2g of potassium hydroxide, 120mL of 1,4-dioxane, and 15mL of deionized water into a 500mL flask, start stirring, stir evenly, add 0.23g of tetrakistriphenylphosphine palladium, continue to heat to reflux and keep warm for 8 to 10 hours until the reaction is complete. The reaction solution is directly poured into water, filtered to precipitate solids, dried solids are dissolved in toluene and purified by column chromatography, and the column liquid is concentrated under reduced pressure and then recrystallized with a mixed solvent of toluene and ethyl acetate to obtain 10.9gg of white solids, with a yield of 78%, and LC-MS shows a molecular weight of 727.29.

[0151] Synthesis of compound 151:

[0152]

[0153] Operation process: The synthesis process was completed by referring to the synthesis process of compound 112, 10 g of M9 was added, 8.6 g of compound 151 was produced, the yield was 63%, HPLC = 99.9%, LC-MS showed a molecular weight of 701.26.

[0154] Synthesis of compound 187:

[0155]

[0156] Operation process: refer to the synthesis process of compound 112, add 10 g of M24, and produce 12.4 g of compound 187, with a yield of 74%. LC-MS shows a molecular weight of 663.29.

[0157] The synthesis processes of Compounds 1 to 188 were all completed by referring to the above-mentioned synthesis example processes. The important starting materials used in the synthesis processes are listed in Table 2 below.

[0158]

[0159]

[0160] Figures 2 to 8 The NMR spectra of Compound 3, Compound 10, Compound 49, Compound 107, Compound 112, Compound 151 and Compound 187 are summarized as follows:

[0161] Proton spectrum data of compound 3:

[0162] 1 H NMR (400MHz, DMSO-d6) δ8.20(dd,J=5.6,3.3Hz,4H),7.83(ddd,J=6.0,4.5,1.9Hz,2H),7.72–7.65(m,2H),7.52(ddd, J=9.0,6.7,2.4Hz,6H),7.47–7.32(m,6H),7.32–7.20(m,7H),7.12(d,J=7.6Hz,1H),7.09–7.02(m,4H),1.55(s,6H).

[0163] Proton spectrum data of compound 10:

[0164] 1 H NMR (400MHz, DMSO-d6) δ8.26(t,J=2.2Hz,1H),8.20(dd,J=5.6,3.3Hz,4H),8.09(d,J=8.0Hz,1H),8.00(ddd,J=6.0,3.5,2.0Hz,1H ),7.91–7.79(m,3H),7.74(dd,J=6.9,1.2Hz,1H),7.71–7.64(m,2H),7.51(dt,J=5.7,3.2Hz,6H),7.45–7.27(m,5H),1.54(s,12H).

[0165] Proton spectrum data of compound 49

[0166] 1 H NMR(400MHz, DMSO-d6)δ8.34–8.26(m,2H),8.19(td,J=7.0,6.4,2.4Hz,3H),8.04–7.95(m,2H),7.86–7.73(m,3H),7.68(td,J=4.3,1.4Hz,3H) ,7.62(ddd,J=7.4,4.0,2.5Hz,3H),7.59–7.53(m,2H),7.51(td,J=6.1 ,2.4Hz,5H),7.47–7.35(m,3H),7.32(s,2H),1.56(s,6H),1.51(s,6H).

[0167] Proton spectrum data of compound 107

[0168] 1 H NMR(400MHz,DMSO-d6)δ8.21–8.12(m,4H),8.09(dd,J=7.8,1.9Hz,2H),8.00(d ,J=8.0Hz,2H),7.96(ddd,J=5.7,3.3,2.0Hz,1H),7.88–7.78(m,3H),7.70–7.62 (m,3H),7.52(ddd,J=13.0,6.0,2.9Hz,3H),7.40(d,J=7.6Hz,1H),7.33–7.19(m ,6H),7.14(d,J=7.5Hz,1H),7.06(dd,J=7.2,1.7Hz,4H),1.64(d,J=1.3Hz,6H).

[0169] Proton spectrum data of compound 112

[0170] 1 H NMR (400MHz, DMSO-d6) δ8.15(d,J=1.9Hz,1H),8.03–7.98(m,1H),7.96(dt,J=9.1,2.3Hz,3H),7.90–7.83(m,3H),7.82–7.75(m,2H),7.59(dd,J=8 .0,1.6Hz,2H),7.51(dt,J=6.1,3.4Hz,2H),7.48–7.35(m,7H),7.32–7.2 1(m,6H),7.14(d,J=7.5Hz,1H),7.10–7.03(m,4H),1.41(d,J=1.2Hz,6H).

