Nanopore chip, manufacturing method thereof and particle detection device

By forming a negative potential film layer on the side wall of the cavity of the nanopore chip, and using the electric field to drive the electrolyte to drive the particles through the micropores, the problem of the need for external driving force and inaccurate measurement in the existing technology is solved, and no external driving force is achieved. Particle detection and high concentration sample measurement.

CN118730830APending Publication Date: 2024-10-01RESUN (SHENZHEN) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410417944.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing RPS detection technology requires external driving force, has a small applicable range, and is affected by the optical properties of the sample, resulting in inaccurate measurements.

Method used

By forming a negative potential film layer on the cavity side wall of the nanopore chip and soaking it in the electrolyte, an electric field is formed to drive the electrolyte to drive the particles through the micropores, achieving detection without external driving force.

Benefits of technology

It realizes the detection of particles without external driving force, expands the scope of application, reduces measurement errors, and is suitable for the detection of high-concentration samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118730830A_ABST
    Figure CN118730830A_ABST
Patent Text Reader

Abstract

The invention discloses a nanopore chip, a manufacturing method thereof and a particle detection device, and relates to the technical field of particle detection, the nanopore chip comprises a substrate, the substrate is provided with a first surface and a second surface which are opposite to each other, and the substrate is provided with a cavity penetrating from the second surface to the first surface; the microporous membrane is formed on the first surface, the microporous membrane is provided with at least one micropore, the aperture of the micropore is smaller than that of the cavity, and the projection of all the micropores on the first surface is covered by the projection of the cavity on the first surface; and the negative potential film layer is formed on the side wall of the cavity, and the negative potential film layer is configured to be soaked in the electrolyte, and the zeta potential of the interface is negative potential. According to the invention, the to-be-tested particles can pass through the micropores without external driving force, and the pulse signals of the to-be-tested particles can be tested through the circuit of the test electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of particle detection, and in particular to a nanopore chip and a manufacturing method thereof, and a particle detection device. Background Art

[0002] Traditional single particle detection technologies include: electron microscopy, NTA (nano-tracer technology), NanoFCM (nano-flow cytometry), and RPS (resistive pulse sensing).

[0003] Although electron microscopes can visually measure the particle size of nanoparticles, they require dry sample preparation before testing and cannot display the state of the sample in liquid.

[0004] The basic principle of NTA (Nanotracer Technology) is to track the Brownian motion rules of nanoparticles in liquid through imaging method, and to infer the particle size of nanoparticles by the speed of Brownian motion. However, this method will be affected by the hydrophilicity of the sample, the light scattering intensity of the sample and the accuracy of image acquisition, resulting in inaccurate particle size measurement.

[0005] The basic principle of NanoFCM (Nano Flow Detection) is to pass the sample particles through the laser individually in a sheath flow mode, and infer the particle size by detecting the scattered signal of the laser. This method is also affected by the difference in the optical properties of the particles, resulting in inaccurate testing.

[0006] RPS (Resistive Pulse Sensing) is a technology used to detect tiny particles (such as cells, microparticles, etc.). In RPS, the particle passes through a tiny fluid channel (generally called a nanopore) containing an electrolyte. When the particle passes through the channel, it causes a sudden change in resistance, which is called a resistive pulse.

[0007] The existing RPS detection technology relies on external driving of particles through nanopores and has a small scope of application. Summary of the invention

[0008] The main technical problem solved by the present invention is that the existing RPS detection technology requires an external driving force for detection.

[0009] According to the first aspect, an embodiment provides a nanopore chip, comprising: A substrate, the substrate having a first surface and a second surface opposite to each other, and a cavity extending from the second surface to the first surface; A microporous membrane is formed on the first surface, the microporous membrane has at least one micropore, the pore size of the micropore is smaller than the pore size of the cavity, and the projections of all the micropores on the first surface are covered by the projections of the cavity on the first surface; The negative potential film layer is formed on the side wall of the cavity, and the negative potential film layer is configured so that the zeta potential of the interface immersed in the electrolyte is negative.

[0010] According to the second aspect, an embodiment provides a method for manufacturing a nanopore chip, comprising: providing a substrate; forming a microporous membrane on the first surface of the substrate, the microporous membrane having at least one micropore; A cavity is formed on the second surface of the substrate and penetrates to the first surface, and a negative potential film layer is formed on the side wall of the cavity; the negative potential film layer is configured so that the zeta potential of the interface immersed in the electrolyte is negative; The aperture of the micropores is smaller than the aperture of the cavity, and the projections of all the micropores on the first surface are covered by the projections of the cavity on the first surface.

[0011] According to the third aspect, an embodiment provides a nanopore chip, which is manufactured using the manufacturing method described in the second aspect.

