Positive photoresist composition and method for fabricating resist pattern

By using alkali-soluble resin, diazonaphthoquinone sulfonate and phenolic hydroxyl-containing compounds in the photoresist, combined with a specific process flow, the gap between resolution and thermal stability of the existing photoresist is solved. Taking into account the difficult problem, it achieves the effects of high sensitivity, high resolution and high residual film rate, and is suitable for the manufacturing of integrated circuits and LCD panels.

CN118732397APending Publication Date: 2024-10-01CHANGZHOU TRONLY ADVANCED ELECTRONICS MATERIALS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310311530.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing photoresists have problems in resolution and pattern shape, especially the challenge of balancing high sensitivity and thermal stability, which is especially suitable for the manufacture of integrated circuits and liquid crystal panels.

Method used

A positive photoresist composition containing an alkali-soluble resin, diazonaphthoquinone sulfonate, a phenolic hydroxyl compound with a molecular weight of less than 1000 and an organic solvent is used, and is passed through a specific polyhydroxy phenolic compound and diazonaphthoquinone sulfonate. The acid chloride reaction product acts as a photosensitizer and is combined with appropriate processes such as heating treatment and development treatment to form a resist pattern with high sensitivity, high resolution and high residual film rate.

Benefits of technology

It achieves high sensitivity and high resolution in the manufacturing of integrated circuits and LCD panels, as well as excellent thermal stability and etching resistance. It is suitable for dry etching processes and improves pattern fidelity and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732397A_ABST
    Figure CN118732397A_ABST
Patent Text Reader

Abstract

A positive photoresist composition for manufacturing an LCD in which an integrated circuit and a liquid crystal display portion are formed on a single substrate, the positive photoresist composition containing (A) an alkali-soluble resin, (B) a diazonaphthoquinone sulfonic acid ester, (C) a phenolic hydroxyl group-containing compound having a molecular weight of 1000 or less, and (D) an organic solvent, component (B) contains a reaction product of a polyhydroxyphenol compound represented by general formula (I) and a diazonaphthoquinone sulfonyl chloride compound (II). According to the present invention, it is possible to provide a positive photoresist composition and a method for forming a resist pattern, which are suitable for systematic LCD manufacturing and can satisfy both high sensitivity and high residual film rate. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive photoresist composition for manufacturing integrated circuits or liquid crystal panels (LCDs) and a method for forming an anti-etching pattern using the positive photoresist composition. Background Art

[0002] Photoresist, also known as photoresist, is an important material in the production process of integrated circuits or liquid crystal panels (LCDs), and is used as an anti-corrosion coating material in the photolithography process. With the development of photolithography technology, the line width of integrated circuits has gradually narrowed, and the exposure wavelength of photoresist has undergone a change process from G line (436nm), I line (365nm), to deep ultraviolet (KrF 248nm). The composition of positive photoresist compositions used for integrated circuit manufacturing or liquid crystal panel (LCD) production has also changed continuously. UV positive photoresists containing alkali-soluble resins (such as linear phenolic resins) and diazonaphthoquinone compounds are the most commonly used photoresists in G line lithography and I line lithography. On the one hand, phenolic resins can be dissolved in alkaline developer and do not swell in the developer. On the other hand, diazonaphthoquinone photosensitizers will be converted into indene carboxylic acid after exposure to increase the solubility of phenolic resins, and will cross-link with phenolic resins in non-exposed areas to act as dissolution inhibitors. Phenolic resin / diazonaphthoquinone system is widely used because of the above advantages.

[0003] To date, photoresist compositions containing diazonaphthoquinone type photosensitizer-phenolic resin have been widely reported.

[0004] In the patent GB1501194A of IBM Corporation of the United States, a positive photoresist composition is reported, which contains 2,3,4-trihydroxybenzophenone diazonaphthoquinone sulfonate and phenolic resin components, which can be used to manufacture semiconductor devices. However, the photoresist containing this type of photosensitizer has problems in resolution and pattern shape (contour).

