LCP (Liquid Crystal Polymer) film as well as preparation method and application thereof
By introducing a cyclic structure into the LCP film, using the polymerization and photochemical cyclization reaction of aromatic monomers and dicarboxylic acids, combined with the blown film method, the anisotropy and molding problems of the LCP film were solved, and uniform mechanical properties were achieved. Improved stability and thickness uniformity, suitable for 5G mobile terminals and antenna applications.
Patent Information
- Application Number
- CN202410982626.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
Smart Images

Figure BDA0004956521500000061
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to an LCP film and a preparation method and application thereof. Background Art
[0002] LCP stands for LIQUID CRYSTAL POLYMER, and its Chinese name is liquid crystal polymer. LCP is a polymer material composed of rigid molecular chains that can have both the fluidity of liquid and the anisotropic physical properties of crystal under certain physical lines. It is a polymer material that has some properties of both crystal and liquid. The 5G commercial era is characterized by higher electromagnetic wave transmission speed and smaller signal propagation loss, requiring the dielectric constant and dielectric loss of the material to be as small as possible. Therefore, LCP film materials are widely used in high-speed connectors, 5G base station antenna oscillators, 5G mobile phone antennas, high-frequency circuit boards, etc. due to their excellent performance.
[0003] Due to the rod-like characteristics of LCP molecules, they have anisotropic defects. During the preparation of LCP films, it is easy to form anisotropy in the transverse and longitudinal tensile strengths, resulting in defective products. That is, stripes are easily formed along the MD direction (mechanical direction, longitudinal direction) and are easy to tear; along the TD direction (film width direction, transverse direction), it is easy to stretch and break. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide an LCP film to solve the problem of large anisotropy of LCP in the prior art. At the same time, the present invention will also provide a method for preparing the LCP film; in addition, the present invention will also provide applications of the LCP film.
[0005] In order to achieve the above-mentioned object and other related objects, the present invention provides the following technical solutions:
[0006] In a first aspect of the present invention, there is provided an LCP film, comprising the following raw materials in parts by weight: 70-100 parts of a liquid crystal polymer, 0-30 parts of a filler, and 0-20 parts of an additive;
[0007] The liquid crystal polymer is composed of the following repeating units: an aromatic monomer (I) containing a hydroxyl group and a coumarin group and an aromatic dicarboxylic acid (II).
[0008] The LCP chain obtained by polymerization of aromatic monomers (I) and aromatic dicarboxylic acids (II) contains coumarin groups, which easily undergo [2+2] photocyclization reaction under ultraviolet light to form a ring structure. Therefore, the photochemical cyclization reaction can effectively introduce a ring structure into the LCP chain to form a new ring LCP. This ring structure will significantly reduce the orientation of the polymer, improve the uniformity of its mechanical properties in different directions, and maintain excellent liquid crystal properties and thermal stability. This new type of ring LCP material has broad application prospects in the fields of high-performance liquid crystal displays, flexible electronic devices and high-strength composite materials.
[0009] Furthermore, the aromatic monomer (I) containing a hydroxyl group and a coumarin group includes at least one of 4-hydroxycoumarin, 4-methoxycoumarin, 7-hydroxycoumarin, 4,4'-dihydroxy-3,3'-dimethoxycoumarin, 4-hydroxy-7-methoxycoumarin, and 4-(4-hydroxyphenyl)-7-methoxycoumarin.
[0010] Furthermore, the aromatic monomer (I) of hydroxyl and coumarin groups is preferably 4,4'-dihydroxy-3,3'-dimethoxycoumarin or 4-(4-hydroxyphenyl)-7-methoxycoumarin.
[0011] 4,4'-dihydroxy-3,3'-dimethoxycoumarin has symmetry (the higher the symmetry, the smaller the dielectric constant) and good liquid crystal properties. When it is processed into a film product, it exhibits extremely low dielectric constant and dielectric loss in the high frequency band due to the high symmetry of the molecular skeleton of the material. 4-(4-hydroxyphenyl)-7-methoxycoumarin has a high molecular weight and can obtain a high molecular weight liquid crystal polymer with higher tensile strength, hardness, toughness, etc., which can improve the performance of film products.
[0012] Among them, 4-(4-hydroxyphenyl)-7-methoxycoumarin is obtained by the following preparation method: 4-hydroxybenzaldehyde and 7-methoxycoumarin are dissolved in ethanol, p-toluenesulfonic acid is added as a catalyst, and the mixture is stirred and reacted for 6-8 hours under reflux. After the reaction is completed, the mixture is cooled, the product is filtered and washed, and the purified 4-(4-hydroxyphenyl)-7-methoxycoumarin is obtained by recrystallization with ethanol.
