Concrete anti-disturbance intelligent control method under axle coupling load effect

By monitoring the negative pressure of concrete pores in real time, determining the disturbance-sensitive period and adjusting the construction time, the problem of disturbance of newly poured concrete by vehicle-bridge coupling vibration is solved, the anti-disturbance performance and durability of concrete are improved, and the interference of traffic operations is avoided. .

CN118730760APending Publication Date: 2024-10-01JIANGSU RES INST OF BUILDING SCI CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410637260.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-29
Filing Date
2024-05-22
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the widening and expansion of highways and railways, the coupling vibration load of the vehicle and bridge has a serious impact on the disturbance of newly poured concrete. It is difficult to fundamentally eliminate this effect with existing technology, and the long-term durability of fast-hardening and early-strength concrete is at risk.

Method used

By monitoring concrete pore negative pressure in real time, the disturbance-sensitive period can be automatically determined, and reasonable construction organization measures can be formulated according to the on-site traffic flow conditions to avoid the disturbance-sensitive period of concrete, thereby avoiding disturbance damage to newly poured concrete caused by vehicle-bridge coupling loads and achieving anti- Disturbance quality and durability improvements.

Benefits of technology

It effectively avoids the disturbance and damage of newly poured concrete caused by the vehicle-bridge coupling load, extends the durability of concrete, reduces the interference of construction on traffic operations, and is suitable for different types of concrete materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118730760A_ABST
    Figure CN118730760A_ABST
Patent Text Reader

Abstract

The invention discloses a concrete anti-disturbance intelligent control method and a related construction method.The concrete anti-disturbance intelligent control method comprises the steps that the negative pressure of pores of concrete to be poured is continuously tested before formal construction, the disturbance sensitive period of the concrete is judged according to the test result, and then a construction organization plan is reasonably formulated; according to the method, the disturbance sensitive period of the concrete to be poured according to the plan is controlled within the time period with the small disturbance quantity, disturbance factors are only planned to be eliminated within the time period, and normal disturbance quantity is not intervened in other stages. The invention provides a method for automatically judging the disturbance sensitive period by monitoring the pore negative pressure of the poured concrete in real time. Therefore, the disturbance sensitive period can be completely avoided by scientifically arranging construction organizations, disturbance damage of axle coupling loads to newly-poured concrete is avoided from the angle of the construction technology, and meanwhile the anti-disturbance capacity of concrete materials can be utilized to the maximum degree. And the interference of concrete pouring in reconstruction and extension construction on the normal operation of the existing traffic system is greatly reduced. Remote, real-time and automatic monitoring of the pore negative pressure can be realized, and a signal is transmitted to a mobile phone terminal, so that intelligent control of traffic interruption is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a construction method for intelligent control of concrete anti-disturbance under vehicle-bridge coupling load, which is suitable for quality control of concrete pouring at a construction site under the disturbance of vehicle-bridge coupling load and belongs to the technical field of concrete construction. Background Art

[0002] With social progress and economic development, the highways and railways built in the early days of my country have reached or exceeded their designed capacity. Widening and expanding the original roads can not only significantly improve the transportation capacity, but also make full use of the existing transportation network system and original resources, reduce construction land, shorten the construction period, and is an important way to achieve conservation, intensive use, low-carbon, environmentally friendly and green development. In this type of project, the original transportation system is mostly a transportation hub, which bears extremely heavy transportation volume. Interrupting traffic and closing the construction for too long will cause huge economic losses and adverse social impacts.

[0003] Therefore, widening and expansion on the basis of the original road usually needs to be carried out beside the existing open highways and railways. High-speed vehicles running on existing highways or railways will have an adverse effect on the performance development and quality of the newly poured concrete in the adjacent structural parts. For example, in the widening of bridges, the concrete at the longitudinal joints of the new and old bridges plays an important structural role in connecting the new and old bridges. However, during its construction, when vehicles pass through the bridge, the moving vehicles will impose a dynamic load on the bridge and cause the bridge to vibrate, which is called vehicle-bridge coupling vibration. Therefore, under open traffic conditions, the newly poured concrete in this structural part will inevitably be disturbed by the vehicle-bridge coupling vibration, causing serious damage to its performance development and service life, and affecting the integrity of the structure. How to solve the disturbance and degradation effect of this vehicle-bridge coupling vibration load on the newly poured concrete is the key to the quality control of concrete in the renovation and expansion project.