[0005] Mitsubishi Chemical Corporation's patent JP1992001340B2 discloses a positive photoresist composition containing 2,3,4,4'-tetrahydroxybenzophenone diazonaphthoquinone sulfonate and a phenolic resin prepared from a mixture of p-cresol and 2,5-xylenol. The positive photoresist exhibits good resolution (up to 1.0 μm) and good thermal stability. The solubility of 2,3,4,4'-tetrahydroxybenzophenone diazonaphthoquinone sulfonate in the patent is very low in the photoresist formulation, and the purpose of increasing the sensitivity of the photoresist cannot be achieved by increasing its addition amount.

[0006] Sumitomo Chemical Co., Ltd.'s patent JP1991007240A reported a positive photoresist composition containing 2-hydroxyphenyl-2-trihydroxyphenylpropane diazonaphthoquinone ester. Compared with positive photoresists containing benzophenone compounds, the resolution is higher, reaching 0.5-0.6 μm. However, the positive photoresist in this patent has obvious defects in thermal stability and cannot be used in dry etching processes. SUMMARY OF THE INVENTION

[0008] In view of the deficiencies in the prior art, the main purpose of the present invention is to provide a positive photoresist composition for use in the manufacture of integrated circuits or liquid crystal panels (LCDs), and a method for forming an anti-etching pattern. The positive photoresist composition not only meets the high sensitivity required for the manufacture of a system LCD having an integrated circuit and a liquid crystal display part, but also has the excellent performance of a high residual film rate.

[0009] The above object can be achieved through the following solutions of the present invention.

[0010] The present invention provides a positive photoresist composition for manufacturing integrated circuits or liquid crystal panels (LCDs) (hereinafter referred to as the photoresist composition of the present invention), characterized in that it contains (A) an alkali-soluble resin, (B) a diazonaphthoquinone sulfonate, (C) a phenolic hydroxyl compound having a molecular weight of 1000 or less, and (D) an organic solvent, wherein the component (B) contains a reaction product of a polyhydroxyphenol compound represented by the following general formula (I) and a diazonaphthoquinone sulfonyl chloride represented by (II),

[0011]

[0012] wherein R1, R2, and R3 each independently represent hydrogen, halogen, C1-C 18 Straight or branched alkyl, C6~C 12 Aryl, C1-C8 alkoxy, C1-C8 alkylthio, C2-C 10 Unsaturated hydrocarbon group, C3~C 12 Cycloalkyl, C4~C 12 Cycloalkyl, C1-C9 alkanoyl, C7-C 13 Aroyl, C3-C6 heterocyclic group in which carbon or hydrogen atoms may be selectively replaced by O, S or N atoms, C1-C 18 Alkylamino or arylamino; a, b, c each independently represent an integer between 0 and 2; x, y, z each independently represent an integer between 0 and 3; the diazonaphthoquinonesulfonyl chloride (II) is one of the following structural compounds.

[0013]

[0014] In addition, the present invention also provides a method for forming an anti-etching pattern, which includes the following steps: (1) applying the positive photoresist composition on a substrate to form a coating film; (2) heating the substrate on which the coating film is formed (pre-baking) to form an anti-etching film on the substrate; (3) using a mask having a mask pattern for forming an anti-etching pattern of less than 2.0 μm and a mask pattern for forming an anti-etching pattern of more than 2.0 μm, to selectively expose the anti-etching film; (4) heating the selectively exposed anti-etching film (post-exposure baking); (5)

[0015] The resist film after the heat treatment (post-exposure drying) is developed with an alkaline aqueous solution to simultaneously form a resist pattern for an integrated circuit with a pattern size of less than 2.0 μm and a resist pattern for a liquid crystal panel (LCD) with a pattern size exceeding 2.0 μm on the substrate. DETAILED DESCRIPTION OF THE INVENTION

[0017] The inventors surprisingly found in their research and application that the positive photoresist composition used in the present invention can have particularly excellent performance when used to manufacture liquid crystal panels (LCDs) or integrated circuits, the components have good compatibility, excellent sensitivity, good developability, and the resulting resist pattern has a high residual film rate.

[0018] "Positive photoresist composition for LCD manufacturing"

[0019] <(A)Component>

[0020] The component (A) is an alkali-soluble resin.