[0013] Furthermore, the molar ratio of 4-hydroxybenzaldehyde, 7-methoxycoumarin and p-toluenesulfonic acid is (80-100):(80-100):(2-5).
[0014] Further, the aromatic dicarboxylic acid (II) includes at least one of terephthalic acid, isophthalic acid, 4,4'-dicarboxybiphenyl, 2,6-naphthalene dicarboxylic acid, 1,6-dinaphthoic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid and derivatives thereof.
[0015] Furthermore, the molar ratio of the aromatic monomer (I) containing a hydroxyl group and a coumarin group to the aromatic dicarboxylic acid (II) is (1-1.2):(1-1.2); preferably 1:1.
[0016] Furthermore, the preparation method of the liquid crystal polymer comprises the following steps:
[0017] (1) Synthesis of linear LCP containing coumarin groups
[0018] The aromatic monomer (I) containing a hydroxyl group and a coumarin group and the aromatic dicarboxylic acid (II) are dissolved in an organic solvent, a catalyst is added, and a polymerization reaction is carried out under stirring. After the reaction is completed, a purified linear LCP is obtained;
[0019] (2) Photochemical cyclization reaction to form cyclic LCP
[0020] The linear LCP is dissolved in an organic solvent, an appropriate amount of photosensitizer is added, and the mixed solution is irradiated under 365nm ultraviolet light for photochemical cyclization reaction. After the reaction is completed, the solvent is removed by rotary evaporation, and the product is washed and dried to obtain a cyclic LCP, namely the liquid crystal polymer.
[0021] In steps (1) and (2), the organic solvent includes dichloromethane, chloroform, toluene, N,N-dimethylformamide (DMF) or N,N-dimethylacetamide (DMAc).
[0022] In step (1), the molar ratio of the aromatic monomer (I) containing a hydroxyl group and a coumarin group to the aromatic dicarboxylic acid (II) is (1-1.2):(1-1.2); preferably 1:1.
[0023] In step (1), the catalyst includes at least one of p-dichlorobenzene, sulfuric acid, p-toluenesulfonic acid, tetramethylammonium salt or bismuth phosphate.
[0024] In step (1), the molar ratio of the aromatic monomer (I) containing a hydroxyl group and a coumarin group, the aromatic dicarboxylic acid (II) and the catalyst is (1-1.2): (1-1.2): (0.1-0.3).
[0025] In step (1), the polymerization reaction time is 12-24 hours.
[0026] In step (2), the photosensitizer is a metal iodide or ammonium iodide.
[0027] In step (2), the mass ratio of the linear LCP to the photosensitizer is 1:(0.01-0.05).
[0028] In step (2), the photochemical cyclization reaction time is 4-8 hours.
[0029] During the photochemical cyclization reaction, when the coumarin group is exposed to 365nm ultraviolet light, the coumarin group absorbs light energy, and the electrons are excited from the ground state to the excited state. Under the action of electron rearrangement in the excited state, a [2+2] cyclization reaction occurs, forming multiple four-membered rings within or between LCP chains. These new ring structures make LCP more flexible, and the formed ring polymer structure will significantly reduce the orientation of the polymer, improve the uniformity of its mechanical properties in different directions, and maintain excellent liquid crystal properties and thermal stability.
[0030] Furthermore, the filler includes at least one of glass fiber, carbon fiber, mineral powder, and nano filler, which is used to improve the mechanical properties and thermal stability of the LCP film.
[0031] Furthermore, the auxiliary agent includes at least one of a stabilizer, an antioxidant, and a lubricant to improve processing performance and enhance the performance of the final product.
[0032] A second aspect of the present invention provides a method for preparing an LCP film, comprising the following steps:
[0033] S1, after drying the liquid crystal polymer, fully and evenly mixing it with the selectively added filler and additive, granulating it by extrusion to obtain LCP particles, and drying it for later use;
[0034] S2, LCP particles are melted and plasticized by an extruder, extruded through a die to form a film bubble, and a gas medium is introduced into the film bubble to inflate the film bubble to obtain a cylindrical film bubble;
[0035] S3, after being air-cooled and shaped, the film is pulled out and rolled up by a guide roller to obtain an LCP film.
[0036] Preferably, the thickness of the LCP film is 10-200 μm; more preferably, the thickness of the LCP film is 30-100 μm.