[0004] Domestic and foreign scholars have studied the influence of this vehicle-bridge coupled vibration load on the mechanical properties, crack resistance and durability of concrete through field investigation combined with laboratory simulation vibration. The results show that this early vehicle-bridge coupled vibration load reduces the mechanical properties and durability of newly poured concrete. The degree of influence mainly depends on the development stage of the concrete's own performance during the disturbance. The degradation effect mainly occurs between the initial setting and final setting of concrete. The vehicle-bridge coupled vibration load disturbance at this stage causes irreversible damage to the concrete microstructure, resulting in a significant decrease in macroscopic mechanical properties and durability. The researchers proposed a technical approach to improve its anti-disturbance performance by adjusting the setting time of concrete, reducing the time interval between the initial and final setting of concrete, accelerating the development of early strength of concrete, and shortening the disturbance sensitive period. The technical approach of using fast-hardening early-strength concrete has achieved certain results. For example, fast-hardening sulphoaluminate cement with anhydrous calcium sulphoaluminate as the main component is used as the main cementitious material. On this basis, the time interval between the initial and final setting of concrete can be controlled within 10min~2h through the deployment of admixtures and admixtures, which greatly shortens the disturbance sensitive period of concrete. The main hydration product of sulphoaluminate cement, calcium sulfonate, grows rapidly, and the initial setting time and final setting time do not exceed 25 minutes and 180 minutes, respectively. The early strength at low temperature is 8 times that of ordinary silicate cement. Using sulphoaluminate cement as a cementitious material can achieve the effect of rapid hardening and early strength, and has been widely studied and applied in anti-disturbance concrete. However, sulphoaluminate cement has a high hydration heat, which increases the temperature; the setting time is short, and large-scale construction, especially in summer, is difficult; the alkalinity of the hydration product is low, and calcium sulfonate is unstable and prone to crystal transformation, and there is controversy about its long-term durability when exposed to the outdoors. Therefore, there are also modifications on the silicate concrete system to improve the anti-disturbance performance of concrete. By adding a setting regulator, the disturbance period of concrete is shortened from 6.0h to 2.5h; the addition of fiber improves the crack resistance of anti-disturbance concrete, and the addition of an expansive agent improves the self-healing rate of disturbed concrete. Comprehensive technical measures are used to prepare high-performance concrete, and the anti-disturbance performance is significantly improved compared with ordinary concrete.

[0005] Most of the existing technical measures shorten the initial and final setting time of concrete from the perspective of material modification, accelerate the development of early strength, and can reduce the impact of disturbance to a certain extent, but have not been fundamentally eliminated, and there are operational difficulties in actual construction. At the same time, there is a risk of reduced long-term durability of fast-hardening and early-strengthening concrete when exposed to the outdoors, which is not conducive to the service life of the project. From a process perspective, the present invention avoids the time when the newly poured concrete may be damaged by disturbance, and combines the on-site traffic conditions to provide a scientific basis for reasonable construction organization measures, fundamentally eliminate the impact of the vehicle-bridge coupling load on the disturbance of the newly poured concrete, and achieve a coordinated improvement in the anti-disturbance quality and durability of the concrete in the renovation and expansion project. Summary of the invention

[0006] The present invention provides a method for accurately determining and controlling the anti-disturbance construction time of structural concrete under the influence of a temperature and humidity coupling environment by in-situ real-time online automatic monitoring of the pore negative pressure of on-site structural concrete, and formulating reasonable construction organization measures in combination with the on-site traffic conditions to avoid the time when the newly poured concrete may be damaged by disturbance, fundamentally eliminating the influence of the vehicle-bridge coupling load on the disturbance of the newly poured concrete, and achieving the coordinated improvement of the anti-disturbance quality and durability of the concrete in the renovation and expansion project.