[0171] Proton spectrum data of compound 151

[0172] 1 H NMR (400MHz, DMSO-d6) δ8.33–8.27(m,2H),8.07–7.95(m,6H),7.92(ddd,J=5. 6,3.3,2.0Hz,1H),7.80–7.74(m,3H),7.70(ddd,J=9.8,7.8,2.2Hz,2H),7.51( dq,J=6.9,3.7Hz,3H),7.40(td,J=7.0,1.2Hz,1H),7.35(d,J=7.5Hz,1H),7.32 –7.20(m,6H),7.15(d,J=7.6Hz,1H),7.06(dd,J=7.2,1.7Hz,4H),1.55(s,6H).

[0173] Compound 187 1H spectroscopy data

[0174] 1 H NMR (400MHz, DMSO-d6) δ8.40(d,J=2.5Hz,1H),8.35(d,J=8.1Hz,1H),8.15(dt,J=5.3,2.5Hz,4H), 8.11(dd,J=6.5,2.1Hz,1H),8.03(t,J=2.2Hz,1H),7.99(dd,J=6.8,2.2Hz,1H),7.81(dd,J=7.8,4. 3Hz, 2H), 7.70 (ddd, J=12.5, 7.9, 2.3Hz, 2H), 7.58 (dd, J=7.6, 2.8Hz, 3H), 7.49 (dq, J=6.5, 3.2Hz, 7H),7.39(d,J=7.8Hz,1H),7.33(d,J=7.3Hz,1H),7.26(d,J=7.3Hz,1H),1.62(s,6H),1.55(s,6H).

[0175] The device implementation process is described as follows:

[0176] Based on the above compounds 1 to 188 being used as the main material of the light-emitting layer in the test device sample, the basic structure and preparation method of the device adopt conventional device preparation process technology, and the device structure schematic diagram is shown in Figure 1 As shown, the method for making the test device is specifically described as follows:

[0177] The schematic diagram of the test device structure of the experimental process of the present invention is introduced as follows: a polymer substrate 1, an anode layer 2 (ITO conductive glass), a hole injection layer 3 material (HIL), a hole transport layer 4 (HTL), an electron blocking layer 5 (EBL5), a light-emitting layer 6 (EML6), a hole blocking layer 7 (HBL), an electron transport layer 8 (ETL), an electron injection layer 9 (EIL), a cathode layer 10 (Mg (10%) -Ag (90%) alloy) and a high refractive index cover layer 11. Among them, one or a combination of two indenofluorene compounds 1 to 188 are used in the light-emitting layer (EML) to be used as the main light-emitting material for the evaluation experimental process. The detailed device preparation process is briefly described as follows:

[0178] A 0.5 mm thick ITO conductive glass is adhered to a polymer substrate with high mechanical strength, excellent thermal stability, excellent waterproofness and excellent transparency as an anode. The conductive glass is pretreated and cleaned in advance, and then different functional layers and organic functional layer materials with set thickness are sequentially evaporated according to the above structural characteristics. After the electron injection layer material is evaporated, a magnesium-silver alloy cathode is sputtered at a low temperature. After the cathode sputtering is completed, a layer of high refractive index covering layer material is evaporated to improve the refractive index of the cathode surface and increase the light extraction rate. Finally, the test device is packaged using conventional device test packaging methods to complete the entire production process of the test device.

[0179] The organic functional layer is distributed between the cathode and the anode, and specifically includes a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, and an electron injection layer; the first electrode and the second electrode are the anode and the cathode respectively, the light-emitting layer is located between the electron blocking layer and the hole blocking layer, and the light-emitting layer is prepared by mixed evaporation of a main light-emitting material and a guest light-emitting material, the main material is selected from one or a combination of two of indenofluorene compounds 1 to 188, the guest material is selected from one of DP-1, DP-2, and DP-3, and other functional layer materials are selected from corresponding functional layer materials with excellent cost-effectiveness in the industry to prepare test devices, and the compatibility between its functional layers needs to be determined through a series of tests and screening processes.

[0180] In addition, the first electrode can also be formed by sputtering or deposition on the substrate. The first electrode as the anode can be selected from oxide transparent conductive materials such as indium tin oxide (ITO), indium zinc oxide (IZO), tin dioxide (SnO2), zinc oxide (ZnO) and any combination thereof. The second electrode as the cathode can also be realized by metals or alloys such as magnesium (Mg), silver (Ag), aluminum (Al), aluminum-lithium (Al-Li), calcium (Ca), magnesium-indium (Mg-In), magnesium-silver (Mg-Ag) and their organic combinations.

