Tyre comprising tread
By using a specific rubber composition in the tire, including solution polymerized styrene butadiene rubber, carbon black and terpene resin, the performance differences and grip issues of the tire under different temperature states are solved, achieving more consistent performance and Higher dry grip.
Patent Information
- Application Number
- CN202410366886.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
There is a significant difference in the performance of existing tires in a cooling state and a warming state, and it is difficult to maintain high grip in dry conditions, affecting driving performance.
Improved performance using a rubber composition comprising 80 phr to 100 phr of solution polymerized styrene butadiene rubber, 80 phr to 200 phr of carbon black filler, 10 phr to 100 phr of a liquid diene based polymer, and 10 phr to 80 phr of a terpene resin. Tire heating behavior and dry grip.
Significantly improves the performance consistency of the tire, bringing the performance in the cooling state close to the heating state, improving dry grip, shortening the tire heating time, and improving the overall driving performance.
Smart Images

Figure CN118725432A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a tire, preferably a motorcycle tire. Background Art
[0002] Although considerable progress has been made in improving the performance of sports tires, such as those for motorcycles and passenger cars, it is still observed in some cases that the performance of the tire may differ significantly between a cold state of the tire (in which the tire, for example, has only ambient temperature) and a warmed-up state of the tire. In particular, it would be desirable to provide a tire having more consistent performance between such cold and warmed-up states. Furthermore, it may be desirable to reach the warmed-up state more quickly and / or to improve the overall grip level. Summary of the invention
[0003] It may be an object of the present invention to provide a tire, preferably one or more of a motorcycle tire, a race tire or a slick tire, having an improved warming behavior while driving.
[0004] Another object of the present invention may be to provide a tire having improved performance consistency as the tire warms up.
[0005] Yet another object of the present invention may be to provide a tire having improved dry performance.
[0006] The invention is defined by the appended claim 1. Further preferred embodiments are provided in the dependent claims and in the following summary of the invention.
[0007] Thus, in a first aspect, the present invention is directed to a tire having a tread, wherein the tread comprises a rubber composition comprising 80 to 100 phr of one or more solution-polymerized styrene butadiene rubbers; 80 to 200 phr of a filler comprising at least 40 phr of carbon black; 10 to 100 phr of one or more liquid diene-based polymers; and 10 to 80 phr of a terpene resin.
[0008] Surprisingly, the inventors have found that the use of terpene resins in such rubber compositions significantly improves warm-up behavior and dry grip. The same behavior is not observed using different resin types. In particular, the tires show better performance consistency. In other words, the driving performance of the tire in the unwarmed or cooled state is closer to the performance of the tire in the warmed state.
[0009] In one embodiment, the one or more solution polymerized styrene butadiene rubbers have a glass transition temperature in the range of -1°C to -45°C, preferably -4°C to -40°C.
[0010] In another embodiment, the filler comprises one or more of the following: 80 to 150 phr of carbon black (preferably, 90 to 130 phr); primarily carbon black; carbon black having an iodine value (or in other words, iodine absorption value) of at least 180 g / kg, preferably at least 190 or 200 g / kg, and optionally up to 250 g / kg as determined by ASTM D1510 or equivalent; less than 20 phr of silica (preferably less than 10 phr or less than 5 phr of silica).
[0011] In yet another embodiment, the rubber composition comprises 15 phr to 45 phr of a terpene resin, preferably 15 phr to 30 phr, or to 25 phr of a terpene resin.
[0012] In yet another embodiment, the resin is a terpene resin based on α-pinene.
[0013] In yet another embodiment, the resin has one or more of the following: a softening point in the range of 100°C to 150°C, preferably 105°C to 140°C; a glass transition temperature in the range of 50°C to 100°C, preferably 60°C to 90°C; a weight average molecular weight (Mw) in the range of 200 g / mol to 900 g / mol, preferably 300 g / mol to 600 g / mol; an aromatic proton content (as a percentage of all protons in the resin, as known in the art), less than 5%, preferably less than 2% or less than 1%.
[0014] In yet another embodiment, the rubber composition further comprises 5 to 70 phr of oil, preferably 20 to 70 phr, or 25 to 60 phr of oil.
[0015] In yet another embodiment, the rubber composition comprises 95 to 100 phr of one or more solution polymerized styrene butadiene rubbers. The rubber composition may also comprise greater than 99 phr of such rubbers or even 100 phr of those.
[0016] In yet another embodiment, the rubber composition further comprises 1 to 10 phr (preferably 2 to 8 phr) of an alkylphenol resin, optionally having a softening point in the range of 120°C to 170°C.
[0017] In yet another embodiment, the liquid (diene-based) polymer has one or more of the following: a glass transition temperature in the range of -1°C to -30°C; a number average molecular weight in the range of 2000 g / mol to 15000 g / mol (preferably in the range of 2000 g / mol to 10000 g / mol); one or more (preferably two types) of butadiene repeating units and styrene repeating units; a homopolymer structure (in other words, no block structure, in particular no diblock structure).
[0018] "Liquid" herein refers to a material which has a liquid state at a temperature of 23°C.
[0019] Liquid polymers are available, for example, from Cray Valley Corporation under the trade name Ricon TM Get, for example, Ricon TM 100 or Ricon TM 184, etc. Typical styrene content is 17% to 27% and / or vinyl content is 20% to 75% RHC.
[0020] In yet another embodiment, the rubber composition comprises less than 5 phr (preferably less than 1 phr) of coumarone-indene resin, or is free of such resin.