[0021] The component (A) is not particularly limited, and one or more components may be arbitrarily selected from substances generally used for film formation in positive photoresist compositions.

[0022] For example, there can be mentioned: novolac resins obtained by condensing phenols (phenol, m-cresol, p-cresol, xylenol, trimethylphenol, etc.) and aldehydes (formaldehyde, formaldehyde precursors, propionaldehyde, 2-hydroxybenzaldehyde, 3-hydroxybenzaldehyde, 4-hydroxybenzaldehyde, etc.) and / or ketones (methyl ethyl ketone, acetone, etc.) in the presence of an acidic catalyst;

[0023] Hydroxystyrene resins such as homopolymers of hydroxystyrene, copolymers of hydroxystyrene and other styrene monomers, and copolymers of hydroxystyrene and acrylic acid or methacrylic acid or their derivatives;

[0024] Copolymers of acrylic acid or methacrylic acid and their derivatives, namely acrylic acid or methacrylic acid resins, etc.

[0025] In order to obtain a resist material with high sensitivity and good resolution, a novolac resin obtained by condensing phenols and aldehydes in the presence of an acidic catalyst is preferred. Particularly preferred is a novolac resin obtained by condensing phenols containing at least two kinds of phenols selected from m-cresol, p-cresol, 3,4-xylenol or 2,3,5-trimethylphenol and an aldehyde containing formaldehyde.

[0026] The novolac resin can be produced according to a conventional method or is commercially available.

[0027] The weight average molecular weight of the novolac resin is preferably 2,000 to 100,000, more preferably 2,000 to 30,000, from the viewpoint of sensitivity and pattern formation.

[0028] <(B) Component>

[0029] The component (B) is a diazonaphthoquinone sulfonate, which contains a reaction product (hereinafter referred to as a photosensitizer) of a specific non-benzophenone PAC, i.e., a polyhydroxyphenol compound represented by the general formula (I) and the diazonaphthoquinone sulfonyl chloride (II). The positive photoresist composition containing the photosensitizer has high sensitivity, high resolution and high residual film rate. It is also suitable for i-line photolithography and is ideal in terms of linearity, depth of focus (DOF) and other characteristics.

[0030] The polyhydroxyphenol compound has a structure as shown in the following formula (I):

[0031]

[0032] wherein R1, R2, and R3 each independently represent hydrogen, halogen, C1-C 18 Straight or branched alkyl, C6~C 12 Aryl, C1-C8 alkoxy, C1-C8 alkylthio, C2-C 10 Unsaturated hydrocarbon group, C3~C 12 Cycloalkyl, C4~C 12 Cycloalkyl, C1-C9 alkanoyl, C7-C 13 Aroyl, C3-C6 heterocyclic group in which carbon or hydrogen atoms may be selectively replaced by O, S or N atoms, C1-C 18 an alkylamino group or an arylamino group; a, b, c each independently represent an integer between 0 and 2, such as 0, 1 or 2; x, y, z each independently represent an integer between 0 and 3, such as 0, 1, 2 or 3.

[0033] By applying the technical solution provided in the present application, the diazonaphthoquinone sulfonate prepared by using the polyhydroxyphenol compound provided in the present application as an intermediate is used as a photosensitizer in a photoresist composition. The obtained photoresist not only has clear resolution and high sensitivity, but also has excellent thermal stability and etching resistance, and has broad application prospects in the semiconductor field.

[0034] In some embodiments of the present application, R1, R2, and R3 each independently represent hydrogen, C1-C6 straight or branched alkyl, C6-C 12 When the polyhydroxyphenol compound is used as an intermediate to prepare a diazo naphthoquinone sulfonate, the diazo naphthoquinone sulfonate is used as a photosensitizer in a photoresist composition, and the obtained photoresist has better resolution, sensitivity, thermal stability and etching resistance.

[0035] In some embodiments of the present application, the polyhydroxyphenol compound is selected from at least one of the following structural compounds:

[0036]

[0037]

[0038]

[0039] The diazonaphthoquinone sulfonate prepared by using the polyhydroxyphenol compound (I) of the above structure as an intermediate is applied as a photosensitizer in a photoresist composition, and the obtained photoresist has better performance, including better resolution, sensitivity, thermal stability and etching resistance.