[0037] In step S2, the blowing ratio (the ratio of the diameter of the film bubble after blowing to the diameter of the die) is between 2-8, preferably 2.5-5.
[0038] In step S3, the draft ratio (the ratio of the traction speed to the extrusion speed) is controlled to be between 1.5 and 6, preferably between 2 and 4, by the traction roller speed.
[0039] At present, the mainstream preparation methods of LCP film include film blowing, biaxial stretching, coating and non-woven hot pressing. Among them, the film blowing method is the simplest, most efficient and the lowest cost. However, due to the anisotropy of the LCP material, wrinkles are easily generated during the winding process, resulting in uneven film winding and poor film thickness uniformity. The present invention introduces a ring structure on the LCP chain to improve the uniformity of its mechanical properties in different directions. The basic film blowing method can be used to prepare an LCP film with good thickness uniformity and few film surface wrinkles, which effectively solves the problem that the LCP film formed by film blowing is prone to wrinkles or uneven thickness, which is beneficial to the subsequent application of the LCP film.
[0040] A third aspect of the present invention provides an application of an LCP film, and the above-mentioned LCP film can be used for antennas of 5G mobile terminals, 5G communication radars or 5G base stations.
[0041] As described above, the LCP film and the preparation method and application thereof of the present invention have the following beneficial effects:
[0042] 1. The liquid crystal polymer of the present invention contains coumarin groups, which undergo [2+2] photocyclization reaction by ultraviolet light irradiation, thereby forming multiple four-membered rings within or between LCP chains to form new cyclic LCPs. The cyclic structure will significantly reduce the orientation of the polymer, improve the uniformity of its mechanical properties in different directions, and maintain excellent liquid crystal properties and thermal stability.
[0043] 2. The present invention improves the uniformity of its mechanical properties in different directions by introducing a ring structure into the liquid crystal polymer, and can prepare an LCP film with good thickness uniformity and few wrinkles on the film surface by using a basic film blowing method, thereby effectively solving the problem that wrinkles or uneven thickness are easily generated in LCP films formed by film blowing, and is beneficial to the subsequent application of LCP films.
[0044] 3. The longitudinal and transverse mechanical properties of the LCP film of the present invention are similar, the film has extremely small anisotropy, high strength and uniform thickness. DETAILED DESCRIPTION
[0045] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0046] Example 1
[0047] 4-(4-Hydroxyphenyl)-7-methoxycoumarin is prepared by the following preparation method: 50 g (0.41 mol) of 4-hydroxybenzaldehyde and 72 g (0.41 mol) of 7-methoxycoumarin are dissolved in 1 L of ethanol, 2 g of p-toluenesulfonic acid is added as a catalyst, and the mixture is stirred and reacted under reflux for 8 hours. After the reaction is completed, the mixture is cooled, the product is filtered and washed, and then recrystallized from ethanol to obtain 104 g of purified 4-(4-hydroxyphenyl)-7-methoxycoumarin with a yield of 85%.
[0048] A liquid crystal polymer, the preparation method of which comprises the following steps:
[0049] (1) Synthesis of linear LCP containing coumarin groups
[0050] 100 g (0.35 mol) of 4-(4-hydroxyphenyl)-7-methoxycoumarin (I) and 83 g (0.35 mol) of 4,4'-biphenyldicarboxylic acid (II) were dissolved in 2 L of dichloromethane, 10 g of p-dichlorobenzene and 5 mL of 98% sulfuric acid were added as catalysts, and the mixture was stirred at room temperature for 24 h. After the reaction, the product was washed with water and recrystallized from dichloromethane to obtain a purified linear LCP;
[0051] (2) Photochemical cyclization reaction to form cyclic LCP
[0052] 100 g of linear LCP was dissolved in 2 L of dichloromethane, 2 g of ammonium iodide was added, and the mixed solution was irradiated under 365 nm ultraviolet light for 6 h to carry out a photochemical cyclization reaction. After the reaction, the solvent was removed by rotary evaporation, and the product was washed with ethanol and dried to obtain a cyclic LCP, i.e., the liquid crystal polymer.
[0053] A LCP film, the preparation method of which comprises the following steps:
[0054] S1, extruding and granulating the liquid crystal polymer prepared above to obtain LCP particles, and drying them for later use;
[0055] S2, LCP particles are melted and plasticized by an extruder, extruded through a die to form a film bubble, and a gas medium is introduced into the film bubble to inflate the film bubble to obtain a cylindrical film bubble;
[0056] S3, after being air-cooled and shaped, the film is pulled out and rolled up by a guide roller to obtain an LCP film.