[0021] In yet another embodiment, the tire is a motorcycle tire. Although the rubber composition of the present invention may be particularly suitable for motorcycle tires and / or motorcycle racing tires, such as slick tires, the composition may also be used in other tires, such as automobile tires and / or automobile racing tires, such as slick tires.
[0022] In another embodiment, the tread has two tread shoulders and a tread center portion between the two tread shoulders, and wherein at least one of the tread shoulders comprises the rubber composition. Optionally, the tread center portion is substantially free of the rubber composition. Preferably, both tread shoulders comprise the rubber composition.
[0023] In yet another embodiment, the tread center portion comprises a different rubber composition than the at least one tread shoulder portion, and wherein the rubber composition of the tread center portion has a wear resistance that is at least 5% (preferably 10%) higher than the rubber composition of the at least one tread shoulder portion. Abrasion resistance is measured herein according to ASTM D412 or equivalent at 23°C with a ring specimen at 300% modulus (M300).
[0024] In another embodiment, the tire is one or more of the following: a motorcycle tire; a motorcycle racing tire; a motorcycle rear tire; a slick tire; a pneumatic tire; a tire without grooves completely surrounding the tire in the circumferential direction; a motorcycle tire comprising two (fabric reinforced, e.g. reinforced with polyamide or in particular nylon) breaker plies radially covered by at least one helically wound (fabric and / or cord reinforced, e.g. comprising aromatic polyamide) ply strip; a motorcycle tire comprising a split tread comprising at least two circumferential tread shoulders comprising the rubber composition (or the first rubber composition) and a circumferential tread center portion comprising another (second) rubber composition, wherein the two rubber compositions are different from each other.
[0025] In yet another embodiment, the tire has two tread shoulders, each of which has a tread cap shoulder (or layer) and a tread base shoulder (or layer) below the respective tread cap shoulder (or layer), and wherein the tread cap shoulder (or layer) comprises the rubber composition.
[0026] In yet another embodiment, the tread base shoulder (or layer) has a base rubber composition having a stiffness G'(1%) that is at least 5% (preferably at least 10%) lower than the rubber composition of the tread cap shoulder (or layer). The stiffness G'(1%) is measured herein based on ASTM D5289 or equivalent using a RubberProcess Analyzer from Alpha Technologies at a given strain percentage, a temperature of 100°C and a frequency of 1 Hz.
[0027] In yet another embodiment, a tread center portion is disposed between the two tread shoulders, wherein the tread center portion has a center portion rubber composition having at least 5% (preferably at least 10%) higher wear resistance than the rubber composition of the tread cap shoulders.
[0028] In a preferred embodiment, the tire is a motorcycle tire, such as a motorcycle slick tire and / or a motorcycle rear tire.
[0029] In one embodiment, the rubber composition comprises at least one and / or one additional diene-based rubber. Representative synthetic polymers can be butadiene and its homologues and derivatives, such as homopolymerization products of methylbutadiene, dimethylbutadiene and pentadiene, and copolymers, such as those formed by butadiene or its homologues or derivatives with other unsaturated monomers. Other unsaturated monomers can be acetylene, such as vinylacetylene; olefins, such as isobutylene, which is copolymerized with isoprene to form butyl rubber; vinyl compounds, such as acrylic acid, acrylonitrile (which is polymerized with butadiene to form NBR), methacrylic acid and styrene (the latter compound is polymerized with butadiene to form SBR), and vinyl esters and various unsaturated aldehydes, ketones and ethers, such as acrolein, methylisopropenyl ketone and vinyl ethyl ether. Specific examples of synthetic rubbers include chloroprene rubber (polychloroprene), polybutadiene (including cis-1,4-polybutadiene), polyisoprene (including cis-1,4-polyisoprene), butyl rubber, halogenated butyl rubber such as chlorobutyl rubber or bromobutyl rubber, styrene / isoprene / butadiene rubber, 1,3-butadiene or isoprene with monomers such as styrene, acrylonitrile and methyl methacrylate The copolymer and ethylene / propylene terpolymer, also known as ethylene / propylene / diene monomer (EPDM), particularly ethylene / propylene / dicyclopentadiene terpolymer. Other examples of rubbers that can be used include alkoxy-silyl terminal functionalized solution polymerized polymers (SBR, PBR, IBR and SIBR), silicon-coupled and tin-coupled star-branched polymers. Preferred rubbers or elastomers can generally be natural rubber, synthetic polyisoprene, polybutadiene and SBR (including SSBR).
[0030] In another embodiment, within the limits of claim 1, the composition may include at least two diene-based rubbers. For example, combinations of two or more rubbers are preferred, such as cis-1,4-polyisoprene rubber (natural or synthetic, but natural rubber is preferred), 3,4-polyisoprene rubber, styrene / isoprene / butadiene rubber, emulsion and solution polymerization derived styrene / butadiene rubber, cis-1,4-polybutadiene rubber, and emulsion polymerization prepared butadiene / acrylonitrile copolymers.
[0031] In another embodiment, an emulsion polymerization derived styrene / butadiene (ESBR) having a styrene content of 20% to 28% bound styrene may be used, or for some applications, an ESBR having a medium to relatively high bound styrene content, i.e., 30% to 45% bound styrene content, may be used. In many cases, the ESBR has a bound styrene content in the range of 26% to 31%. ESBR prepared by emulsion polymerization may refer to styrene and 1,3-butadiene as aqueous emulsion copolymers. This is well known to those skilled in the art. The bound styrene content may vary, for example, from 5% to 50%. In one aspect, the ESBR may also contain acrylonitrile to form a terpolymer rubber in the form of ESBAR, the amount of bound acrylonitrile in the terpolymer being, for example, 2 to 30% by weight. It is also contemplated that a styrene / butadiene / acrylonitrile copolymer rubber prepared by emulsion polymerization containing 2 to 40% by weight bound acrylonitrile in the copolymer may be used as a diene-based rubber.