[0012] According to a fourth aspect, an embodiment provides a particle detection device, comprising a measurement container, a first electrode, a second electrode, and the nanopore chip described in the first aspect or the third aspect; The measuring container is used to contain the electrolyte; The nanopore chip is configured to be placed vertically at the bottom of a measuring container and immersed in an electrolyte, and the measuring container is divided into a first chamber and a second chamber; one of the first chamber and the second chamber is used to place particles to be measured; The first electrode and the second electrode are respectively disposed on both sides of the first surface of the nanopore chip, and the first electrode and the second electrode are configured to input a preset voltage difference to form an electric field in the electrolyte; The negative potential membrane layer is configured so that the zeta potential of the interface immersed in the electrolyte is negative, so that the electrolyte in the cavity has a positive potential. The electrolyte moves under the action of the electric field and drives the particles to be tested to flow from one chamber to another through the micropores.

[0013] According to the nanopore chip and its manufacturing method, and particle detection device of the above-mentioned embodiments, the zeta potential of the interface of the negative potential membrane layer immersed in the electrolyte is negative, so that the electrolyte in the cavity has a positive potential. The electrolyte moves under the action of the electric field and drives the particles to be tested to flow from one chamber through the micropores to another chamber, thereby allowing the particles to be tested to pass through the micropores without the need for external driving force, and the pulse signal of the particles to be tested can be tested through the circuit of the test electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 A schematic diagram of the structure of a nanopore chip provided in one embodiment of the present application; Figure 2 A schematic diagram of the structure of a particle detection device provided in one embodiment of the present application; Figure 3 A schematic diagram of a manufacturing method according to an embodiment of the present application; Figure 4 A process schematic diagram of a manufacturing method provided in one embodiment of the present application (I); Figure 5 A schematic diagram of a manufacturing method according to an embodiment of the present application (II); Figure 6 A process schematic diagram of a manufacturing method provided in one embodiment of the present application (III); Figure 7 A process schematic diagram of a manufacturing method provided in one embodiment of the present application (IV); Figure 8 A process schematic diagram of a manufacturing method provided in one embodiment of the present application (V); Fig. 9 A schematic diagram of a manufacturing method according to an embodiment of the present application (VI); Fig.10 A schematic diagram of a pulse signal of a particle to be detected provided in one embodiment of the present application (I); Fig.11 A schematic diagram of a pulse signal of a standard particle provided in one embodiment of the present application (I); Fig.12 A schematic diagram of a pulse signal of a particle to be detected provided in one embodiment of the present application (II); Fig.13 Schematic diagram of the pulse signal of the particles to be tested provided in one embodiment of the present application (II).

[0015] Figure numerals: 1-substrate; 2-microporous membrane; 3-negative potential membrane layer; 4-transition layer; 5-protective layer; 101-cavity; 201-micropore; 301-passivation layer; 100-nanopore chip; 200-measuring container; 310-first electrode; 320-second electrode. DETAILED DESCRIPTION

[0016] The present invention is further described in detail below by specific embodiments in conjunction with the accompanying drawings. Wherein similar elements in different embodiments adopt associated similar element numbers. In the following embodiments, many detailed descriptions are for making the present application better understood. However, those skilled in the art can easily recognize that some features can be omitted in different situations, or can be replaced by other elements, materials, methods. In some cases, some operations related to the present application are not shown or described in the specification, this is to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations according to the description in the specification and the general technical knowledge in the art.

[0017] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations. At the same time, the steps or actions in the method description can also be interchanged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the various sequences in the specification and the drawings are only for the purpose of clearly describing a certain embodiment and are not meant to be a required sequence, unless otherwise specified that a certain sequence must be followed.

[0018] The serial numbers assigned to the components herein, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings).

[0019] The existing patent CN211122429U describes a device for detecting nanoparticles, but the patent does not mention the source of the driving force for the nanoparticles to pass through the nanopores. At the same time, the patent relies on single-particle electrophoresis in an electrophoresis tank to test the potential, and needs to be tested under low sample concentration conditions (to prevent two particles from being in the electrophoresis tank at the same time), so the scope of application is small.

[0020] The nanopore chip provided in the embodiment of the present application has a negative potential membrane layer arranged in the cavity (or called an electroosmotic tank or an electrophoretic tank), which can drive particles through the micropores without an external power source to achieve particle measurement.

[0021] Embodiment 1 like Figure 1 and Figure 2 As shown, an embodiment of the present application provides a nanopore chip 100 and a particle detection device. The nanopore chip 100 can be used in the particle detection device.

[0022] like Figure 1 As shown in (A) in FIG. 1 , the nanopore chip 100 may include: a substrate 1 , a microporous membrane 2 , and a negative potential membrane layer 3 .

[0023] The substrate 1 has a first surface and a second surface opposite to each other. The substrate 1 has a cavity 101 penetrating from the second surface to the first surface.

[0024] The microporous membrane 2 is formed on the first surface. The microporous membrane 2 has at least one micropore 201. The pore size of the micropore 201 is smaller than the pore size of the cavity 101. The micropore 201 is connected to the chamber 101. The projections of all micropores 201 on the first surface are covered by the projections of the cavity 101 on the first surface.

[0025] The negative potential film layer 3 is formed on the side wall of the cavity 101 , and the negative potential film layer 3 is configured such that the zeta potential of the interface immersed in the electrolyte is negative.