[0007] The technical principle of the present invention is as follows: no matter whether it is a rapid-hardening early-strength concrete prepared with sulphoaluminate cement or an early-strength concrete modified and prepared on the silicate concrete system, there is a disturbance-sensitive period. Before the disturbance-sensitive period, the newly poured concrete material has thixotropy, and the deformation under the disturbance shearing action caused by the vehicle-bridge coupling external load can be naturally repaired, so no disturbance damage will be caused; after the disturbance-sensitive period, the strength of the concrete itself is sufficient to resist the disturbance caused by the external load, and no disturbance damage will be caused; during the disturbance-sensitive period, the concrete material no longer has thixotropy because the network structure has begun to form, and the newly formed network structure is not sufficient to resist the disturbance caused by the external load, so disturbance damage will occur.

[0008] After a large number of experimental studies, the applicant found that the development law of the pore negative pressure of freshly mixed concrete and its disturbance sensitive period have the following relationship: Figure 1 The corresponding relationship shown is as follows: for newly poured concrete, before the pore negative pressure begins to increase, the various properties of the concrete will not change significantly before and after the disturbance caused by the external load, so no disturbance damage affecting its performance will occur; after the pore negative pressure begins to increase, when the pore negative pressure reaches the stage of rapid increase (50~70kPa), the capillary network structure of the concrete material has begun to form and it is no longer thixotropic. At the same time, this newly formed network structure is not sufficient to resist the disturbance caused by the external load. Therefore, the performance will be significantly attenuated before and after the disturbance caused by the external load, resulting in disturbance damage; when the pore negative pressure further increases rapidly (1~2h after exceeding 60±10kPa), the strength developed by the concrete itself is sufficient to resist the disturbance caused by the external load, and no disturbance damage will occur.

[0009] Based on the above experimental research findings, the present invention proposes to automatically determine the disturbance sensitive period by real-time monitoring of the pore negative pressure of the poured concrete, so as to scientifically arrange the construction organization to completely avoid the disturbance sensitive period. Figure 2As shown, from the perspective of construction technology, the disturbance damage of the vehicle-bridge coupling load to the newly poured concrete can be avoided, while at the same time the anti-disturbance ability of the concrete material itself can be utilized to the greatest extent, greatly reducing the interference of concrete pouring on the normal operation of the existing transportation system during the renovation and expansion construction. In addition, the present invention is applicable not only to high-early-strength concrete prepared with special technical measures such as sulphoaluminate cement, but also to normal early-strength concrete prepared with ordinary Portland cement, avoiding the durability risk caused by the use of sulphoaluminate cement, and achieving dual protection of anti-disturbance and durability. The monitoring of pore negative pressure can realize remote, real-time and automatic monitoring, and transmit the signal to the mobile phone end, thereby realizing intelligent control of traffic interruption.

[0010] The method for intelligent control of concrete anti-disturbance according to the present invention is: Before formal construction, the concrete pore negative pressure is continuously tested at the construction site or a nearby laboratory. The disturbance-sensitive period of the concrete is determined based on the test results, and a reasonable construction organization plan is then formulated so that the disturbance-sensitive period of the concrete poured according to the plan is controlled during time periods with less traffic flow, such as nighttime. Traffic closures are planned only during these time periods, while normal open traffic is maintained at other stages.

[0011] The judgment standard of the concrete disturbance sensitive period is: starting from the moment when the pore negative pressure deducted from the initial value reaches 1±0.5 kPa, and ending two hours after the pore negative pressure deducted from the initial value reaches 60±10.0 kPa.

[0012] The disturbance sensitive period of concrete usually does not exceed 4 to 6 hours.

[0013] The construction method of concrete anti-disturbance intelligent control described in the present invention: Step 1) According to the above method, the disturbance sensitive period of the concrete to be poured is measured in the laboratory, and the construction schedule is preset so that the concrete disturbance sensitive period is staggered with the disturbance peak period.