[0032] In another embodiment, the SBR prepared by solution polymerization (solution polymerized styrene butadiene rubber (SSBR)) may have a combined styrene content of 5% to 50%, preferably 30% to 45% herein. SSBR can be conveniently prepared, for example, by anionic polymerization in an inert organic solvent. More specifically, SSBR can be synthesized by copolymerizing styrene with 1,3-butadiene monomers using an organic lithium compound as an initiator in a hydrocarbon solvent. In yet another embodiment, the solution styrene butadiene rubber is a tin-coupled polymer. In yet another embodiment, the SSBR is functionalized to improve compatibility with silica. In addition, or alternatively, the SSBR is sulfur-functionalized (thio-functionalized). This helps to improve the stiffness and / or its hysteresis behavior of the rubber compound. Therefore, for example, the SSBR can be a copolymer of sulfur-functionalized, tin-coupled solution-polymerized butadiene and styrene. However, as another option, the SSBR can have any other functionalization known in the art, such as amino, alkoxy, carboxyl, siloxy, hydroxyl and / or other functionalizations.
[0033] In one embodiment, in addition to SSBR, synthetic or natural polyisoprene rubber may be used. Synthetic cis-1,4-polyisoprene and natural rubber are well known to those skilled in the art of rubber. In particular, the cis-1,4-microstructure content may be at least 90%, and typically at least 95% or even higher.
[0034] In one embodiment, in addition to SSBR, cis-1,4-polybutadiene rubber (BR or PBD) is used. Suitable polybutadiene rubbers can be prepared, for example, by organic solution polymerization of 1,3-butadiene. BR can conveniently be characterized, for example, by having at least 90% cis-1,4-microstructure content ("high cis" content) and a glass transition temperature (Tg) in the range of -95°C to -110°C. Suitable polybutadiene rubbers are commercially available, for example from The Goodyear Tire & Rubber Company. 1207, 1208, 1223 or 1280. These high cis-1,4-polybutadiene rubbers can be synthesized, for example, using a nickel catalyst system comprising a mixture of (1) an organonickel compound, (2) an organoaluminum compound, and (3) a fluorine-containing compound, as described in U.S. Pat. No. 5,698,643 and U.S. Pat. No. 5,451,646, which are incorporated herein by reference.
[0035] The glass transition temperature or Tg of an elastomer refers to the glass transition temperature of the corresponding elastomer in its uncured state. The glass transition temperature of an elastomeric composition refers to the glass transition temperature of the elastomeric composition in its cured state. Tg is determined by differential scanning calorimetry (DSC) at a heating rate of 20°C / min as the peak midpoint according to ASTM D3418 or equivalent.
[0036] As used herein, and in accordance with conventional practice, the term "phr" means "parts by weight of the respective material per 100 parts by weight of rubber or elastomer". Typically, using this convention, a rubber composition comprises 100 parts by weight of rubber / elastomer. The claimed composition may contain other rubbers / elastomers in addition to those explicitly mentioned in the claims, provided that the phr value of the claimed rubber / elastomer complies with the claimed phr range and the amount of all rubbers / elastomers in the composition results in a total of 100 parts of rubber. In one example, the composition may also contain 1 phr to 10 phr, optionally 1 phr to 5 phr of one or more additional diene-based rubbers, such as SBR, SSBR, ESBR, PBD / BR, NR and / or synthetic polyisoprene. In another example, the composition may contain less than 5 phr, preferably less than 3 phr of additional diene-based rubber, or may also be substantially free of such additional diene-based rubber. Unless otherwise indicated, the terms "rubber" and "composition" and "formulation" are used interchangeably herein. The terms "rubber" and "elastomer" are also used interchangeably herein.
[0037] Gel permeation chromatography (GPC) is used herein to determine the molecular weight of elastomers / rubbers, such as Mn (number average molecular weight), Mw (weight average molecular weight), and Mz (z average molecular weight), according to ASTM 5296-11 using polystyrene calibration standards, or equivalent.
[0038] The Tg of the resin is determined by differential scanning calorimetry (DSC) at a heating rate of 10°C / min as the peak midpoint according to ASTM D6604 or equivalent. Preferably, the resin has a softening point above 70°C as determined by ASTM E28, which may sometimes be referred to as the ring and ball softening point.
[0039] In another embodiment, the additional resin is selected from coumarone-indene resins (less preferred or preferred even completely omitted), petroleum hydrocarbon resins, terpene polymers / resins, styrene / α-methylstyrene resins, terpene phenol resins, rosin-derived resins and copolymers and / or mixtures thereof.
[0040] The coumarone-indene resin preferably contains coumarone and indene as monomer components constituting the resin backbone (main chain). Monomer components other than coumarone and indene that can be incorporated into the backbone are, for example, methylcoumarone, styrene, α-methylstyrene, methylindene, vinyltoluene, dicyclopentadiene, cyclopentadiene, and dienes such as isoprene and piperlyene. The coumarone-indene resin preferably has a softening point (as measured by the ball-and-ring method) of 10° C. to 160° C. Even more preferably, the softening point is 30° C. to 100° C.
