Preparation process of wear-resistant acrylic resin ink

Through the combination of POSS-based copolymer modifier and acrylic resin, the deficiencies in hardness, impact strength and wear resistance of acrylic resin ink are solved, the performance is improved and the gloss is maintained, and the overall quality of the ink is significantly improved. performance.

CN118725643AInactive Publication Date: 2024-10-01XIAMEN OUHUA IND

Patent Information

Application Number
CN202410944407.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing acrylic resin inks have poor flexibility and heat resistance in applications, and are difficult to meet the requirements for high hardness, impact strength and wear resistance.

Method used

The POSS-based copolymer modifier is combined with acrylic resin to generate 4,4'-thiophenol biphenyl dicarboximide through amic acidification and chemical imidization reactions, and combines it with divinyl hexamethyl octameric cage Type silsesquioxane undergoes thiol-ene click polymerization to form POSS-based copolymer modifier, which is filled with modified acrylic resin ink.

Benefits of technology

Significantly improves the hardness, adhesion, impact strength and abrasion resistance of the ink, while maintaining excellent gloss, reducing water absorption and improving water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725643A_ABST
    Figure CN118725643A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of printing ink, and discloses a preparation process of wear-resistant acrylic resin printing ink. The preparation method comprises the following steps: carrying out an amidation reaction and a chemical imidization reaction on 4, 4 '-thiophenol biphenyl dicarboximide and 4, 4'-diphenyl ether dianhydride to obtain 4, 4 '-thiophenol biphenyl dicarboximide, and carrying out a sulfydryl-alkene click polymerization reaction on the 4, 4'-thiophenol biphenyl dicarboximide and divinyl hexamethyl octa-polyhedral oligomeric silsesquioxane to obtain a novel POSS-based copolymer modifier which contains a rigid imide structure and a POSS nanostructure hybrid system. The acrylic resin printing ink is subjected to filling modification, so that the hardness, adhesive force, impact strength, wear resistance and other properties of the printing ink are improved, and the printing ink keeps excellent glossiness, lower water absorption and excellent water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inks, in particular to a preparation process of a wear-resistant acrylic resin ink. Background Art

[0002] Ink is an important material used in printing, mainly including base resin, pigment, additives and solvents. Among them, acrylic resin ink has good chemical stability and is widely used in various printing aspects such as books and magazines, building decoration, electronic circuit boards, etc.; Improving the hardness, impact strength and wear resistance of acrylic resin ink is of great significance; for example, the document "Preparation Process of Soluble Polyimide for UV Resin Modification" has prepared a soluble polyimide for epoxy acrylic resin modification to improve its flexibility, heat resistance and other comprehensive properties when epoxy acrylic resin is used in UV light-curing solder mask ink for flexible circuit boards. The epoxy acrylic resin has good chemical stability and is widely used in various printing aspects such as books and magazines, building decoration, electronic circuit boards, etc. Improving the hardness, impact strength and wear resistance of acrylic resin ink is of great significance; for example, the document "Preparation Process of Soluble Polyimide for UV Resin Modification" has prepared a soluble polyimide for epoxy acrylic resin modification to improve its flexibility, heat resistance and other comprehensive properties when epoxy acrylic resin is used in UV light-curing solder mask ink for flexible circuit boards. POSS cage-type polysilsesquioxane is an inorganic core composed of a silicon-oxygen skeleton alternately connected by Si-O to form a nanostructured hybrid system, which is widely used in the enhancement and modification of materials such as acrylic resins; for example, patent CN109535351A "A POSS / fluorosilicon co-modified polymethyl methacrylate resin and its preparation and molding method" discloses that perfluoroalkylethylene, hydrogen-containing siloxane oligomers and double-end diacrylates are subjected to hydrosilylation addition to first synthesize hydrophobic and oleophobic, polymerizable reactive fluorocarbon siloxane-modified acrylate monomers, which are then polymerized with methyl methacrylate, etc. The resulting polymethacrylate resin has excellent thermal stability and scratch resistance. Summary of the invention

[0003] 1. Technical issues to be solved

[0004] In view of the deficiencies in the prior art, the present invention provides a process for preparing an acrylic resin ink with high hardness, high impact strength and excellent wear resistance.