[0014] Step 2) While keeping the existing traffic system open to normal traffic, pour concrete at the anti-disturbance location. After the concrete is poured, bury the pore negative pressure sensor 1 5 cm below the surface of the earliest poured location, cover the surface with a film, start monitoring, and continue pouring concrete. After the concrete pouring is completed, bury the pore negative pressure sensor 2 5 cm below the surface near the last poured location.

[0015] Step 3) When the pore negative pressure value measured by the pore negative pressure sensor 1 minus the initial value is greater than 0.5-1.5 kPa, a traffic interruption signal is issued.

[0016] Step 4) When the pore negative pressure value measured by the pore negative pressure sensor 2 minus the initial value is greater than 50-70 kPa two hours later, a traffic resumption signal is issued.

[0017] The range of the pore negative pressure sensor is not less than 85kPa, and the accuracy is not less than ±1KPa. It is composed of a ceramic head, a pressure sensor, a gas collecting pipe and a pipe plug. The ceramic head is installed at the bottom of the gas collecting pipe, and the pipe plug is installed at the top. There are tiny pores inside the ceramic head with an average pore size of about 0.02 µm. The outer edge of the bottom of the gas collecting pipe is embedded in the ceramic head and tightly bonded to the ceramic head, and the pressure sensor is installed at the top.

[0018] The ceramic head of the pore negative pressure sensor and the plastic hose must be tightly bonded to each other without leakage.

[0019] Before using the pore negative pressure sensor, the ceramic head must be pre-filled with water and the pipe plug must be tightly plugged to prevent air leakage.

[0020] Furthermore, the ceramic head is pre-soaked in airless water for more than 24 hours.

[0021] The still water refers to water that is heated to boiling using ordinary tap water, then continued to be heated for more than 20 minutes and then cooled.

[0022] The other end of the pressure sensor of the pore negative pressure sensor is connected to a data acquisition and transmission device. The data transmission device can be various devices in the prior art, and can be a wired monitoring system (transmitted via cable) as described in CN200610038805.0. A more optimized solution is to use a wireless monitoring system.

[0023] The pore negative pressure data acquisition and transmission device can be composed of a single-chip microcomputer measurement and control system. The sensor-sensed signal is transmitted to the AD converter, which is converted into a numerical signal by the AD converter and transmitted to the central processing unit of the single-chip microcomputer. The central processing unit of the single-chip microcomputer mainly controls the acquisition time period of the sensor, sets the threshold, and distinguishes the signal. The data acquisition instrument can be connected to the computer serial port. The acquisition time period and threshold can be set directly on the data acquisition instrument or on the computer by connecting to the computer.

[0024] The concrete includes but is not limited to the following types of concrete: concrete with a strength grade of 50-100MPa prepared by using ordinary Portland cement, polycarboxylate high-efficiency water-reducing agent in an appropriate ratio, mineral admixtures such as silica powder, mineral powder, fly ash in an appropriate ratio, and sand and stone that meet the requirements of relevant standards; and concrete with expansion agent or steel fiber added to improve interface bonding and fatigue resistance; or concrete prepared by adding various admixtures to promote early hydration of cement and improve early strength in order to improve early strength.

[0025] On the basis of the above, the self-compacting concrete prepared by further optimizing the variety and increasing the dosage of polycarboxylic acid high-efficiency water-reducing agent, reasonably using thickeners, increasing the amount of adhesive and reducing the sand ratio is a more optimized solution. Through the rapid flow and self-compacting molding of concrete, the vibration process after pouring can be omitted, the construction progress can be accelerated, the interval time between the buried pore negative pressure sensor at the beginning of concrete pouring and the buried pore negative pressure sensor at the end of pouring can be shortened, and the construction closure time can be greatly reduced.

[0026] In order to further shorten the time of anti-disturbance construction and reduce interference with traffic opening, sulphoaluminate cement can also be used to partially or completely replace ordinary silicate to prepare high early strength concrete, shorten the initial and final setting time of concrete, and accelerate the development of early strength. At the same time, in order to improve its construction performance, suitable retarders can be added.