[0041] Suitable petroleum resins include aromatic and non-aromatic types. Several types of petroleum resins are available. Some resins have low unsaturation and high aromatic content, while some resins are highly unsaturated, and some resins do not contain aromatic structures at all. The difference in resins is largely due to the olefins in the raw materials from which the resins are derived. Conventional derivatives in such resins include any C5 species (olefins and dienes containing an average of five carbon atoms), such as cyclopentadiene, dicyclopentadiene, dienes such as isoprene and piperylene, and any C9 species (olefins and dienes containing an average of 9 carbon atoms), such as vinyl toluene, α-methylstyrene and indene. Such resins are made from any mixture of the above-mentioned C5 species and C9 species, and are referred to as C5 / C9 copolymer resins. The softening point of petroleum resins is generally 10°C to 120°C. Preferably, the softening point is 30 to 100°C.
[0042] In one embodiment, the C5 resin is an aliphatic resin made from one or more of the following monomers: 1,3-pentadiene (eg, cis or trans), 2-methyl-2-butene, cyclopentene, cyclopentadiene, and dicyclopentadiene.
[0043] In another embodiment, the C9 resin is a resin made from one or more aromatic monomers, preferably selected from the group consisting of indene, methylindene, vinyltoluene, styrene, and methylstyrene (eg, alpha-methylstyrene).
[0044] In yet another embodiment, the C9 modified resin is a resin (eg, a C5 resin) that has been modified or functionalized with one or more aromatic monomers, preferably selected from indene, methylindene, vinyltoluene, styrene, and methylstyrene (eg, α-methylstyrene).
[0045] The terpene resin preferably contains a polymer of at least one of limonene, α-pinene, β-pinene, and δ-3-carene.
[0046] Terpene-phenol resins can be obtained by copolymerization of phenolic monomers with terpenes such as limonene, pinene and delta-3-carene.
[0047] Representative examples of resins derived from rosin and its derivatives are, for example, gum rosin, wood rosin and tall oil rosin. Gum rosin, wood rosin and tall oil rosin have similar compositions, although the amounts of the components of the rosin may vary. Such resins may be dimerized, polymerized or disproportionated. Such resins may be in the form of esters of rosin acid and polyols such as pentaerythritol or diols.
[0048] Styrene / α-methylstyrene resins are considered herein to be (preferably relatively short chain) copolymers of styrene and α-methylstyrene, wherein the styrene / α-methylstyrene molar ratio is from about 0.05 to about 1.50. In one aspect, such resins can be suitably prepared, for example, by cationic copolymerization of styrene and α-methylstyrene in a hydrocarbon solvent. Thus, a contemplated styrene / α-methylstyrene resin can be characterized, for example, by its chemical structure, i.e., its styrene and α-methylstyrene content, and by its glass transition temperature, molecular weight, and molecular weight distribution.
[0049] In one embodiment, the resin is partially or fully hydrogenated.
[0050] In one embodiment, the rubber composition includes oil, such as processing oil. Oil can be included in the rubber composition as an extender oil commonly used for extending elastomers. Oil can also be included in the rubber composition by directly adding oil during rubber compounding. The oil used can include both the extender oil present in the elastomer and the (processing) oil added during compounding. Suitable oil can include various oils known in the art, including aromatic oils, paraffin oils, naphthenic oils, vegetable oils and low PCA oils, such as MES, TDAE, SRAE and heavy naphthenic oils. Suitable low PCA oils can include those with polycyclic aromatic content less than 3 weight % as measured by IP346 method. The procedure of IP346 method can be found in Standard Methods for Analysis & Testing of Petroleum and Related Products and British Standard 2000 Parts, 2003, the 62nd edition published by the Institute of Petroleum, United Kingdom. Some representative examples of vegetable oils that can be used include soybean oil, sunflower oil, canola (rapeseed) oil, corn oil, coconut oil, cottonseed oil, olive oil, palm oil, peanut oil, and safflower oil. Soybean oil and corn oil are generally preferred vegetable oils.
[0051] The glass transition temperature, Tg, of the oil is determined by differential scanning calorimetry (DSC) at a heating rate of 10°C / min as the peak midpoint according to ASTM E1356 or equivalent.
[0052] In one embodiment, the rubber composition comprises silica. The silica can be, for example, pyrolytic / gas phase or precipitated silica. In a preferred embodiment, precipitated silica is used. The silica can be, for example, characterized by having a BET surface area as measured using nitrogen. In one embodiment, the BET surface area can be in the range of 40 to 600 square meters per gram. In another embodiment, the BET surface area can be in the range of 50 to 300 square meters per gram. The BET surface area is determined according to ASTM D6556 or an equivalent and is described in Journal of the American Chemical Society, Vol. 60, p. 304 (1930). The silica can also be characterized by having a 100 cm surface area as measured according to ASTM D 2414 or an equivalent. 3 / 100g to 400cm 3 / 100g, or 150cm 3 / 100g to 300cm 3The silica may have an average final particle size in the range of 0.01 to 0.05 micrometers, for example, as determined by electron microscopy, but the size of the silica particles may be even smaller or possibly larger. Various commercially available silicas may be used, such as, by way of example only and without limitation, silicas available from PPG Industries under the Hi-Sil trademark, with designations 210, 315G, EZ160G, etc.; silicas available from Solvay, such as designations Z1165MP and Premium200MP, etc.; and silicas available from Evonik AG, such as designations VN2 and Ultrasil 6000GR, 9100GR, etc.
[0053] In another embodiment, the rubber composition may include pre-silanized and / or hydrophobized silica, which may have a molecular weight of, for example, 130 m 2 / g to 210m 2 / g, optional 130m 2 / g to 150m 2 / g and / or 190m 2 / g to 210m 2 / g, or even 195m 2 / g to 205m 2 The CTAB (cetyltrimethylammonium bromide) method (ASTM D6845) for determining the surface area of silica is known to those skilled in the art.