[0026] In some embodiments, the negative potential film layer 3 may be an amorphous carbon layer or a carbon chain polymer layer; the carbon layer or the carbon chain polymer layer may be formed by ionizing hydrocarbons or fluorocarbons in plasma and then deposited. The hydrocarbons or fluorocarbons may form carbon ions after ionization, and the carbon ions may form an amorphous carbon layer carbon chain polymer.

[0027] For example, plasma fluorinated carbon (C4F8) can be used to passivate the side wall of the cavity 101. C4F8 decomposes into ionic CF+x groups, CF-x groups and active F- groups in a plasma state. The CF+x groups and CF-x groups react with the silicon surface to form a (CF2)n polymer passivation film. The (CF2)n long chain is a fluorinated carbon polymer and a type of carbon chain polymer.

[0028] For another example, the amorphous carbon layer is formed by thermal decomposition or plasma deposition of hydrocarbon gas (such as methane, ethylene, etc.), and the carbon atoms or carbon ions ionized from the hydrocarbon gas in the plasma are then deposited on the surface of the substrate 1 to form an amorphous carbon layer.

[0029] In some embodiments, the substrate 1 may be a silicon substrate; the microporous membrane 2 is an insulating film layer, which may be a silicon nitride layer, a silicon oxynitride layer or a silicon oxide layer. The present application takes a silicon nitride layer as an example.

[0030] In some embodiments, such as Figure 1 As shown in (B) to (D), the nanopore chip 100 may further include a transition layer 4, which is formed between the microporous membrane 2 and the substrate 1. The transition layer 4 has a hollow structure or through hole connecting the micropore 201 and the cavity 101. The transition layer 4 ensures that the micropore 201 is connected to the cavity 101. The transition layer 4 can be etched under the same mask as the chamber 101. The transition layer 4 located on the second surface can be used as a hard mask when etching the chamber 101.

[0031] In some embodiments, such as Figure 1As shown in (B) to (D) in the figure, the nanopore chip 100 may further include a protective layer 5. The protective layer 5 is formed on the second surface, and the protective layer 5 has a hollow structure or a through hole connected to the cavity 101. The transition layer 4 may also be formed between the protective layer 5 and the substrate 1. The protective layer 5 located on the second surface may also be used as a hard mask when etching the chamber 101.

[0032] That is, when etching to form the micropore 201 or the cavity 101 , the transition layer 4 or the protective layer 5 can be used as a hard mask, and has a hollow structure or through hole corresponding to the upper and lower ports of the cavity 101 .

[0033] like Figure 2 As shown, the particle detection device provided in the embodiment of the present application may include a measurement container 200, a first electrode 310, a second electrode 320, and the nanopore chip 100 described above.

[0034] The measuring container 200 contains an electrolyte; the electrolyte may be an alkaline salt solution, a phosphate solution or a HEPES solution, for example, a NaCl aqueous solution, a NaOH aqueous solution, a PBS aqueous solution, a sodium phosphate aqueous solution, a sodium perchlorate solution The nanopore chip 100 is configured to be placed vertically at the bottom of the measurement container 200 and immersed in an electrolyte, and the measurement container 200 is divided into a first chamber and a second chamber; a particle to be measured is placed in one of the first chamber and the second chamber.

[0035] The first electrode 310 and the second electrode 320 are respectively disposed on both sides of the first surface of the nanopore chip 100 and in two chambers. The first electrode 310 and the second electrode 320 are configured to input a preset voltage difference to form an electric field in the electrolyte.

[0036] The negative potential membrane layer 3 is configured to have a negative zeta potential at the interface when immersed in the electrolyte, so that the electrolyte in the cavity 101 has a positive potential. The electrolyte moves under the action of the electric field and drives the particles to be tested to flow from one chamber to another through the micropores 201.

[0037] For example, when the voltage of the first electrode 310 is greater than the voltage of the second electrode 320, the particle to be tested is placed in the first chamber, and the negative potential film layer 3 in the electrolyte is negatively charged. Due to the principle of electrical neutrality, the electrolyte in the chamber 101 (or electroosmotic tank) will be positively charged. When a negative 200mV voltage is applied to the first electrode 310 and the second electrode 320 (such as the first electrode 310 is grounded and the second electrode 320 is connected to a negative voltage), an electric field will be formed in the electrolyte, and the positively charged electrolyte in the electroosmotic tank will move toward the second electrode 320 as a whole under the action of the electric field, thereby driving the liquid in the first chamber to pass through the nanopores and replenish the electroosmotic tank, and then driving the particle to be tested (such as polyethylene microspheres) in the first chamber to pass through the micropores 201 (or nanopores). Therefore, under the condition that there is no other driving force between the first chamber and the second chamber, this mechanism can also be used to enable the nanoparticles in the first chamber to pass through the nanopores.