[0057] Example 2
[0058] A liquid crystal polymer, the preparation method of which comprises the following steps:
[0059] (1) Synthesis of linear LCP containing coumarin groups
[0060] 100 g (0.34 mol) of 4,4'-dihydroxy-3,3'-dimethoxycoumarin (I) and 86 g (0.34 mol) of 2,6-naphthalenedicarboxylic acid (II) were dissolved in 2 L of DMF, 15 g of tetramethylammonium salt was added as a catalyst, and the mixture was refluxed at 180°C for 12 h. After the reaction was completed, the mixture was cooled and the product was washed to obtain a purified linear LCP;
[0061] (2) Photochemical cyclization reaction to form cyclic LCP
[0062] 100 g of linear LCP was dissolved in 2 L of dichloromethane, 2 g of ammonium iodide was added, and the mixed solution was irradiated under 365 nm ultraviolet light for 6 h to carry out a photochemical cyclization reaction. After the reaction, the solvent was removed by rotary evaporation, and the product was washed with ethanol and dried to obtain a cyclic LCP, i.e., the liquid crystal polymer.
[0063] A LCP film, the preparation method of which comprises the following steps:
[0064] S1, extruding and granulating the prepared liquid crystal polymer to obtain LCP particles, and drying them for later use;
[0065] S2, LCP particles are melted and plasticized by an extruder, extruded through a die to form a film bubble, and a gas medium is introduced into the film bubble to inflate the film bubble to obtain a cylindrical film bubble;
[0066] S3, after being air-cooled and shaped, the film is pulled out and rolled up by a guide roller to obtain an LCP film.
[0067] Example 3
[0068] A liquid crystal polymer, the preparation method of which comprises the following steps:
[0069] (1) Synthesis of linear LCP containing coumarin groups
[0070] 100 g (0.62 mol) of 4-hydroxycoumarin (I) and 102 g (0.62 mol) of terephthalic acid (II) were dissolved in 2 L of dichloromethane, 15 g of p-toluenesulfonic acid was added as a catalyst, and the mixture was refluxed at 150° C. for 24 h. After the reaction was completed, the mixture was cooled and the product was washed to obtain a purified linear LCP;
[0071] (2) Photochemical cyclization reaction to form cyclic LCP
[0072] 100 g of linear LCP was dissolved in 2 L of dichloromethane, 2 g of ammonium iodide was added, and the mixed solution was irradiated under 365 nm ultraviolet light for 6 h to carry out a photochemical cyclization reaction. After the reaction, the solvent was removed by rotary evaporation, and the product was washed with ethanol and dried to obtain a cyclic LCP, i.e., the liquid crystal polymer.
[0073] A LCP film, the preparation method of which comprises the following steps:
[0074] S1, extruding and granulating the prepared liquid crystal polymer to obtain LCP particles, and drying them for later use;
[0075] S2, LCP particles are melted and plasticized by an extruder, extruded through a die to form a film bubble, and a gas medium is introduced into the film bubble to inflate the film bubble to obtain a cylindrical film bubble;
[0076] S3, after being air-cooled and shaped, the film is pulled out and rolled up by a guide roller to obtain an LCP film.
[0077] Comparative Example
[0078] A LCP film, the preparation method of which comprises the following steps:
[0079] S1, extruding and granulating a commercially available liquid crystal polymer to obtain LCP particles, which are then dried for later use;
[0080] S2, LCP particles are melted and plasticized by an extruder, extruded through a die to form a film bubble, and a gas medium is introduced into the film bubble to inflate the film bubble to obtain a cylindrical film bubble;
[0081] S3, after being air-cooled and shaped, the film is pulled out and rolled up by a guide roller to obtain an LCP film.
[0082] Performance Testing
[0083] 1) Tensile strength: The longitudinal (MD) tensile strength and transverse (TD) tensile strength of the film were tested according to GB / T1040.3-2006 standard, wherein the longitudinal direction refers to the direction perpendicular to the film and the transverse direction refers to the direction parallel to the film.
[0084] 2) Thickness uniformity: Measure the thickness of the film at different positions for 50 times, and calculate the average thickness and relative deviation of the film.
[0085] 3) Film flatness: The number of wrinkles on the film surface within 300m of visually observed film length is used as the basis for judgment.