[0181] The functional organic layer can be formed on the electrode by vacuum thermal evaporation, spin coating, printing and other means or methods. The compounds used as each organic layer except the light-emitting layer can be organic small molecules, organic macromolecules and polymers, and combinations thereof.

[0182] The light-emitting layer (EML) is constructed by a composite light-emitting layer, and the test device of the present invention adopts a host-guest combination. Similarly, a sensitizer material can be further added to further optimize the structure of the light-emitting layer. The light-emitting layer material is selected from any one or a combination of two of the compounds described in the present invention. The light-emitting layer is located between the above-mentioned electron blocking layer and the hole blocking layer. The preferred host light-emitting material is selected from any one or a combination of two of the indenofluorene compounds 1 to 188, and the host material and the guest material are used in a mass ratio of 95:5 to 99:1. After the functional layers are evaporated, they are finally packaged using a device packaging method commonly used in the industry. The sample used for the test device is prepared into a 30mm×30mm sample, and then the various luminescence performance indicators of the above sample are tested. Compared with the test device prepared with the existing commonly used host light-emitting material, the test device prepared with the preferred compound of the present invention has a better life when the luminescence brightness is consistent, and a higher brightness under the same test voltage.

[0183] The specific device preparation details are as follows:

[0184] Device Comparison Example 1:

[0185] The organic electroluminescent device was prepared by following the steps below:

[0186] like Figure 1As shown, the substrate layer 1 (polyethylene terephthalate (PET) plastic 1.5 mm); the anode layer 2 (indium tin oxide ITO 0.25 mm) is washed before use, that is, alkaline washing, pure water washing, drying, and then ultraviolet-ozone washing are performed in sequence to remove organic residues on the surface of the anode layer. On the anode layer 2 after the above washing, a hole injection layer 3 (HIL) with a thickness of 20 nm is evaporated by a vacuum evaporation device. The material of the hole injection layer 3 (HIL) can be selected from HI-1, HI-2 or HI-3 (HI-1 is selected in this test); then a hole transport layer 4 (HTL) with a thickness of 150 nm is evaporated. The material can be selected from HT-1, HT-2, HT-2, HT-3, HT-4, HT-5, HT-6 and HT-7 (HT-1 is selected in this test); then an electron blocking layer 5 (EBL) with a thickness of 30 nm is evaporated. The material is selected from one of EB-1, EB-2 and EB-3 (EB-1 is selected in this test); the light-emitting layer 6 (EML) is continuously evaporated on the electron blocking layer 5. The main material of the light-emitting layer is selected from one of EM-1, EM-2 and EM-3 (EM-1 is selected in this test embodiment), and the guest material is selected from one of DP-1, DP-2 and DP-3 (DP-1 is selected in this test embodiment), and the main material and The guest material is co-evaporated at a mass ratio of 98:2, and the thickness of the light-emitting layer is controlled to be 60nm; a 10nm thick hole blocking layer 7 (HBL) is continuously evaporated on the light-emitting layer, and the material is selected from one of HB-1 and HB-2 (HB-1 is selected in this embodiment); then a 30nm thick electron transport layer 8 (ETL) is continuously evaporated, and the material is selected from one of ET-1, ET-2, ET-3, ET-4, and ET-5 (ET-1 is selected in this embodiment); a 30nm thick electron injection layer 9 (EIL) is continuously evaporated on the electron transport layer 8, and the material is selected from one of EI-1, EI-2, and EI-3 (EI-1 is selected in this embodiment); after the electron injection layer 9 is evaporated, a 10nm thick Ag-Mg (Ag:Mg=9:1) alloy is sputtered as a cathode by low-temperature sputtering, and finally a 40nm thick covering layer 11 is continuously evaporated on the cathode, and the material is selected from CP-1; finally, the above functional layers are vacuum packaged, and the device is prepared.

[0187] The device comparative examples 2 to 3 were prepared in the same manner as in comparative example 1, except that the guest materials were DP-2 (comparative example 2) and DP-3 (comparative example 3), respectively, and the other functional layers remained the same;

[0188] Device Comparative Examples 4 to 5 are also prepared by referring to the preparation process of Device Comparative Example 1, except that the main material EM-1 is replaced by EM-2 (Comparative Example 4) and EM-3 (Comparative Example 5), and other functional layers remain the same.