[0040] The polyhydroxyphenols having the above structures may be used alone or in combination of two or more after being esterified with naphthoquinone diazide.

[0041] The method for esterifying the phenolic hydroxyl group of the compound represented by the general formula (I) with naphthoquinone diazide is as follows:

[0042] The preparation method comprises: step A1, mixing a polyhydroxyphenol compound represented by general formula (I) and diazonaphthoquinone sulfonyl chloride (II) in an organic solvent, reacting under the action of an acid binding agent to obtain the diazonaphthoquinone ester product.

[0043] The reaction is carried out under the protection of an inert gas, which includes but is not limited to nitrogen or argon; the reaction temperature is 20 to 60° C., and the reaction time is 0.5 to 6 hours. In particular, when the reaction temperature is 25 to 40° C. and the reaction time is 1 to 3 hours, it is more conducive to improving the preparation efficiency of diazoquinone sulfonate.

[0044] The type of the acid binding agent is not limited, and any substance that can promote the reaction of the polyhydroxyphenol compound represented by the general formula (I) and the diazonaphthoquinonesulfonyl chloride (II) can be used, including but not limited to at least one of triethylamine, tripropylamine, ethylenediamine, pyridine, 4-dimethylaminopyridine, quinoline, N,N-dimethylaniline, tetramethylammonium hydroxide, sodium methoxide, sodium ethoxide, potassium tert-butoxide, lithium diisopropylamide, sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium hydroxide, ammonium hydroxide, and sodium hydride, preferably a mixture of one or more of triethylamine, pyridine, and sodium bicarbonate.

[0045] The type of the above-mentioned organic solvent is not limited, and any substance that can promote the reaction of the polyhydroxyphenol compound represented by the general formula (I) and diazonaphthoquinonesulfonyl chloride (II) can be used, including but not limited to a mixture of one or more of methanol, ethanol, benzene, toluene, dichloromethane, dichloroethane, acetone, butanone, tetrahydrofuran, o-xylene, m-xylene, N,N-dimethylformamide, tetrahydrofuran, ethyl acetate, 1,4-dioxane, pyridine, and N-methylpyrrolidone.

[0046] Step A2, purifying the diazo naphthoquinone sulfonate product to obtain diazo naphthoquinone sulfonate; wherein the polyhydroxyphenol compound is the polyhydroxyphenol compound provided in the first typical embodiment or the polyhydroxyphenol compound obtained according to the preparation method provided in the second typical embodiment, and the diazosulfonyl chloride (II) represents at least one of the following structural compounds.

[0047]

[0048] In the above step A2, purification includes at least one of solid-liquid separation, crystallization, washing and drying;

[0049] The crystallization step is preferably carried out in dilute hydrochloric acid, and the mass concentration of the dilute hydrochloric acid is 0.1-5.0%, preferably 0.5-2.0%.

[0050] In order to further improve the drying efficiency, it is preferred to adopt a reduced pressure drying method, wherein the pressure of the reduced pressure drying is 10 to 500 mbar and the temperature is 40 to 60°C.

[0051] Typically but not limiting, when preparing naphthoquinone diazosulfonate (B), the reaction temperature is 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C or any range between two values; the reaction time is 1h, 1.5h, 2h, 2.5h, 3h or any range between two values; the mass concentration of dilute hydrochloric acid used for crystallization is 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 3% , 4%, 5% or a range consisting of any two values; the drying pressure is 10mbar, 20mbar, 50mbar, 100mbar, 150mbar, 200mbar, 300mbar, 400mbar, 500mbar or a range consisting of any two values; the drying temperature is 40°C, 42°C, 45°C, 48°C, 50°C, 52°C, 55°C, 58°C, 60°C or a range consisting of any two values.