[0038] For another example, when the voltage of the first electrode 310 is less than the voltage of the second electrode 320, the particles to be tested are placed in the second chamber, and the negative potential membrane layer 3 is negatively charged in the NaCl aqueous solution. Due to the principle of electrical neutrality, the electrolyte in the electroosmotic tank will be positively charged. When a voltage is applied to the first electrode 310 and the second electrode 320 (such as the first electrode 310 is grounded and the second electrode 320 is connected to a positive voltage), an electric field will be formed in the electrolyte, and the positively charged electrolyte in the electroosmotic tank will move toward the first electrode 310 as a whole under the action of the electric field, thereby driving the liquid in the second chamber into the electroosmotic tank, and then driving the particles to be tested (such as magnetic beads) in the second chamber into the electroosmotic tank, and finally passing through the nanopore. Therefore, under the condition that there is no other driving force between the first chamber and the second chamber, this mechanism can also be used to enable the magnetic beads in the second chamber to pass through the nanopore.

[0039] When no particle detection is performed, the nanopore chip 100 can be stored in an alkaline salt solution, a PBS aqueous solution or a HEPES aqueous solution, which can keep the zeta potential value of the interface of the negative potential membrane layer 3 stable.

[0040] Embodiment 2 like Figure 3 As shown, the present embodiment provides a method for manufacturing a nanopore chip 100, which can be used to manufacture the nanopore chip 100 described in the first embodiment. The manufacturing method may include: Step 1, provide a substrate 1. In the present application, the substrate 1 is used as a support layer for the microporous membrane 2, and the side wall of the cavity 101 is used for the deposition of the negative potential film layer 3. In the present application, the material of the substrate 1 is not limited. The present application takes silicon wafer as an example, which does not exclude the availability of other substrates.

[0041] For example, a double-sided polished silicon wafer is provided as the substrate 1, and the thickness thereof may be 0.5 mm.

[0042] In some embodiments, after step 1, the following steps may also be included: Step 100: Figure 4 As shown in (A) and (C), transition layers 4 are formed on both sides of the substrate 1, and the transition layers 4 are insulating film layers.

[0043] The transition layer 4 can be silicon dioxide or other insulating materials. When the substrate 1 is a silicon substrate, a silicon dioxide layer with a thickness of 1 micron can be formed on the first surface and the second surface of the substrate 1 by a thermal oxidation process as the transition layer 4. The transition layer 4 is formed at least between the microporous membrane 2 and the substrate 1.

[0044] Of course, the transition layer 4 may also be formed by physical vapor deposition or chemical vapor deposition. In this case, the transition layer 4 may be formed on the first surface, or on the first surface and the second surface.

[0045] Step 2: forming a microporous membrane 2 on the first surface of the substrate 1 , wherein the microporous membrane 2 has at least one micropore 201 .

[0046] Step 2 above may include: Step 200: Figure 4 As shown in (B) and (C) in the figure, an insulating film layer is deposited on the first surface of the substrate 1 as the microporous film 2.

[0047] When the transition layer 4 is formed on the first surface of the substrate 1 , an insulating film layer is formed on the transition layer 4 on the first surface as the microporous film 2 .

[0048] For example, Figure 4 As shown in (C), a silicon nitride layer of about 500 nm is deposited on each of the transition layers 4 on both sides by low stress chemical vapor deposition (LPCVD), one layer is used as the microporous membrane 2, and the other layer is used as the protective layer 5.

[0049] Step 210: Figure 5 As shown, the microporous membrane 2 is patterned to form at least one micropore 201, wherein the pore size of the micropore 201 is larger than the particle size of the particles to be measured. Generally, the particle size of the particles to be measured is at the nanometer level, and the pore size of the micropore 201 can be at the micrometer level.

[0050] Step 3: Figure 1 , Figure 7 and Figure 8 As shown, a cavity 101 penetrating to the first surface is formed on the second surface of the substrate 1, and a negative potential film layer 3 is formed on the side wall of the cavity 101; the negative potential film layer 3 is configured so that the zeta potential of the interface immersed in the electrolyte is negative.

[0051] The aperture of the micropores 201 is smaller than the aperture of the cavity 101, and the projections of all the micropores 201 on the first surface are covered by the projections of the cavity 101 on the first surface. The negative potential film layer 3 can be formed after the cavity 101; or, the negative potential film layer 3 can be formed during the formation of the cavity 101.

[0052] The embodiment of the present application focuses on forming a negative potential film layer 3 on the side wall of the cavity 101, and the zeta potential of the interface of the negative potential film layer 3 immersed in the electrolyte is negative. The specific formation method of the negative potential film layer 3 is not limited, and the specific material of the negative potential film layer 3 is not limited.

[0053] In some embodiments, the negative potential film layer 3 may be an amorphous carbon layer or a carbon chain polymer layer; the negative potential film layer 3 is formed after the cavity 101 .