[0189] Embodiments of the present invention

[0190] Embodiment 1~embodiment 6:

[0191] The device preparation process is carried out according to the method of device comparison example 1, except that the preferred compound described in the present invention is used as the main material of the light-emitting layer to prepare the device, and the matching guest material is DP-1. The corresponding compounds used in the examples are compound 3, compound 10, compound 49, compound 112, compound 151, and compound 187.

[0192] Embodiment 7~embodiment 10:

[0193] The device preparation process is carried out according to the method of device comparative example 1, except that the preferred compounds described in the present invention are used as the main materials of the light-emitting layer for device preparation, and compound 3, compound 10, compound 49, and compound 151 are selected respectively; DP-2 is selected as the guest material.

[0194] Embodiment 11~embodiment 14:

[0195] The device preparation process is carried out according to the method of device comparative example 1, except that the preferred compounds described in the present invention are used as the main materials of the light-emitting layer to prepare the device, and compound 3, compound 10, compound 49, and compound 151 are selected respectively; DP-3 is selected as the guest material.

[0196] The structure of each functional layer of the above-mentioned test device is summarized in Table 3 below:

[0197] Part Number Luminescent layer main body Light-emitting layer guest Percentage of object materials Comparative Example 1 EM-1 DP-1 2% Comparative Example 2 EM-1 DP-2 2% Comparative Example 3 EM-1 DP-3 2% Comparative Example 4 EM-2 DP-1 2% Comparative Example 5 EM-3 DP-1 2% Example 1 Compound 3 DP-1 2% Example 2 Compound 10 DP-1 2% Example 3 Compound 49 DP-1 2% Example 4 Compound 112 DP-1 2% Example 5 Compound 151 DP-1 2% Example 6 Compound 187 DP-1 2% Example 7 Compound 3 DP-2 2% Example 8 Compound 10 DP-2 2% Example 9 Compound 49 DP-2 2% Example 10 Compound 151 DP-2 2% Embodiment 11 Compound 3 DP-3 2% Example 12 Compound 10 DP-3 2% Embodiment 13 Compound 49 DP-3 2% Embodiment 14 Compound 151 DP-3 2%

[0198] The functional layer materials involved in the above device preparation process can be selected from one or more combinations of corresponding related functional layer materials. During the device implementation process, the specific functional layer structures are introduced as follows:

[0199] The HIL functional layer can be selected from one or more of the following HI-1 to HI-3:

[0200]

[0201] The HTL functional layer can be selected from one or more of the following HT-1 to HT-7:

[0202]

[0203] The EBL functional layer is selected from one or more of the following EB-1 to EB-3:

[0204]

[0205] EML functional layer material: The comparative material uses one of the following EM-1 to EM-3 as the main material, and the embodiment of the present invention uses one or more of compounds 1 to 188 as the main material; the guest material uses one of DP-1 to DP-3:

[0206]

[0207]

[0208] The HBL functional layer material is selected from one or two of the following HB-1 and HB-2:

[0209]

[0210] The ETL functional layer material is selected from one or more of the following ET-1 to ET-5:

[0211]

[0212] The EIL functional layer can be selected from one or more of the following EI-1 to EI-3:

[0213]

[0214] The covering material is selected as follows CP-1:

[0215]

[0216] The performance test data of the multilayer composite structure test device and the control device prepared by using the compound of the present invention are summarized in the following test device result summary table 4:

[0217] Table 4

[0218]

[0219]

[0220] (Note: SM is the abbreviation of the compound)

[0221] As shown in Table 4 above, from the test data, under the same device manufacturing process conditions, the device performance was tested under the same current density conditions. Compared with the traditional main materials EM-1, EM-2, and EM-3, the test device prepared by using the preferred compound of the present invention as the main material of the light-emitting layer has a current efficiency increased by more than 30%, and the LT95 life of the device is increased by nearly 30%. This shows that: the test device prepared by using the preferred compound of the present invention as the main light-emitting material has a significantly improved device life and a significantly improved comprehensive luminous efficiency.

[0222] From the above experimental results, it can be seen that the present invention effectively connects the indenofluorene main structure with the advantageous fragments of the traditional fluorescent main body. When this type of material is used as the main light-emitting material, its excellent performance is due to its larger spatial stereo configuration and relatively fixed orientation, thereby obtaining a sufficiently high glass transition temperature, good device film forming properties and higher device stability.