[0005] (II) Technical solution

[0006] The invention discloses a preparation process of a wear-resistant acrylic resin ink. The ink is prepared from the following components in weight proportion: 60-75% of water-based acrylic resin, 0.5-5% of a POSS-based copolymer modifier, 18-30% of a pigment, 0.1-0.6% of a dispersant, 0.2-1% of a defoamer, 0.1-0.5% of a thickener, and 1-2% of a pH regulator. The preparation process comprises the following steps: adding acrylic resin to a mixed solvent, stirring evenly, then sequentially adding a POSS-based copolymer, a pigment, a dispersant, a defoamer, a thickener, and a pH regulator, dispersing evenly in a high-speed disperser, and then grinding the mixture in a grinder to obtain the wear-resistant acrylic resin ink.

[0007] Preferably, the pigment includes any one of phthalocyanine blue, phthalocyanine green, benzidine yellow, pigment yellow, carbon black, and titanium dioxide.

[0008] Preferably, the pH regulator is ethanolamine or ammonia water with a concentration of 12-25%.

[0009] Preferably, the mixed solvent is any one of water and isopropanol, water and n-butanol, water and ethanol, and water and acetone.

[0010] Preferably, the preparation process of the POSS-based copolymer modifier is:

[0011] S1. Add 4-aminothiophenol and 4,4'-biphenyl ether dianhydride to N,N-dimethylacetamide, stir and react at room temperature for 3-8 hours, then add triethylamine and acetic anhydride, raise the temperature to 40-60°C, react for 18-36 hours, add deionized water and ethyl acetate after the reaction, let stand and extract by stratification, dry the ethyl acetate organic layer to remove water, concentrate under reduced pressure, and recrystallize the crude product with ethanol to obtain 4,4'-thiophenol biphenyl dicarboximide.

[0012] S2. Add 4,4'-benzenethiol biphenyl dicarboximide and divinyl hexamethyl octasilsesquioxane as polymerization monomers to dimethyl sulfoxide, stir to dissolve and drop photoinitiator benzoin dimethyl ether, irradiate under ultraviolet light for reaction for 1-2 hours, filter the solvent after the reaction, wash with ethanol, and obtain a POSS-based copolymer modifier.

[0013] Preferably, the molar ratio of the 4-aminothiophenol to the 4,4'-biphenyl ether dianhydride is 2-2.5:1.

[0014] Preferably, the molar ratio of the 4,4'-thiophenol biphenyl dicarboximide to the divinyl hexamethyl octameric cage-type silsesquioxane is 0.8-1.3:1.

[0015] Preferably, the amount of benzoin dimethyl ether used is 0.5-0.8% of the total amount of polymerization monomers.

[0016] (III) Beneficial technical effects

[0017] The invention utilizes 4-aminothiophenol and 4,4'-biphenyl ether dianhydride to carry out amidation reaction and chemical imidization reaction to obtain 4,4'-thiophenol biphenyl dicarboximide, and then carries out mercapto-ene click polymerization reaction with divinyl hexamethyl octameric cage-type silsesquioxane to obtain a novel POSS-based copolymer modifier, which contains a rigid imide structure and a POSS nanostructure hybrid system, performs filling and modification on acrylic resin ink, improves the hardness, adhesion, impact strength, abrasion resistance and other properties of the ink, and the ink maintains excellent gloss, low water absorption and excellent water resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is the preparation process route of POSS-based copolymer modifier. DETAILED DESCRIPTION

[0019] The preparation method of divinylhexamethyl octameric cage-type silsesquioxane refers to: the paper "Research on water-soluble acrylic resin and flexographic water-based ink".

[0020] To 300 mL of ethanol, add 13 mL of deionized water and 11.4 mL of concentrated hydrochloric acid, then add dropwise 12.6 g of methyltrimethoxysilane and 4.5 g of vinyltrimethoxysilane, react at 50°C for 48 h, filter the solvent, wash the solid with a mixed solution of tetrahydrofuran and methanol to obtain divinylhexamethyloctameric cage-type silsesquioxane.