[0054] In the above step 3, forming the cavity 101 on the second surface of the substrate 1 and penetrating to the first surface may include: Step 301: Figure 6 As shown, the substrate 1 is patterned by wet etching, the protective layer 5 and the transition layer 4 (if any) on the second surface are etched, and then the substrate 1 is etched. A cavity 101 penetrating to the first surface is formed on the second surface of the substrate 1. The transition layer 4 can prevent the microporous membrane 2 from being etched, thereby ensuring the integrity of the microporous membrane 2.

[0055] For example, KOH may be used to etch the silicon substrate, and then BOE etching solution may be used to etch the silicon oxide layer (transition layer 4 ) and the silicon nitride layer (microporous membrane 2 ) on the first surface.

[0056] In the above step 3, forming the negative potential film layer 3 on the side wall of the cavity 101 may include: Step 302 : Use hydrocarbon or fluorocarbon in plasma to perform passivation treatment on the side wall of the cavity 101 to form an amorphous carbon layer or a carbon chain polymer layer as the negative potential film layer 3 .

[0057] For example, a silicon substrate is placed in a reaction chamber of C4F8 with plasma, and an amorphous carbon layer or a carbon chain polymer layer is formed on the side wall of the cavity 101 as the negative potential film layer 3 .

[0058] Step 4: Slice the substrate 1 to obtain a plurality of nanopore chips 100 .

[0059] Step 5: Immerse the nanopore chip 100 in an alkaline salt solution, a phosphate solution or a HEPES solution.

[0060] For example, a silicon wafer is sliced ​​using laser cutting to obtain a plurality of chips of a size of 10 mm x 10 mm.

[0061] In some embodiments, the negative potential film layer 3 may be an amorphous carbon layer or a carbon chain polymer layer; the negative potential film layer 3 is formed during the formation process of the cavity 101 .

[0062] In step 3, forming a cavity 101 penetrating from the second surface of the substrate 1 to the first surface, and forming a negative potential film layer 3 on the side wall of the cavity 101 may include: Etching steps, such as Fig. 9 As shown in (A), the substrate 1 is patterned by dry etching to form a groove with a first depth on the second surface of the substrate 1; the first depth is less than the thickness of the substrate 1.

[0063] Passivation steps, such as Fig. 9 As shown in (B), the side wall of the groove body is passivated by plasma hydrocarbons or carbon fluorides to form an amorphous carbon layer or a carbon chain polymer layer as the negative potential film layer 3. At this time, the negative potential film layer 3 has not been completely formed. The negative potential film layer 3 in this state is defined as a passivation layer 301.

[0064] like Fig. 9 (C) to (E) and Figure 8 As shown, the etching step and the passivation step are repeated until the depth of the groove is equal to the thickness of the substrate 1 , forming a cavity 101 penetrating to the first surface, and a negative potential film layer 3 is formed on the side wall of the cavity 101 .

[0065] For example, the silicon substrate is dry-etched using plasma SF6. The exposed sidewalls are then passivated using plasma C4F8. As the groove body deepens, the length of the passivation layer 301 on the sidewalls also increases until it is completely deposited on the sidewalls to form a negative potential film layer 3.

[0066] There is no limit to the number of times the above etching steps are repeated, or the first etching depth in each etching step can be different, and the depth of the groove body is continuously deepened by etching to form the final cavity 101 and form a negative potential film layer 3 on the side wall of the cavity 101.

[0067] Embodiment 3 Corresponding to the preparation method in the second embodiment, the nanopore chip 100 can be prepared by the following steps.

[0068] 1. On a double-sided polished 0.5 mm thick 4-inch silicon wafer (substrate 1), a layer of silicon nitride (microporous membrane 2 and protective layer 5) with a thickness of about 30 nm is deposited on both sides by low pressure chemical vapor deposition (LPCVD).

[0069] 2. Spin-coat photoresist on the wafer and expose it through a photolithography process. Take a unit area of ​​5 mm x 5 mm to develop a circular pattern with a diameter of 20 nm to be etched. Use reactive ion etching (RIE) technology to etch a 20 nm circular hole (micropore 201) in the silicon nitride of the exposed area.

[0070] 3. Remove the photoresist on the top layer of the wafer and apply photoresist on the back of the wafer. Use exposure and development processes again to create a 2mmX2mm back cavity groove on the photoresist at the position corresponding to the circular hole on the back of the silicon substrate. Etch the silicon nitride through reactive ion etching (RIE) technology and remove the photoresist on the back of the wafer.

[0071] Silicon is released by dry etching to form a cavity 101, forming a self-supporting SiNx suspended membrane. The dry etching method is to etch the silicon exposed by the groove using etching gas SF6 in plasma to react with silicon, and then react in C4F8 (octafluorocyclobutane) in the plasma for passivation. After the reaction, C4F8 can form a carbon layer or carbon chain polymer (negative potential film layer 3), which is deposited on the silicon surface to prevent the reaction between fluorine ions and silicon; physical sputtering bombardment is performed in the depth direction, so that the carbon layer or carbon chain polymer in the depth direction is removed while the carbon layer or carbon chain polymer on the side can be retained, and the silicon in the depth direction is exposed and can be etched again; through this periodic "etching-passivation-etching", dry deep silicon etching is achieved.