[0223] The indenofluorene structure main body designed by the present invention has high structural stability. Firstly, the 9-position (R1, R2 or R3, R4 substitution position) of fluorene is effectively substituted to increase the spatial rigidity of the entire molecule. Secondly, the main structure is effectively connected with a common fluorescent main material structure fragment (B). In this way, the conventional fluorescent main material structure is effectively transformed, and the efficient fluorescent luminescence efficiency of the conventional fluorescent main structure is retained. The stability of the traditional fluorescent main material in terms of the spatial structure is further improved, so that the device life is further extended.

[0224] The present invention introduces an indenofluorene structure with a high triplet energy level, which can further improve the triplet energy level of the fluorescent main light-emitting body after being adapted to the traditional fluorescent main structure. When this type of material is used as a main material, it can more efficiently transmit and transfer the energy of its triplet excitons to the matching guest material, thereby greatly improving the luminous efficiency of the light-emitting layer.

[0225] The indenofluorene derivatives designed in the present invention have a large spatial stereo configuration. In addition to having a high glass transition temperature, the molecules have a significant asymmetric configuration and excellent film-forming properties during molecular evaporation, which significantly improves the luminescence consistency, thereby effectively improving the device yield.

[0226] The designed material of the present invention has good compatibility with the traditional high-efficiency fluorescent main body core structure, has little impact on the application matching mode of the above-mentioned traditional main body core structure, and is conducive to the rapid application of the material to the existing mature fluorescent main body material application scenarios.

[0227] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

[0228] Many other changes and modifications may be made without departing from the concept and scope of the present invention.It should be understood that the present invention is not limited to the specific embodiments, and the scope of the present invention is defined by the appended claims.

Claims

1. An indenofluorene derivative, It is characterized in that The general structural formula of the indenofluorene derivative is shown in the following general formula 1: in: A is selected from C 5 ~C 15 The aromatic condensed ring, A and the main structure are bonded by a single bond or a ring-joined bond; B is selected from phenyl, naphthyl, anthracenyl, phenanthrenyl and C 5 ~C 20 Aromatic fused ring or aromatic fused heterocyclic ring, B is bonded to the main structure by a single bond; R 1 ,R 2 ,R 3 ,R 4 are independently selected from H, deuterium, C 1 ~C 5 Alkyl, C 5 ~C 15 R 5 ,R 6 are independently selected from H, deuterium, C 3 ~C 15 Alkyl, C 6 ~C 20 The aromatic group, C 5 ~C 20 The heterocyclic aromatic group.

2. An indenofluorene derivative according to claim 1, It is characterized in that The general formula 1 includes general formulas 2-1, 2-2, 2-3, 2-4 and 2-5, and the specific structural formulas are as follows: in: B is selected from phenyl, naphthyl, anthracenyl, phenanthrenyl and C 5 ~C 20 Aromatic fused ring or aromatic fused heterocyclic ring, B is bonded to the main structure by a single bond; R 1 ,R 2 ,R 3 ,R 4 are independently selected from H, deuterium, C 1 ~C 5 Alkyl, C 5 ~C 15 R 5 ,R 6 are independently selected from H, deuterium, C 3 ~C 15 Alkyl, C 6 ~C 20 The aromatic group, C 5 ~C 20 The heterocyclic aromatic group.

3. An indenofluorene derivative according to any one of claims 1 to 2, It is characterized in that The indenofluorene derivatives include compounds 1 to 188, and the specific structural formulas are as follows:

4. An electroluminescent device comprising a first electrode, a second electrode and an organic layer located between the first electrode and the second electrode, Features: The organic layer comprises a combination of any one or more of the indenofluorene derivative compounds 1 to 188 described in claim 3.

5. An electroluminescent device according to claim 4, Features: The organic layer includes a hole transport layer, a light emitting layer and an electron transport layer, wherein the light emitting layer comprises a combination of one or more of compounds 1 to 188.

6. An electroluminescent device according to claim 5, Features: The light-emitting layer is composed of a host material and a guest material, wherein the ratio of the host material to the guest material is 95:5 to 99:

1.

7. An electroluminescent device according to claim 6, Features: The ratio of the host material to the guest material is 98:

2.

8. An electroluminescent device according to claim 6, Features: The host material is selected from one or a combination of two of compounds 1 to 188, and the guest material is selected from

Citation Information

Cited By

  • Triphenylmethyl fused ring derivative and electroluminescent device thereof

    CN119176790A

  • A trityl condensed ring derivative and electroluminescent device thereof

    CN119176790B