[0054] Some non-limiting examples of pretreated silicas (i.e., silicas that have been pre-surface treated with silanes) suitable for use in the practice of the present invention include, but are not limited to, silicas that have been pre-treated with mercaptosilanes. 255LD and LP (PPG Industries) silica, and as an organosilane bis (triethoxysilylpropyl) polysulfide (Si69) and The reaction product between VN3 and silica 8113(Degussa), and 6508, from PPG Industries 400 Silica, from PPG Industries 454 silica, and from PPG Industries 458Silicon dioxide.
[0055] In one embodiment, carbon black comprises one or more of N110, N121, N134, N191, N220, N231, N234, N242, N293, N299, N315, N326, N330, N332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990 and N991 grades. It may also include one or more other grades not listed herein. Carbon black has different iodine absorption values / numbers, which are measured according to ASTM D1510 or equivalent.
[0056] In one embodiment, the rubber composition may contain a sulfur-containing organosilicon compound or silane. Examples of suitable sulfur-containing organosilicon compounds have the following formula:
[0057] Z-Alk-S n -Alk-Z I
[0058] Where Z is selected from
[0059]
[0060] Where R 1 is an alkyl group of 1 to 4 carbon atoms, a cyclohexyl group or a phenyl group; R 2 is an alkoxy group of 1 to 8 carbon atoms, or a cycloalkoxy group of 5 to 8 carbon atoms; Alk is a divalent hydrocarbon of 1 to 18 carbon atoms; and n is an integer of 2 to 8. In one embodiment, the sulfur-containing organosilicon compound is 3,3'-bis(trimethoxy or triethoxysilylpropyl)polysulfide. In one embodiment, the sulfur-containing organosilicon compound is 3,3'-bis(triethoxysilylpropyl)disulfide and / or 3,3'-bis(triethoxysilylpropyl)tetrasulfide. Therefore, for Formula I, Z can be
[0061]
[0062] Where R 2 is an alkoxy group of 2 to 4 carbon atoms, or 2 carbon atoms; Alk is a divalent hydrocarbon of 2 to 4 carbon atoms, or 3 carbon atoms; n is an integer of 2 to 5, or 2 or 4. In another embodiment, suitable sulfur-containing organosilicon compounds include compounds disclosed in U.S. Pat. No. 6,608,125. In one embodiment, the sulfur-containing organosilicon compound includes 3-(octanoylthio)-1-propyltriethoxysilane, CH3(CH2)6C(=O)-S-CH2CH2CH2Si(OCH2CH3)3, which can be used as NXT TMAvailable from Momentive Performance Materials. In another embodiment, suitable sulfur-containing organosilicon compounds include those disclosed in U.S. Patent Application Publication No. 2003 / 0130535. In one embodiment, the sulfur-containing organosilicon compound is Si-363 from Degussa. The amount of the sulfur-containing organosilicon compound in the rubber composition can vary depending on the level of other additives used. Generally speaking, in one embodiment, the amount of the compound can be 0.5phr to 10phr, but preferably exists at most 4phr, because the composition of the present invention preferably contains only a limited amount of silica or no silica at all.
[0063] It is readily understood by those skilled in the art that rubber composition can be compounded by methods known in the rubber compounding field, for example, various sulfur-vulcanizable component rubbers are mixed with various common additive materials, such as sulfur donors, curing aids such as activators and scorch retarders and processing additives such as oils, resins (including tackifying resins) and plasticizers, fillers, pigments, fatty acids, zinc oxide, waxes, antioxidants and antiozonants and peptizing agents (peptizing agents). As known to those skilled in the art, according to the intended use of sulfur-vulcanizable and sulfur-vulcanized materials (rubber), the above-mentioned additives are selected and usually used in conventional amounts. Some representative examples of sulfur donors include elemental sulfur (free sulfur), disulfide amines (amine disulfide), polymerized polysulfide and sulfur olefin adducts. In one embodiment, sulfur-vulcanizing agent is elemental sulfur. Sulfur-vulcanizing agent can be used, for example, with an amount in the range of 0.5phr to 8phr, or 1.5phr to 6phr. If a tackifying resin is used, a typical amount thereof includes, for example, 0.5 phr to 10 phr, typically 1 phr to 5 phr. If a processing aid is used, a typical amount thereof includes, for example, 1 phr to 50 phr (this may particularly include oils). If an antioxidant is used, a typical amount thereof may, for example, include 1 phr to 5 phr. Representative antioxidants may be, for example, diphenyl-p-phenylenediamine and others, such as those disclosed in The Vanderbilt Rubber Handbook (1978), pages 344-346. If an antiozonant is used, a typical amount thereof may, for example, include 1 phr to 5 phr. If a fatty acid (which may include stearic acid) is used, a typical amount thereof may, for example, include 0.5 phr to 3 phr. If a wax is used, a typical amount thereof may, for example, include 1 phr to 5 phr. Microcrystalline wax is typically used. If a peptizing agent is used, a typical amount thereof may, for example, include 0.1 phr to 1 phr. Typical peptizing agents may be, for example, pentachlorothiophenol and dibenzamidodiphenyl disulfide.