[0072] 4. Laser cut the silicon wafer into single chips of 5mmX5mm size.

[0073] 5. Soak the single chip in a 3 mol / L NaOH aqueous solution for 2 hours, then wash it with clean water and transfer it to a PBS aqueous solution for storage.

[0074] The single chip was tested by electron microscope EDX and the elemental analysis results showed that there was a carbon layer on the silicon substrate surface.

[0075] The zeta potential of the carbon layer at the interface in PBS electrolyte was measured using an atomic force microscope and found to be -65 mV.

[0076] When the single chip is not used for testing, the chip / carbon layer (negative potential film layer 3) is stored in a PBS aqueous solution to keep the zeta potential value of the interface stable.

[0077] like Figure 2As shown, the above-mentioned single chip is placed vertically in a measuring container 200, and the container is horizontally divided into two cavities 101, namely a first chamber and a second chamber, and the first chamber and the second chamber respectively contain a first electrode 310 and a second electrode 320. The first chamber, the nanopore (micropore 201), the cavity 101 (also known as the electroosmotic tank), and the second chamber are all filled with PBS electrolyte, and the PBS electrolyte in the first chamber contains polyethylene microsphere particles to be measured.

[0078] The negative potential film layer 3 in the electrolyte is negatively charged, and due to the principle of electrical neutrality, the electrolyte in the cavity 101 will be positively charged. When a negative 200mV voltage is applied to the first electrode 310 and the second electrode 320 (such as the first electrode 310 is grounded and the second electrode 320 is connected to a negative voltage), an electric field will be formed in the electrolyte, and the positively charged electrolyte in the electroosmotic tank will move toward the second electrode 320 as a whole under the action of the electric field, thereby driving the liquid in the first chamber to pass through the nanopores and replenish the electroosmotic tank, and then driving the particles to be tested (such as polyethylene microspheres) in the first chamber to pass through the micropores 201. Therefore, under the condition that there is no other driving force between the first chamber and the second chamber, this mechanism can also be used to enable the nanoparticles in the first chamber to pass through the nanopores.

[0079] like Fig.10 As shown, the current flowing through the electrodes is tested, and the pulse signal to the polyethylene microspheres is tested.

[0080] like Fig.11 As shown, similarly, using 15 nm standard microsphere sample / standard particles (average particle size 15 nm, concentration 2E9 particle / mL) in the measuring device, the pulse signal shown in the figure is obtained.

[0081] According to the following formula, the amplitude of the pulse signal is proportional to the particle volume and proportional to the cube of the particle diameter.

[0082] ∆V=4ρe / πD 4 Id 3 ; in, ∆V is the pulse voltage amplitude, ρe is the resistivity of the electrolyte solution, I is the current of the nanopore, π is the circumference of the circle, d is the particle size of the nanoparticles, D is the pore size of the nanopore.

[0083] The average pulse peak value of the 15nm standard microsphere sample is 19000, and the average pulse peak value of the polyethylene microsphere to be tested is 5600. It can be calculated that the polyethylene microsphere to be tested is 10nm.

[0084] The flow rate passing through the nanopore per unit time is a constant, so the more particles there are in a unit volume, the more pulse signals are generated. The frequency of the pulse signals tested in the device is directly proportional to the particle concentration in the sample.

[0085] The pulse signal frequency measured for the 15nm standard microsphere sample is 90 / minute, and the pulse signal frequency measured for the polyethylene microsphere sample to be tested is 60 / minute. It can be calculated that the concentration of the polyethylene microsphere sample to be tested is 1.333E9particle / mL.

[0086] Embodiment 4 Corresponding to the preparation method in the second embodiment, the nanopore chip 100 can be prepared by the following steps.

[0087] 1. Thermally oxidize a silicon oxide layer (transition layer 4) about 1 micron thick on a double-sided polished 6-inch silicon wafer (substrate 1). Use low stress chemical vapor deposition (LPCVD) to deposit a silicon nitride layer (microporous membrane 2 and protective layer 5) about 500 nm thick on the silicon oxide on both sides of the silicon wafer.

[0088] 2. Spin-coat photoresist on the wafer, with a unit area of ​​10mmX10mm, and use the photolithography process to expose and develop the circular pattern that needs to be thinned on the photoresist; use the reactive ion etching (RIE) technology to etch the silicon nitride and silicon oxide in the exposed area into a 5um aperture (micropore 201).

[0089] 3. Remove the photoresist on the top layer of the wafer, and apply photoresist on the back of the wafer. Use exposure and development processes again to create a release pattern of the silicon substrate on the photoresist at the position corresponding to the circular hole on the back. Etch silicon nitride and silicon oxide by reactive ion etching (RIE) technology, and remove the photoresist on the back of the wafer. Release silicon by KOH, etch to form cavity 101, and form a self-supporting SiNx / SiO2 suspended membrane. Use BOE etching solution to release the silicon oxide layer (transition layer 4) under the silicon nitride layer (microporous membrane 2). Then react the silicon base in C4F8 (octafluorocyclobutane) of the plasma. C4F8 can form a carbon layer or carbon chain polymer (negative potential membrane layer 3) after reacting on the cavity wall.