[0052] In some embodiments of the present application, diazonaphthoquinone sulfonate is prepared according to the following steps:

[0053] (1) in an inert gas atmosphere, uniformly mixing a second organic solvent, a polyhydroxyphenol compound and DNQ;

[0054] (2) slowly adding an acid binding agent at room temperature, raising the temperature to the reaction temperature, and maintaining the temperature to continue the reaction;

[0055] (3) After the reaction in step (2) is completed, the solid precipitated in the system is removed by filtration, and the mother liquor obtained after filtration is slowly added into dilute hydrochloric acid (mass concentration 0.5% to 2.0%), stirred for crystallization, and filtered for a second time to obtain a crude product of diazoquinone sulfonate;

[0056] (4) The crude diazoquinone sulfonate obtained in step (3) is washed three times with pure water and dried under reduced pressure to obtain diazonaphthoquinone sulfonate.

[0057] In addition to the preferred naphthoquinone diazide esters as exemplified above, other naphthoquinone diazide sulfonates generally used as photosensitive components in positive photoresist compositions may be used as component (B), for example, esterification products of phenolic compounds such as polyhydroxybenzophenone and gallic acid alkyl esters and naphthoquinone diazide sulfonic acid compounds. One or more of the other naphthoquinone diazide esters may be selected and used.

[0058] The amount of the other naphthoquinonediazide ester compound used in the component (B) is preferably 80% by mass or less, and particularly preferably 50% by mass or less in order to enhance the effect of the present invention.

[0059] The amount of the component (B) in the positive photoresist composition of the present invention is 20 to 70% by mass, preferably 25 to 60% by mass, based on the total amount of the component (A) and the component (C) described below.

[0060] When the amount of component (B) is set to be equal to or greater than the lower limit, an image faithful to the pattern can be obtained, while when it is set to be equal to or less than the upper limit, sensitivity degradation can be prevented and the homogeneity and resolution of the formed resist film can be improved.

[0061] In the semiconductor field including display panels (LCD), resist materials having a sensitivity in the range of 30 to 50 mJ are required from the perspectives of improving productivity and process controllability.

[0062] In addition, in the manufacture of semiconductor components, the largest silicon wafer used is a disk-shaped wafer with a diameter of 8 inches (about 200 mm) to 12 inches (about 300 mm), while in the manufacture of LCDs, the smallest square glass substrate used is 360 mm × 460 mm. Therefore, from the perspective of improving production capacity, it is hoped that the exposure area will be as large as possible, at least as large as 100 mm. 2 In the manufacture of LCD, it is generally preferred to use an exposure process under conditions of relatively low NA (numerical aperture of the lens). When manufacturing a system LCD, in order to form an integrated circuit portion on the substrate in addition to the display portion, the substrate tends to be further enlarged, and it is required to perform exposure under conditions of lower NA than in the usual LCD manufacturing. It is preferred to use an exposure process under conditions of low NA of 0.3 or less, and particularly preferably, 0.2 or less.

[0063] Furthermore, in a display panel LCD, for example, the pattern size of the display portion is 2 to 10 μm, while the integrated circuit portion is formed with a fine size of 0.5 to 2.0 μm. Therefore, it is preferable to be able to form a fine resist pattern of 0.5 to 2.0 μm. However, when performing exposure processing under the low NA condition as described above, there is a problem of poor resolution.

[0064] In addition, the positive photoresist composition used in the manufacture of display panels LCD is required to have good linear properties that can simultaneously and correctly form anti-etching patterns of display parts and integrated circuit parts with large size differences. Moreover, since a glass substrate with lower surface smoothness than a silicon wafer is used, good depth of focus (DOF) characteristics are also required.

[0065] According to the present invention, by using a specific multi-strong integral compound represented by the general formula (I) and a reaction product of naphthoquinone diazide sulfonyl chloride (II) as the component (B), a positive photoresist composition can be obtained which satisfies both high sensitivity and high resolution even under low NA conditions and has excellent properties such as linearity and DOF.

[0066] <(C) Ingredients>

[0067] Component (C) is a phenolic hydroxyl group-containing compound. By using the component (C), a positive photoresist composition suitable for system LCD can be obtained, which has excellent sensitivity improvement effect, high sensitivity and high resolution even in i-line exposure processing under low NA conditions, and good linearity.