[0064] It is preferred but not necessary to use an accelerator to control the time and / or temperature required for vulcanization, and to improve the properties of the vulcanizate. In one embodiment, a single accelerator system, i.e., a primary accelerator, can be used. The total amount of (one or more) primary accelerators can be 0.5phr to 4phr, or 0.8phr to 1.5phr. In another embodiment, a combination of a primary accelerator and an auxiliary accelerator can be used, and the auxiliary accelerator is used in a smaller amount, such as 0.05phr to 3phr, to activate and improve the properties of the vulcanizate. The combination of these accelerators can be expected to produce a synergistic effect on the final properties, and to a certain extent, the effect produced by using any accelerator alone is better. In addition, a delayed-acting accelerator that is not affected by normal processing temperature but produces satisfactory curing at conventional vulcanization temperatures can be used. Vulcanization retardants can also be used. Accelerators of suitable types that can be used in the present invention are, for example, amines, disulfides, guanidines, thioureas, thiazoles, thiurams, sulfonamides, dithiocarbamates, and xanthates. In one embodiment, the primary accelerator is a sulfonamide. If a secondary accelerator is used, it can be, for example, a guanidine, dithiocarbamate or thiuram compound. Suitable guanidines include diphenylguanidine and the like. Suitable thiurams include tetramethylthiuram disulfide, tetraethylthiuram disulfide and tetrabenzylthiuram disulfide.
[0065] The mixing of the rubber composition can be accomplished by methods known to those skilled in the art of rubber mixing. For example, the ingredients can be mixed in at least two stages, i.e., at least one non-productive stage, followed by a productive mixing stage. The final curing agent (curatives) including a sulfur-vulcanizing agent can be mixed in the final stage, which is generally referred to as a "productive" mixing stage, wherein the mixing is generally carried out at a temperature or final temperature lower than the mixing temperature of the previous (one or more) non-productive mixing stage (s). The terms "non-productive" and "productive" mixing stages are well known to those skilled in the art of rubber mixing. In one embodiment, the rubber composition can be subjected to a thermomechanical mixing step. The thermomechanical mixing step generally includes a period of time in a mixer or extruder, such as a mechanical process suitable for producing a rubber temperature of 140°C to 190°C. The appropriate duration of the thermomechanical process varies with the operating conditions and the volume and properties of the components. For example, the thermomechanical process can be carried out for 1 to 20 minutes.
[0066] The vulcanization of the (preferred) pneumatic tire of the present invention can be carried out, for example, at conventional temperatures of 100° C. to 200° C. In one embodiment, the vulcanization is carried out at a temperature in the range of 110° C. to 180° C. Any conventional vulcanization method can be used, such as heating in a press or mold, heating with superheated steam or hot air. Such tires can be manufactured, shaped, molded and cured by various known methods and are obvious to those skilled in the art.
[0067] The present invention discloses the following embodiments:
[0068] Solution 1. A tire having a tread, wherein the tread comprises a rubber composition, the rubber composition comprising:
[0069] 80 phr to 100 phr of one or more solution polymerized styrene butadiene rubbers;
[0070] 80 phr to 200 phr of a filler, the filler comprising at least 40 phr of carbon black;
[0071] 10 phr to 100 phr of one or more liquid diene-based polymers; and
[0072] 10 phr to 80 phr of terpene resin.
[0073] Option 2. The tire according to Option 1, wherein the one or more solution-polymerized styrene butadiene rubbers have a glass transition temperature in the range of -1°C to -45°C.
[0074] Option 3. The tire according to Option 1, wherein the filler comprises one or more of the following:
[0075] 80 to 150 phr of carbon black;
[0076] Mainly carbon black;
[0077] Carbon black having an iodine value of at least 180 g / kg;
[0078] Less than 20 phr of silica.
[0079] Aspect 4. The tire according to aspect 1, wherein the rubber composition comprises 15 to 45 phr of the terpene resin.
[0080] Aspect 5. The tire according to aspect 1, wherein the resin is an α-pinene-based terpene resin.
[0081] Aspect 6. The tire according to aspect 1, wherein the resin comprises one or more of the following:
[0082] Softening point in the range of 100°C to 150°C;
[0083] A glass transition temperature in the range of 50°C to 100°C;
[0084] A weight average molecular weight in the range of 200 g / mol to 900 g / mol;
[0085] Less than 5% aromatic proton content.
[0086] Option 7. The tire according to Option 1, wherein the rubber composition further comprises 5 to 70 phr of oil.
[0087] Option 8. The tire according to Option 7, wherein the rubber composition comprises 25 to 60 phr of the oil.
[0088] Embodiment 9. The tire according to embodiment 1, wherein the rubber composition comprises 95 phr to 100 phr of the one or more solution-polymerized styrene butadiene rubbers.
[0089] Aspect 10. The tire according to aspect 1, wherein the rubber composition further comprises 1 to 10 phr of an alkylphenol resin, the alkylphenol resin optionally having a softening point in the range of 120°C to 170°C.
[0090] Option 11. The tire according to Option 1, wherein the liquid diene-based polymer has one or more of the following:
[0091] Glass transition temperature in the range of -1°C to -30°C;
[0092] a number average molecular weight Mn in the range of 2000 g / mol to 15000 g / mol;
[0093] One or more of butadiene repeating units and styrene repeating units;
[0094] Homopolymer structure.
[0095] Embodiment 12. The tire according to embodiment 1, wherein the rubber composition has less than 5 phr of coumarone-indene resin.
[0096] Option 13. The tire according to Option 1, wherein the tire is a motorcycle tire.
[0097] Option 14. A tire according to Option 13, wherein the tread has two tread shoulders and a tread center portion arranged between the two tread shoulders, and wherein at least one of the tread shoulders contains the rubber composition, while the tread center portion is substantially free of the rubber composition.
[0098] Option 15. A tire according to Option 14, wherein the tread center portion comprises a rubber composition different from that of the at least one tread shoulder portion, and wherein the rubber composition of the tread center portion has a wear resistance that is at least 5% higher than the rubber composition of the at least one tread shoulder portion.