[0027] The above-mentioned concretes can be produced in a premixed manner or mixed on site. The premixed method is easier to control quality and speed up construction progress, which is a more optimized solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 : Relationship between negative pore pressure and disturbance sensitivity of laboratory concrete.

[0029] Figure 2 : Schematic diagram of anti-disturbance construction organization based on concrete pore negative pressure test on site; T1: start pouring concrete and burying pore negative pressure sensor 1; T2: The negative pore pressure of the first poured concrete reaches 1±0.5KPa, and traffic begins to be interrupted; T3: The final poured concrete, and the pore negative pressure sensor 2 is buried; T4: Traffic is opened after the pore negative pressure of the last poured concrete reaches 60±10 KPa1-2 hours later.

[0030] Figure 3 : Laboratory determined disturbance sensitive period trend diagram of specific implementation method.

[0031] Figure 4 : A curve graph obtained by testing sensor 1 according to a specific implementation method.

[0032] Figure 5 : A curve graph obtained by testing sensor 2 according to a specific implementation method. Implementation

[0033] The concrete mix proportions are as shown in the following table: Table 1 Concrete mix ratio (kg / m 3 )

[0034] First, the slump was tested in the laboratory with a value of 230 mm and an air content of 3.5%. One group of compressive strength specimens was formed and covered with plastic film, and the other group monitored the pore negative pressure simultaneously. Under different pore negative pressure values, the compressive strength specimens were placed on the concrete vibration table and re-vibrated for 2 minutes. The strength changes before and after vibration were compared to determine the disturbance sensitive period. The results are shown in the attached figure. Figure 3 As shown in the figure, the disturbance sensitive period of the concrete is 3h~14h after adding water and mixing.

[0035] On this basis, a construction organization plan was formulated. The concrete pouring and vibrating time was 3 hours. In order to arrange the traffic interruption time at night when the traffic volume was small, the concrete pouring of the joint part began at 3 pm and the pore negative pressure sensor 1 was buried. The monitoring was started and the concrete pouring continued at the same time. When the sensor emission signal reached the initial threshold of 1.5kPa, as shown in the attached figure Figure 4 At 6:00 p.m., as shown by the red line in the middle, the traffic on the existing road was interrupted and the pouring of concrete continued. A pore negative pressure sensor 2 was buried in the last concrete pouring part and monitoring began. Two hours after the sensor emission signal reached the final threshold of 60 kPa, as shown in the attached figure Figure 4 Traffic will resume at 8 a.m. the next day as indicated by the red line.

[0036] Test example: Set vibration disturbance conditions and use an electric vibration test bench to simulate vibration disturbances with a vibration frequency of 15 ~ 20 Hz and an amplitude of 5 mm The concrete mix ratio is as described in Table 1. According to the determined concrete disturbance sensitive period, three concrete test blocks are obtained under different vibration disturbance conditions.

[0037] Concrete test block 1: It was placed in a vibrating environment immediately after pouring and the vibration was stopped after 3 hours. After 14 hours, the vibration was continued for 10 hours.

[0038] Concrete test block 2: It was in a vibration disturbance environment from the start of pouring until 24 hours.

[0039] Concrete test block 3: From the start of pouring until 24 hours, it is in static conditions throughout the process.

[0040] Table 2 Concrete test block strength table

[0041] 1d strength (MPa) 3d strength (MPa) 28d strength (MPa) Concrete test block 1 34.5 44.3 62.5 Concrete test block 2 24.5 32.6 50.8 Concrete test block 3 32.3 43.5 61.8

[0042] The strength of the above concrete test blocks was tested with reference to GB / T 50081-2019, and the following data were obtained.

Claims

1. A method for intelligent control of concrete anti-disturbance is characterized by: Before formal construction, the pore negative pressure of the concrete to be poured is continuously tested, and the disturbance sensitive period of the concrete is determined based on the test results. Then, a reasonable construction organization plan is formulated so that the disturbance sensitive period of the concrete poured according to the plan is controlled within a time period with a small disturbance, and disturbance factors are eliminated only in this time period, while normal disturbance is not interfered with in other stages. The judgment standard of the concrete disturbance sensitive period is: starting from the moment when the pore negative pressure deducted from the initial value reaches 1±0.5 kPa, and ending two hours after the pore negative pressure deducted from the initial value reaches 60±10.0 kPa.