[0086] Table 1. Test results of LCP films of Examples 1-3 and Comparative Examples
[0087]
[0088] It can be seen from the data of Examples 1-3 and the comparative example that the cyclic structure of the LCP prepared by the present invention destroys the orientation of the molecular chain and reduces the anisotropy of the film, so that the longitudinal and transverse mechanical properties of the LCP resin are similar during the film forming process, and the obtained film has small anisotropy, high strength and uniform thickness.
[0089] In summary, the liquid crystal polymer of the present invention contains coumarin groups, and the coumarin groups undergo a [2+2] photocyclization reaction by ultraviolet light irradiation, thereby forming multiple four-membered rings within or between LCP chains to form a new cyclic LCP. The cyclic structure will significantly reduce the orientation of the polymer, improve the uniformity of its mechanical properties in different directions, and maintain excellent liquid crystal properties and thermal stability. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.
[0090] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. An LCP film, comprising the following raw materials in parts by weight: 70-100 parts of liquid crystal polymer, 0-30 parts of filler, and 0-20 parts of additive; It is characterized in that The liquid crystal polymer is composed of the following repeating units: an aromatic monomer (I) containing a hydroxyl group and a coumarin group and an aromatic dicarboxylic acid (II).
2. The LCP film according to claim 1, characterized in that: The aromatic monomer (I) containing hydroxyl and coumarin groups includes at least one of 4-hydroxycoumarin, 4-methoxycoumarin, 7-hydroxycoumarin, 4,4'-dihydroxy-3,3'-dimethoxycoumarin, 4-hydroxy-7-methoxycoumarin and 4-(4-hydroxyphenyl)-7-methoxycoumarin.
3. The LCP film according to claim 2, characterized in that: 4-(4-hydroxyphenyl)-7-methoxycoumarin is obtained by the following preparation method: 4-hydroxybenzaldehyde and 7-methoxycoumarin are dissolved in ethanol, p-toluenesulfonic acid is added as a catalyst, and the mixture is stirred and reacted under reflux for 6-8 hours. After the reaction is completed, the mixture is cooled, the product is filtered and washed, and the purified 4-(4-hydroxyphenyl)-7-methoxycoumarin is obtained by recrystallization with ethanol.
4. The LCP film according to claim 1, characterized in that: The aromatic dicarboxylic acid (II) includes at least one of terephthalic acid, isophthalic acid, 4,4'-dicarboxybiphenyl, 2,6-naphthalene dicarboxylic acid, 1,6-dinaphthoic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid and derivatives thereof.
5. The LCP film according to any one of claims 1 to 4, characterized in that: The preparation method of the liquid crystal polymer comprises the following steps: (1) Synthesis of linear LCP containing coumarin groups The aromatic monomer (I) containing a hydroxyl group and a coumarin group and the aromatic dicarboxylic acid (II) are dissolved in an organic solvent, a catalyst is added, and a polymerization reaction is carried out under stirring. After the reaction is completed, a purified linear LCP is obtained; (2) Photochemical cyclization reaction to form cyclic LCP The linear LCP is dissolved in an organic solvent, an appropriate amount of photosensitizer is added, and the mixed solution is irradiated under 365nm ultraviolet light for photochemical cyclization reaction. After the reaction is completed, the solvent is removed by rotary evaporation, and the product is washed and dried to obtain a cyclic LCP, namely the liquid crystal polymer.
6. The LCP film according to claim 5, characterized in that: In step (1), the catalyst includes at least one of p-dichlorobenzene, sulfuric acid, p-toluenesulfonic acid, tetramethylammonium salt or bismuth phosphate.
7. The LCP film according to claim 5, characterized in that: In step (1), the molar ratio of the aromatic monomer (I) containing a hydroxyl group and a coumarin group, the aromatic dicarboxylic acid (II) and the catalyst is (1-1.2): (1-1.2): (0.1-0.3).
8. The LCP film according to claim 5, characterized in that: In step (2), the photosensitizer is a metal iodide or ammonium iodide.
9. A method for preparing an LCP film according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, after drying the liquid crystal polymer, fully and evenly mixing it with the selectively added filler and additive, granulating it by extrusion to obtain LCP particles, and drying it for later use; S2, LCP particles are melted and plasticized by an extruder, extruded through a die to form a film bubble, and a gas medium is introduced into the film bubble to inflate the film bubble to obtain a cylindrical film bubble; S3, after being air-cooled and shaped, the film is pulled out and rolled up by a guide roller to obtain an LCP film.
10. A use of the LCP film according to any one of claims 1 to 8, characterized in that: The LCP film can be used for antennas of 5G mobile terminals, 5G communication radars or 5G base stations.