[0099] Option 16. The tire according to Option 1, wherein the tire is one or more of the following:
[0100] Motorcycle tires;
[0101] Motorcycle racing tires;
[0102] Motorcycle rear tire;
[0103] Bald tires;
[0104] Pneumatic tires;
[0105] A tire that does not have grooves that completely surround the tire in the circumferential direction;
[0106] A motorcycle tire comprising two textile-reinforced breaker layers radially covered by at least one helically wound ply strip;
[0107] A motorcycle tire comprising a split tread including two circumferential tread shoulders each comprising the rubber composition and at least one circumferential tread center portion comprising another rubber composition, wherein the two rubber compositions are different from each other.
[0108] Option 17. A tire according to Option 13, wherein the tire has two tread shoulders, each of the tread shoulders having a tread cap shoulder and a tread base shoulder below the corresponding tread cap shoulder, and wherein at least one tread cap shoulder comprises the rubber composition.
[0109] Embodiment 18. The tire according to embodiment 17, wherein the tread base shoulder has another rubber composition, the other rubber composition having a stiffness G'(1%) at least 5% lower than the rubber composition of the tread cap shoulder.
[0110] Option 19. A tire according to Option 18, wherein a tread center portion is arranged between the two tread shoulders, and wherein the tread center portion has a tread center portion rubber composition, and the tread center portion rubber composition has a wear resistance that is at least 5% higher than the rubber composition of the tread crown shoulder portion.
[0111] Embodiment 20. The tire according to embodiment 13, wherein the motorcycle tire is a slick tire.
[0112] The above-described embodiments and the features mentioned therein can be combined with one another. BRIEF DESCRIPTION OF THE DRAWINGS
[0113] The present invention will now be described by way of example with reference to the accompanying drawings, in which:
[0114] Figure 1 is a schematic partial cross-section of a motorcycle tire tread and underlying reinforcing rubber ply according to a non-limiting embodiment of the present invention. DETAILED DESCRIPTION
[0115] Figure 1 A non-limiting embodiment of a tire tread 10 supported by a reinforced rubber ply is shown. The tread 10 includes a tread center portion 2 disposed between two outer tread shoulders 3. Each tread shoulder 3 has a tread cap shoulder portion 4 and a tread base shoulder portion 5 disposed below the tread cap shoulder 4. A pair of breaker plies includes a first breaker ply 6 covered by a second breaker ply 7. Both breaker plies 6, 7 are covered by a radially wound ply strip 8 contacting the tread shoulders 3 (particularly the tread base shoulders 5) and the tread center portion 2.
[0116] According to the present embodiment of the tire tread 10, the tread cap shoulder 4 comprises a rubber composition as shown in the third column of Table 1 below (ie, an example of the present invention).
[0117] Although in the present embodiment only the tread crown shoulder 4 has an example rubber compound according to an embodiment of the present invention, the entire tread or multiple parts of the tread may also contain such a rubber compound. In the present embodiment, it is preferred that the tread center portion 2 has another rubber composition having a higher wear resistance than the rubber composition of the tread crown shoulder 4. The tread shoulder 3 may also have only one rubber compound, i.e. without a tread crown / base construction. In the present embodiment, the rubber composition of the tread base shoulder 5 is preferably softer than the composition of the tread crown shoulder 4, which helps to warm up the tire to achieve the desired performance as early as possible. However, such a feature is not necessary for the present invention, which is more concerned with the rubber composition in the crown shoulder area that comes into contact with the road when driving, especially when driving in a curve. The tread 10 shown is an example of a rear tire tread of a motorcycle racing tire without circumferential grooves. The tread 10 and the circumferential direction of the tire are in Figure 1The radial direction of the tread 10 or the tire is indicated by the letter "c". It extends perpendicularly from the axis of rotation of the tire (not shown). The axial direction, which is not drawn here, extends perpendicularly to the radial direction r and the circumferential direction c. The axial direction can also be described as the transverse direction. It can also be understood as being parallel to the axis of the tire.
[0118] The ply strip 8 is preferably a helically wound ply strip 8 which is wound around the breaker layers 6, 7 at an angle of less than 5° relative to the circumferential direction of the tire (or, in other words, relative to the equatorial plane of the tire, as is known to those skilled in the art). Preferably, such an angle is less than 2° or even less than 1°. In this context it is sometimes also referred to as a zero-degree ply strip or a covering ply strip.
[0119] Table 1
[0120]
[0121] 1 Solution polymerized styrene butadiene rubber having 40% styrene and 14% vinyl and a Tg of -29°C;
[0122] 2 Solution polymerized styrene butadiene rubber having 40% styrene and 39% vinyl and a Tg of -5°C;
[0123] 3 a liquid styrene butadiene rubber comprising 10 phr of a liquid styrene butadiene rubber having a Tg of -15°C and 41 phr of a second liquid styrene butadiene rubber having a Tg of -21°C;
[0124] 4 Carbon black, from Cabot as Propel X14, with an iodine absorption value of 202 g / kg;
[0125] 5 oil, comprising a blend of TDAE, SRAE and RAE oils;
[0126] 6 coumarone-indene resin, available from Rain Carbon as Novares C120;
[0127] 7 Terpene resins based on α-pinene, available from DRT as Dercolyte A115;
[0128] 8 Alkylphenol resin, available as Koresin from BASF;
[0129] 9 Fatty acid soap, as WB16 from Struktol;
[0130] 10 dihydroquinolines and phenylenediamines;
[0131] 11 Accelerators, including TBBS and TBzTD
[0132] The rubber composition shown in Table 1 can be preferably used as a tread or tread cap composition of a racing tire, for example, as Figure 1 The tread cap and shoulder compound of a motorcycle tire tread 10 is shown. The difference between the comparative example and the inventive example is that the inventive example includes a terpene resin instead of the coumarone-indene resin present in the comparative example, each of which is present in an amount of 20 phr. After testing, the inventors unexpectedly discovered that the terpene resin surprisingly improves the warm-up behavior of the tire, i.e., reduces the time required for the tire to provide good performance after the vehicle starts to run. Although the terpene resin used may be known in the art to provide improved wet traction compared to some other resin types, the effect of improving the warm-up behavior compared to the comparative resin, especially in dry conditions, has been newly determined.