[0021] Example 1

[0022] (1) Add 0.06 mol of 4-aminothiophenol and 0.03 mol of 4,4'-biphenyl ether dianhydride to N,N-dimethylacetamide, stir and react at room temperature for 3 h, then add 5 mL of triethylamine and 10 mL of acetic anhydride, heat to 40°C, react for 18 h, add deionized water and ethyl acetate after the reaction, stand and extract, dry the ethyl acetate organic layer to remove water, concentrate under reduced pressure, and recrystallize the crude product with ethanol to obtain 4,4'-thiophenol biphenyl dicarboximide.

[0023] (2) Add 0.04 mol of 4,4'-thiophenol biphenyl dicarboximide and 0.05 mol of divinyl hexamethyl octameric cage-type silsesquioxane as polymerization monomers to dimethyl sulfoxide, stir to dissolve and dropwise add 0.5% of the total amount of polymerization monomer as photoinitiator benzoin dimethyl ether, irradiate under ultraviolet light for reaction for 1 hour, filter the solvent after the reaction, wash with ethanol, and obtain a POSS-based copolymer modifier.

[0024] (3) Add 72% by weight of an aqueous acrylic resin to a mixed solvent of water and isopropanol, stir evenly, then add 0.5% of a POSS-based copolymer, 25% of a titanium dioxide pigment, 0.2% of a dispersant, 0.5% of a defoaming agent, 0.1% of a thickener, and 1% of a pH regulator, ethanolamine, in sequence, disperse evenly in a high-speed disperser, and then grind in a grinder to obtain a wear-resistant acrylic resin ink.

[0025] Example 2

[0026] (1) Add 0.075 mol of 4-aminothiophenol and 0.03 mol of 4,4'-biphenyl ether dianhydride to N,N-dimethylacetamide, stir and react at room temperature for 8 h, then add 6 mL of triethylamine and 12 mL of acetic anhydride, heat to 60°C, react for 36 h, add deionized water and ethyl acetate after the reaction, stand and extract, dry the ethyl acetate organic layer to remove water, concentrate under reduced pressure, and recrystallize the crude product with ethanol to obtain 4,4'-thiophenol biphenyl dicarboximide.

[0027] (2) Add 0.065 mol of 4,4'-thiophenol biphenyl dicarboximide and 0.05 mol of divinyl hexamethyl octameric cage-type silsesquioxane as polymerization monomers to dimethyl sulfoxide, stir to dissolve and dropwise add 0.8% of the total amount of polymerization monomer as photoinitiator benzoin dimethyl ether, irradiate under ultraviolet light for reaction for 2 hours, filter the solvent after the reaction, wash with ethanol, and obtain a POSS-based copolymer modifier.

[0028] (3) Add 67% by weight of an aqueous acrylic resin to a mixed solvent of water and acetone, stir evenly, then add 1% of a POSS-based copolymer, 30% of a titanium dioxide pigment, 0.1% of a dispersant, 1% of a defoaming agent, 0.2% of a thickener, and 1% of a pH adjuster, ammonia water, to a concentration of 25%, disperse evenly in a high-speed disperser, and then grind in a grinder to obtain a wear-resistant acrylic resin ink.

[0029] Example 3

[0030] (1) Add 0.068 mol of 4-aminothiophenol and 0.03 mol of 4,4'-biphenyl ether dianhydride to N,N-dimethylacetamide, stir and react at room temperature for 4 h, then add 6 mL of triethylamine and 12 mL of acetic anhydride, heat to 45°C, react for 24 h, add deionized water and ethyl acetate after the reaction, stand and extract, dry the ethyl acetate organic layer to remove water, concentrate under reduced pressure, and recrystallize the crude product with ethanol to obtain 4,4'-thiophenol biphenyl dicarboximide.

[0031] (2) Add 0.05 mol of 4,4'-thiophenol biphenyl dicarboximide and 0.05 mol of divinyl hexamethyl octameric cage-type silsesquioxane as polymerization monomers to dimethyl sulfoxide, stir to dissolve and dropwise add 0.8% of the total amount of polymerization monomer as photoinitiator benzoin dimethyl ether, irradiate under ultraviolet light for reaction for 2 hours, filter the solvent after the reaction, wash with ethanol, and obtain a POSS-based copolymer modifier.