[0090] 4. Laser cut the silicon wafer into single chips of 10mmX10mm size.

[0091] 5. Soak the single chip in a 1 mol / L sodium phosphate aqueous solution for 2 hours, then wash it with clean water and transfer it to a 10 mmol / L HEPES aqueous solution for storage.

[0092] The single chip was tested by electron microscope EDX and the elemental analysis results showed that there was a carbon layer on the silicon substrate surface.

[0093] The zeta potential of the carbon layer at the interface in PBS electrolyte was measured using an atomic force microscope and was -45 mV.

[0094] When the single chip is not used for testing, the carbon layer (negative potential film layer 3) is kept in a HEPES aqueous solution to keep the zeta potential value of the interface stable.

[0095] like Figure 2 As shown, the above-mentioned single chip is placed vertically in a plastic measuring container 200, and the container is horizontally divided into two chambers 101, namely the first chamber and the second chamber, and the first chamber and the second chamber respectively contain the first electrode 310 and the second electrode 320. The first chamber, the nanopore, the electroosmotic tank, and the second chamber are all filled with NaCl aqueous solution, and the NaCl aqueous solution in the first chamber contains magnetic bead microsphere particles to be measured.

[0096] In the NaCl aqueous solution, the negative potential film layer 3 is negatively charged, and due to the principle of electrical neutrality, the electrolyte in the electroosmotic tank will be positively charged. When a voltage is applied to the first electrode 310 and the second electrode 320 (such as the first electrode 310 is grounded and the second electrode 320 is connected to a positive voltage), an electric field will be formed in the electrolyte, and the positively charged electrolyte in the electroosmotic tank will move toward the first electrode 310 as a whole under the action of the electric field, thereby driving the liquid in the second chamber into the electroosmotic tank, and then driving the particles to be tested (such as magnetic beads) in the second chamber into the electroosmotic tank, and finally passing through the nanopore. Therefore, under the condition that there is no other driving force between the first chamber and the second chamber, this mechanism can also be used to enable the magnetic beads in the second chamber to pass through the nanopore.

[0097] like Fig.12 As shown, the pulse signal generated by the magnetic beads in the device was tested.

[0098] like Fig.13 As shown, the pulse signal of the 800nm ​​standard microsphere sample with a concentration of 1.2E8particle / mL was tested.

[0099] Similarly, similar to Example 3, based on the comparison of the amplitude and frequency of the pulse signal, it can be calculated that the particle size of the magnetic microspheres is 1000 nm and the concentration is 0.4E7particle / mL.

[0100] As described in the third and fourth embodiments, the nanopore chip 100 and the particle detection device provided in the present application can realize measurement without an external power source and can realize measurement under high sample concentration conditions, and have a wide range of applications.

[0101] To summarize, the embodiment of the present application forms a negative potential film layer on the cavity, and the zeta potential of the interface of the negative potential film layer immersed in the electrolyte is negative, so that the electrolyte in the cavity has a positive potential. The electrolyte moves under the action of the electric field and drives the particles to be tested to flow from one chamber through the micropores to another chamber, thereby enabling the particles to be tested to pass through the micropores without the need for an external driving force, and the pulse signal of the particles to be tested can be tested through the circuit of the test electrode.

[0102] This document is described with reference to various exemplary embodiments. However, those skilled in the art will recognize that changes and modifications may be made to the exemplary embodiments without departing from the scope of this document. For example, various operating steps and components for performing the operating steps may be implemented in different ways (e.g., one or more steps may be deleted, modified, or combined into other steps) depending on the specific application or considering any number of cost functions associated with the operation of the system.

[0103] Although the principles of this invention have been shown in various embodiments, many modifications of structures, arrangements, proportions, elements, materials and components particularly suitable for specific environments and operational requirements can be used without departing from the principles and scope of this invention. The above modifications and other changes or amendments will be included in the scope of this invention.

[0104] The foregoing specific description has been described with reference to various embodiments. However, those skilled in the art will recognize that various modifications and changes can be made without departing from the scope of the present disclosure. Therefore, the consideration of the present disclosure will be illustrative rather than restrictive, and all these modifications will be included in its scope. Similarly, the advantages, other advantages and solutions to the problems of various embodiments have been described above. However, the benefits, advantages, solutions to the problems and any elements that can produce these, or make them more clear, should not be interpreted as critical, necessary or necessary. The term "include" and any other variants used in this article are all non-exclusive inclusions, so that the process, method, article or device including the list of elements not only includes these elements, but also includes other elements that are not explicitly listed or do not belong to the process, method, system, article or device. In addition, the term "coupled" and any other variants used in this article refer to physical connections, electrical connections, magnetic connections, optical connections, communication connections, functional connections and / or any other connections.

[0105] Those skilled in the art will appreciate that many changes may be made to the details of the above-described embodiments without departing from the basic principles of the invention. Therefore, the scope of the present invention should be determined solely by the claims.