[0068] The molecular weight (M) of the component (C) is preferably 1,000 or less, preferably 700 or less, and substantially 200 or more, preferably 300 or more.

[0069] Component (C) is a phenolic hydroxyl compound generally used as a sensitivity improver or sensitizer in resist compositions, preferably one that satisfies the above molecular weight conditions, and is not particularly limited, and one or more of them can be arbitrarily selected for use. Among them, the phenol compound represented by the following general formula (III) exhibits good above-mentioned properties.

[0070]

[0071] In the formula, R 4 ~R 11 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or a cycloalkyl group having 3 to 6 carbon atoms; R 13 , R 14 Each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R 12 It can be a hydrogen atom or an alkyl group with 1 to 6 carbon atoms. In this case, Q 1 It is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a residue represented by the following chemical formula (IV).

[0072]

[0073] (Where R 15 and R 16 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or a cycloalkyl group having 3 to 6 carbon atoms; g represents an integer of 0 to 3), Q 1 You can also use R 12 The end of Q 1 and R 12 and Q 1 and R 12 The carbon atoms between represent a cycloalkyl group with a carbon chain of 3 to 6; e and f represent integers of 1 to 3, and h represents an integer of 0 to 3. When e, f or h is 3, R 6 , R 9 or R 11do not exist respectively; m represents an integer from 0 to 3.

[0074] From the viewpoint of effect, the blending amount of the component (C) is 10 to 70% by mass, preferably 20 to 60% by mass, based on the component (A).

[0075] <(D) Component>

[0076] Component (D) can be any general organic solvent used in resist compositions without particular limitation, and one or more thereof may be selected, and substances containing propylene glycol monoalkyl ether acetate and / or 2-heptanone are preferred in terms of excellent coating properties and excellent uniformity of film thickness of the resist film on a large glass substrate.

[0077] In addition, propylene glycol monoalkyl ether acetate and 2-heptanone may be used together, but use of each alone or in a mixture with other organic solvents is generally more preferable in terms of uniformity of film thickness during coating by a spin coating method or the like.

[0078] It is preferable that propylene glycol monoalkyl ether acetate is contained in (D)component in an amount of 50 to 100 mass %.

[0079] Propylene glycol monoalkyl ether acetate is a substance having a straight-chain or branched alkyl group having 1 to 3 carbon atoms. Among them, when propylene glycol monomethyl ether acetate (hereinafter referred to as PGMEA) is used, the film thickness uniformity of the resist film on a large glass substrate is very good, so it is particularly ideal.

[0080] On the other hand, the use of 2-heptanone is not particularly limited, but is a relatively suitable solvent when combined with a non-benzophenone-based photosensitive component of (B) naphthoquinone diazide ester, as described above.

[0081] 2-Heptanone has excellent heat resistance compared to PGMEA and has the characteristics of being able to obtain a resist composition with less scum, and is therefore a very ideal solvent.

[0082] When 2-heptanone is used alone or in a mixture with other organic solvents, it is preferably contained in the component (D) in an amount of 50 to 100% by mass.

[0083] Furthermore, the above-mentioned preferred solvents may be used in combination with other solvents.

[0084] For example, when an alkyl lactate such as methyl lactate or ethyl lactate (preferably ethyl lactate) is added, it is preferable because a resist pattern having excellent uniformity in thickness of the resist film and good shape can be formed.

[0085] When propylene glycol monoalkyl ether acetate and alkyl lactate are used in combination, the amount of ethyl lactate blended is 0.1 to 10 times, preferably 1 to 5 times, by mass ratio based on propylene glycol monoalkyl ether acetate.

[0086] In addition, organic solvents such as γ-butyrolactone and propylene glycol monobutyl ether may also be used.

[0087] When γ-butyrolactone is used, it is blended in an amount of 0.01 to 1 times, preferably 0.05 to 0.5 times, based on propylene glycol monoalkyl ether acetate in terms of mass ratio.