[0032] (3) Add 75% by weight of an aqueous acrylic resin to a mixed solvent of water and n-butanol, stir evenly, then add 2.5% of a POSS-based copolymer, 20% of a titanium dioxide pigment, 0.6% of a dispersant, 0.5% of a defoaming agent, 0.2% of a thickener, and 1% of a pH adjuster, ammonia water, to a concentration of 25%, disperse evenly in a high-speed disperser, and then grind in a grinder to obtain a wear-resistant acrylic resin ink.

[0033] Example 4

[0034] (1) Add 0.075 mol of 4-aminothiophenol and 0.03 mol of 4,4'-biphenyl ether dianhydride to N,N-dimethylacetamide, stir and react at room temperature for 8 h, then add 5 mL of triethylamine and 12 mL of acetic anhydride, heat to 60°C, react for 18 h, add deionized water and ethyl acetate after the reaction, stand and extract, dry the ethyl acetate organic layer to remove water, concentrate under reduced pressure, and recrystallize the crude product with ethanol to obtain 4,4'-thiophenol biphenyl dicarboximide.

[0035] (2) Add 0.045 mol of 4,4'-thiophenol biphenyl dicarboximide and 0.05 mol of divinyl hexamethyl octameric cage-type silsesquioxane as polymerization monomers to dimethyl sulfoxide, stir to dissolve and dropwise add 0.5% of the total amount of polymerization monomer as photoinitiator benzoin dimethyl ether, irradiate under ultraviolet light for reaction for 2 hours, filter the solvent after the reaction, wash with ethanol, and obtain a POSS-based copolymer modifier.

[0036] (3) Add 69% by weight of an aqueous acrylic resin to a mixed solvent of water and ethanol, stir evenly, then add 4% of a POSS-based copolymer, 25% of a titanium dioxide pigment, 0.5% of a dispersant, 1% of a defoaming agent, 0.3% of a thickener, and 1.5% of a pH adjuster ammonia water in sequence, with a concentration of 15%, disperse evenly in a high-speed disperser, and then grind in a grinder to obtain a wear-resistant acrylic resin ink.

[0037] Example 5

[0038] (1) Add 0.06 mol of 4-aminothiophenol and 0.03 mol of 4,4'-biphenyl ether dianhydride to N,N-dimethylacetamide, stir and react at room temperature for 8 h, then add 6 mL of triethylamine and 10 mL of acetic anhydride, heat to 60°C, react for 18 h, add deionized water and ethyl acetate after the reaction, stand and extract, dry the ethyl acetate organic layer to remove water, concentrate under reduced pressure, and recrystallize the crude product with ethanol to obtain 4,4'-thiophenol biphenyl dicarboximide.

[0039] (2) Add 0.065 mol of 4,4'-thiophenol biphenyl dicarboximide and 0.05 mol of divinyl hexamethyl octameric cage-type silsesquioxane as polymerization monomers to dimethyl sulfoxide, stir to dissolve and dropwise add 0.6% of the total amount of polymerization monomer as photoinitiator benzoin dimethyl ether, irradiate under ultraviolet light for reaction for 1 hour, filter the solvent after the reaction, wash with ethanol, and obtain a POSS-based copolymer modifier.

[0040] (3) Add 67% by weight of water-based acrylic resin to a mixed solvent of water and isopropanol, stir evenly, then add 5% of POSS-based copolymer, 25% of titanium dioxide pigment, 0.6% of dispersant, 0.2% of defoamer, 0.3% of thickener, and 2% of pH adjuster ammonia water in sequence, with a concentration of 12%, disperse evenly in a high-speed disperser, and then grind in a grinder to obtain a wear-resistant acrylic resin ink.

[0041] Comparative Example 1

[0042] (1) Add 73% by weight of water-based acrylic resin to a mixed solvent of water and isopropyl alcohol, stir evenly, then add 25% of titanium dioxide pigment, 0.1% of dispersant, 1% of defoamer, 0.3% of thickener, and 1% of pH adjuster ammonia water in sequence to a concentration of 20%, disperse evenly in a high-speed disperser, and then grind in a grinder to obtain acrylic resin ink.

[0043] The hardness is tested according to GB / T6739-2006 standard.

[0044] The adhesion is measured with reference to GB / T 9286-2021 standard.

[0045] The glossiness of ink color is measured with reference to the standard "GB / T 13217.2-2009".

[0046] The impact resistance is measured with reference to the "GB / T 1732-2020" standard.