Claims

1. A nanopore chip, characterized in that: include: A substrate (1), the substrate (1) having a first surface and a second surface opposite to each other, the substrate (1) having a cavity (101) extending from the second surface to the first surface; A microporous membrane (2) formed on the first surface, the microporous membrane (2) having at least one micropore (201), the pore size of the micropore (201) being smaller than the pore size of the cavity (101), and the projections of all the micropores (201) on the first surface are covered by the projections of the cavity (101) on the first surface; A negative potential film layer (3), the negative potential film layer (3) being formed on a side wall of the cavity (101), the negative potential film layer (3) being configured such that the zeta potential of the interface when immersed in an electrolyte is negative.

2. The nanopore chip according to claim 1, characterized in that The negative potential film layer (3) is an amorphous carbon layer or a carbon chain polymer layer; And / or, the substrate (1) is a silicon substrate; And / or, the microporous membrane (2) is a silicon nitride layer.

3. The nanopore chip according to claim 1, characterized in that: Also includes: a transition layer (4) formed between the microporous membrane (2) and the substrate (1), the transition layer (4) having a hollow structure or through holes connecting the micropores (201) and the cavity (101); and / or, A protective layer (5) is formed on the second surface, the protective layer (5) having a hollow structure or a through hole connected to the cavity (101).

4. A method for manufacturing a nanopore chip, characterized in that: include: Providing a substrate (1); A microporous membrane (2) is formed on the first surface of the substrate (1), wherein the microporous membrane (2) has at least one micropore (201); A cavity (101) is formed on the second surface of the substrate (1) and extends through the first surface, and a negative potential film layer (3) is formed on the side wall of the cavity (101); the negative potential film layer (3) is configured such that the zeta potential of the interface when immersed in an electrolyte is negative; The aperture of the micropores (201) is smaller than the aperture of the cavity (101), and the projections of all the micropores (201) on the first surface are covered by the projections of the cavity (101) on the first surface.

5. The manufacturing method according to claim 4, characterized in that: The negative potential film layer (3) is an amorphous carbon layer or a carbon chain polymer layer; the negative potential film layer (3) is formed after the cavity (101); Wherein, the cavity (101) formed on the second surface of the substrate (1) and penetrating to the first surface comprises: Patterning the substrate (1) using wet etching to form a cavity (101) on the second surface of the substrate (1) that penetrates to the first surface; A negative potential film layer (3) is formed on the side wall of the cavity (101), comprising: The side wall of the cavity (101) is passivated using hydrocarbons or fluorocarbons in plasma to form an amorphous carbon layer or a carbon chain polymer layer as the negative potential film layer (3).

6. The manufacturing method according to claim 4, characterized in that: The negative potential film layer (3) is an amorphous carbon layer or a carbon chain polymer layer; the negative potential film layer (3) is formed during the formation process of the cavity (101); A cavity (101) is formed on the second surface of the substrate (1) and penetrates to the first surface, and a negative potential film layer (3) is formed on the side wall of the cavity (101), comprising: An etching step, patterning the substrate (1) by dry etching, to form a groove of a first depth on the second surface of the substrate (1); the first depth being less than the thickness of the substrate (1); A passivation step, using hydrocarbons or fluorocarbons in plasma to passivate the side walls of the tank body to form an amorphous carbon layer or a carbon chain polymer layer as the negative potential film layer (3); The etching step and the passivation step are repeated until the depth of the groove is equal to the thickness of the substrate (1), a cavity (101) penetrating to the first surface is formed, and the negative potential film layer (3) is formed on the side wall of the cavity (101).

7. The manufacturing method according to claim 5 or 6, characterized in that: The fluorocarbon is octafluorocyclobutane.

8. The manufacturing method according to any one of claims 4 to 6, characterized in that: Also includes: The nanopore chip is immersed in an alkaline salt solution, a phosphate solution or a HEPES solution.

9. A nanopore chip, characterized in that: The method is manufactured by the manufacturing method described in any one of claims 4 to 8.

10. A particle detection device, characterized in that: A nanopore chip (100) comprising a measurement container (200), a first electrode (310), a second electrode (320), and any one of claims 1 to 3 and 9; The measuring container (200) is used to contain electrolyte; The nanopore chip (100) is configured to be vertically placed at the bottom of the measurement container (200) and immersed in an electrolyte, and the measurement container (200) is divided into a first chamber and a second chamber; one of the first chamber and the second chamber is used to place particles to be measured; The first electrode (310) and the second electrode (320) are respectively arranged on both sides of the first surface of the nanopore chip (100), and the first electrode (310) and the second electrode (320) are configured to input a preset voltage difference to form an electric field in the electrolyte; The negative potential membrane layer (3) is configured such that the zeta potential of the interface immersed in the electrolyte is negative, so that the electrolyte in the cavity (101) has a positive potential. The electrolyte moves under the action of the electric field and drives the particles to be tested to flow from one cavity through the micropores (201) to another cavity.