[0133] Further details on the physical properties of the two compounds are shown in Table 2 below.
[0134] Table 2
[0135] nature Comparative Example Embodiments of the present invention <![CDATA[E* at 30 °C a > 8.6 6.9 <![CDATA[E* at 50 °C a > 4.0 3.3 <![CDATA[E* at 70 °C a > 2.6 2.2 <![CDATA[E* at 90 °C a > 2.1 1.8
[0136] a Modulus of elasticity E* (in MPa) measured on cured rubber samples at 10% prestrain, 2.5% dynamic strain and a frequency of 10 Hz using an Eplexor 150N device from Netzsch.
[0137] As can be seen from Table 2, the elastic modulus E* of the rubber compositions of the comparative examples and the examples of the invention has been determined at different temperatures. All values of E* at the same temperature are lower for the examples of the invention compared to the comparative examples. This indicates that the stiffness of the rubber composition according to the examples of the invention is reduced, which also indicates that dry grip is improved. It is worth noting that the difference in E* between the comparative examples and the examples of the invention is even greater at low temperatures than at high temperatures, so that the examples of the invention provide much better grip than the comparative examples at low rubber composition temperatures. In addition, it is worth noting that the difference between the E* value at 30°C and the E* value at 70°C is much smaller for the examples of the invention than for the comparative examples. For example, the difference in E* between 30°C and 70°C for the comparative example is 6 MPa, while for the same temperature, the corresponding value for the examples of the invention is only 4.7 MPa. This means that the consistency of the rubber composition of the invention is also improved relative to the comparative example. In other words, the grip and / or stiffness properties of the relatively cold rubber composition and the heated rubber composition are more similar in the examples of the invention than in the comparative examples.
[0138] Such behavior has also been confirmed by additional tire testing, where test riders have confirmed that the dry grip level of tires using the inventive examples as the tread crown shoulder compound is overall improved compared to the dry grip level of tires of the same construction but with the comparative examples as the tread crown shoulder compound. In addition, improved performance consistency was observed during test rides by test riders.
[0139] Another notable result is that the stiffness of the inventive examples at very high temperatures (e.g., at 90° C.) does not drop too much, which is also desirable, compared to the values of the comparative examples at the same temperature. In other words, it is also advantageous that the stiffness does not drop too much at very high temperatures, which is also achieved by the inventive examples.
[0140] According to the description of the invention provided herein, variations of the present invention are possible. Although certain representative embodiments and details have been shown for the purpose of illustrating the present invention, it will be apparent to those skilled in the art that changes can be made to the specific embodiments described, and these changes will be within the full intended scope of the present invention defined by the appended claims.
Claims
1. A tire with a tread, characterized in that The tread comprises a rubber composition comprising: 80 phr to 100 phr of one or more solution polymerized styrene butadiene rubbers; 80 to 200 phr of filler, characterized in that it contains at least 40 phr of carbon black; 10 phr to 100 phr of one or more liquid diene-based polymers; and 10 phr to 80 phr of terpene resin.
2. The tire according to claim 1, characterized in that The one or more solution polymerized styrene butadiene rubbers have a glass transition temperature in the range of -1°C to -45°C.
3. The tire according to claim 1, characterized in that The filler comprises one or more of the following: 80 to 150 phr of carbon black; Mainly carbon black; Carbon black having an iodine value of at least 180 g / kg; Less than 20 phr of silica.
4. The tire according to claim 1, characterized in that The rubber composition comprises 15 to 45 phr of the terpene resin.
5. The tire according to claim 1, characterized in that The resin is a terpene resin based on α-pinene.
6. The tire according to claim 1, characterized in that The rubber composition comprises 25 to 60 phr of oil.
7. The tire according to claim 1, characterized in that The rubber composition also includes 1 to 10 phr of an alkylphenol resin, optionally having a softening point in the range of 120°C to 170°C.
8. The tire according to claim 1, characterized in that The tire is one or more of the following: Motorcycle tires; Motorcycle racing tires; Motorcycle rear tire; Bald tires; Pneumatic tires; A tire that does not have grooves that completely surround the tire in the circumferential direction; A motorcycle tire comprising two textile-reinforced breaker layers radially covered by at least one helically wound ply strip; A motorcycle tire comprising a split tread comprising two circumferential tread shoulders each comprising the rubber composition and at least one circumferential tread center portion comprising another rubber composition, characterized in that the two rubber compositions are different from each other.
9. The tire according to claim 1, characterized in that The tire has two tread shoulders, each of which has a tread cap shoulder and a tread base shoulder below the respective tread cap shoulder, and is characterized in that at least one tread cap shoulder comprises the rubber composition.
10. The tire according to claim 9, characterized in that The base tread shoulder has another rubber composition having a stiffness G'(1%) at least 5% lower than the rubber composition of the cap tread shoulder.