[0047] The polyurethane film was weighed and immersed in deionized water for 24 hours. After being taken out, the surface moisture was wiped and weighed to calculate the water absorption rate W, W = (m1-m) / m; m1 is the weight of the ink film after water absorption; m is the weight before water absorption.

[0048]

[0049] Compared with the acrylic resin ink prepared in Comparative Example 1, Examples 1-5 use a POSS-based copolymer modifier to fill and modify the acrylic resin ink, and its hardness, adhesion, impact strength and other properties are significantly improved, while maintaining excellent gloss, low water absorption and excellent water resistance.

Claims

1. A process for preparing a wear-resistant acrylic resin ink, which is prepared from the following components in weight proportion: 60-75% water-based acrylic resin, 0.5-5% POSS-based copolymer modifier, 18-30% pigment, 0.1-0.6% dispersant, 0.2-1% defoamer, 0.1-0.5% thickener, 1-2% pH regulator, characterized in that: The preparation process comprises the following steps: adding acrylic resin into a mixed solvent, stirring evenly, then sequentially adding a POSS-based copolymer, a pigment, a dispersant, a defoamer, a thickener, and a pH regulator, dispersing evenly in a high-speed disperser, and then grinding in a grinder to obtain a wear-resistant acrylic resin ink.

2. The process for preparing the wear-resistant acrylic resin ink according to claim 1, characterized in that: The pigment includes any one of phthalocyanine blue, phthalocyanine green, benzidine yellow, pigment yellow, carbon black and titanium dioxide.

3. The process for preparing the wear-resistant acrylic resin ink according to claim 1, characterized in that: The pH regulator is ethanolamine or ammonia water with a concentration of 12-25%.

4. The process for preparing the wear-resistant acrylic resin ink according to claim 1, characterized in that: The mixed solvent is any one of water and isopropanol, water and n-butanol, water and ethanol, and water and acetone.

5. The process for preparing the wear-resistant acrylic resin ink according to claim 1, characterized in that: The preparation technology of the POSS-based copolymer modifier is: S1. Add 4-aminothiophenol and 4,4'-biphenyl ether dianhydride to N,N-dimethylacetamide, stir and react for 3-8 hours at room temperature, then add triethylamine and acetic anhydride, heat to 40-60°C, react for 18-36 hours, add deionized water and ethyl acetate after the reaction, stand and extract by stratification, dry the ethyl acetate organic layer to remove water, concentrate under reduced pressure, and recrystallize the crude product with ethanol to obtain 4,4'-thiophenol biphenyl dicarboximide; S2. Add 4,4'-benzenethiol biphenyl dicarboximide and divinyl hexamethyl octasilsesquioxane as polymerization monomers to dimethyl sulfoxide, stir to dissolve and drop photoinitiator benzoin dimethyl ether, irradiate under ultraviolet light for reaction for 1-2 hours, filter the solvent after the reaction, wash with ethanol, and obtain a POSS-based copolymer modifier.

6. The process for preparing the wear-resistant acrylic resin ink according to claim 5, characterized in that: The molar ratio of the 4-aminothiophenol to the 4,4'-biphenyl ether dianhydride is 2-2.5:

1.

7. The process for preparing the wear-resistant acrylic resin ink according to claim 5, characterized in that: The molar ratio of the 4,4'-thiophenol biphenyl dicarboximide to the divinyl hexamethyl octameric cage-type silsesquioxane is 0.8-1.3:

1.

8. The process for preparing the wear-resistant acrylic resin ink according to claim 5, characterized in that: The amount of benzoin dimethyl ether used is 0.5-0.8% of the total amount of polymerization monomers.

Citation Information

Patent Citations

  • POSS (polyhedral oligomeric silsesquioxane)-containing polyimide resin oil abrasion-resistant high temperature-resistant solid lubricant coating material and method

    CN106867395A

  • High-wear-resistant water-based plastic printing ink and preparation method thereof

    CN108070294A

Cited By

  • Surface ion layer reaction method based on household appliance colored crystal deep processing

    CN119143405A

  • UV printing ink for cigarette packaging paper and printing process of UV printing ink

    CN119490770A

  • UV ink for cigarette packaging paper and printing process thereof

    CN119490770B

  • Wear-resistant rubber material for automobile sealing strip and preparation method of wear-resistant rubber material