2. According to the method of concrete anti-disturbance intelligent control in claim 1, the pore negative pressure is measured by a pore negative pressure sensor, and the range of the pore negative pressure sensor is not less than 85kPa and the accuracy is not less than ±1KPa.

3. According to the method of concrete anti-disturbance intelligent control in claim 2, the feature is that the pore negative pressure sensor is composed of a ceramic head, a pressure sensor, a gas collecting pipe and a pipe plug. A ceramic head is installed at the bottom of the gas collecting pipe, and a pipe plug is provided on the top. There are tiny pores inside the ceramic head, and the pore diameter is not greater than 2µm. The outer edge of the bottom of the gas collecting pipe is embedded in the ceramic head and tightly bonded to the ceramic head, and a pressure sensor is installed at the top of the gas collecting pipe.

4. According to the method of concrete anti-disturbance intelligent control as claimed in claim 3, its characteristic is that the ceramic head of the pore negative pressure sensor must be pre-filled with water and the pipe plug must be tightly plugged before use to prevent air leakage.

5. According to the method of concrete anti-disturbance intelligent control as claimed in claim 4, the feature is that the ceramic head is pre-soaked in air-free water for more than 24 hours; the air-free water refers to water that is heated to boiling using ordinary tap water, and then continued to be heated for more than 20 minutes and then cooled.

6. A concrete anti-disturbance intelligent control construction method, characterized in that: Here are the steps: Step 1) Using the method of claim 1, the disturbance sensitive period of the concrete to be poured is measured in the laboratory, the construction schedule is preset, the disturbance sensitive period of the concrete is staggered with the peak period of disturbance, and the disturbance factors are eliminated during the low peak period of disturbance; Step 2) While maintaining the normal traffic opening of the existing traffic system, pour concrete at the anti-disturbance part. After the concrete is poured, bury the pore negative pressure sensor 1 below 5 cm below the surface of the earliest poured part, cover the surface with a film, start monitoring, and continue pouring concrete. After the concrete pouring is completed, bury the pore negative pressure sensor 2 below 5 cm below the surface near the last poured part. Step 3) When the pore negative pressure value measured by the pore negative pressure sensor 1 minus the initial value is greater than 0.5-1.5 kPa, a traffic interruption signal is issued; Step 4) When the pore negative pressure value of the pore negative pressure sensor 2 minus the initial value is greater than 50-70 kPa two hours later, a traffic resumption signal is issued.

7. The construction method of concrete anti-disturbance intelligent control according to claim 6 is characterized in that: Step 2) The other end of the pressure sensor of the pore negative pressure sensor is connected to a pore negative pressure data acquisition and transmission device.

8. The construction method of concrete anti-disturbance intelligent control according to claim 7 is characterized in that: The pore negative pressure data acquisition and transmission device is composed of a single-chip microcomputer measurement and control system. The signal sensed by the sensor is transmitted to the AD converter, converted into a numerical signal by the AD converter and transmitted to the central processing unit of the single-chip microcomputer. The central processing unit of the single-chip microcomputer mainly controls the acquisition time period of the sensor, sets the threshold value, and distinguishes the signal.

9. The construction method of concrete anti-disturbance intelligent control according to claim 8 is characterized in that: The pore negative pressure data acquisition instrument is connected to the computer serial port, and the acquisition time period and threshold value are set directly on the data acquisition instrument, or are set on the computer by connecting to the computer.

10. Application of the construction method of concrete anti-disturbance intelligent control according to claim 6, characterized in that: Applicable concrete includes but is not limited to the following types of concrete: ordinary Portland cement, concrete with a strength grade of 50~100MPa; concrete with expansion agent or steel fiber material added on this basis to improve interface bonding and fatigue resistance; or concrete prepared with various admixtures that promote early hydration of cement and improve early strength in order to improve early strength.