[0088] In addition, other organic solvents that can be used include the following:

[0089] That is, ketones such as acetone, methyl ethyl ketone, cyclohexanone, and methyl isoamyl ketone; polyvalent alcohols such as ethylene glycol, propylene glycol, diethylene glycol, ethylene glycol monoacetate, propylene glycol monoacetate, diethylene glycol monoacetate, or their monomethyl ether, monoethyl ether, monopropyl ether, monobutyl ether, or monophenyl ether, and their derivatives; cyclic ethers such as dioxane; and esters such as methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, and ethyl ethoxypropionate.

[0090] When the above solvent is used, it is preferable that the content of the solvent in the component (D) is 50% by mass or less.

[0091] Without prejudice to the purpose of the present invention, the positive photoresist composition of the present invention may also contain compatible additives as needed, for example, resins added to improve the performance of the resist film, plasticizers, storage stabilizers, surfactants, colorants for making the developed image clearer, sensitizers for further enhancing the sensitization effect, dyes for reducing haloing, adhesion enhancers, and other conventional additives.

[0092] The following ultraviolet absorbers can be used as dyes for reducing halo, such as: 2,2′,4,4′-tetrahydroxybenzophenone, 4-dimethylamino-2′,4′-dihydroxybenzophenone, 5-amino-3-methyl-1-phenyl-4-(4-hydroxyphenylazo)pyrazole, 4-dimethylamino-4′-hydroxyazobenzene, 4-diethylamino-4′-ethoxyazobenzene, 4-diethylaminoazobenzene, curcumin, etc.

[0093] Surfactants can be added to prevent the formation of streaks, etc. For example, the following surfactants can be used: Fluoro-do FC-430, FC431 (trade names, manufactured by Sumitomo 3M Co., Ltd.), Eftectro EF122A, EF122B, EF122C, EF126 (trade names, manufactured by To-Kemu Project Co., Ltd.), and other fluorine-based surfactants, Megafilter R-08 (trade name, manufactured by Dainippon Ink and Chemicals Co., Ltd.), etc.

[0094] A preferred method for preparing the positive photoresist composition of the present invention is to dissolve the component (A), the component (B), the component (C), and other components used as required in the organic solvent (D).

[0095] In order to dissolve components (A) to (C) and other components used as needed, a uniform positive photoresist composition can be obtained, and the amount of component (D) used can be appropriately adjusted. The solid content concentration [components (A) to (C) and other components used as needed] is preferably 10 to 50% by mass, more preferably 20 to 35% by mass.

[0096] The positive photoresist composition of the present invention is preferably modulated so that the Mw (hereinafter referred to as the resist molecular weight) of the solid component contained in the photoresist composition is in the range of 5000 to 30000, and the more preferred Mw is 6000 to 10000. By setting the Mw of the solid component of the photoresist composition to the above range, high resolution can be achieved without reducing the sensitivity, and a positive photoresist composition with excellent linearity and DOF characteristics and excellent heat resistance can be obtained. By setting the Mw of the solid component of the photoresist composition to the above range, high resolution can be achieved without reducing the sensitivity, and a positive photoresist composition with excellent linearity and DOF characteristics and excellent heat resistance can be obtained.

[0097] When the photoresist molecular weight is below the above range, the resolution, linearity, DOF characteristics and heat resistance become insufficient, while when it exceeds the above range, the sensitivity decreases significantly and the coating properties of the resist composition may be impaired.

[0098] In this specification, the molecular weight of the resist can be measured by the following GPC system.

[0099] Device name: SYSTEM11 (product name, made by Showa Denko Co., Ltd.)

[0100] Pre-column: KF-G (product name, manufactured by Shodex)

[0101] Column: KF-805, KF-803, KF-802 (product name, manufactured by Shodex)

[0102] Detector: UV41 (product name, manufactured by Shodex), measurement at 280 nm.

[0103] Solvent etc.: Tetrahydrofuran was flowed at a flow rate of 1.0 ml / min, and the measurement was performed at 35°C.

[0104] Preparation method of measurement sample: The photoresist composition to be measured is adjusted so that the solid content concentration is 30% by mass, and it is diluted with tetrahydrofuran to prepare a measurement sample with a solid content concentration of 0.1% by mass. 20 microliters of the measurement sample is injected into the above-mentioned device for measurement.

[0105] In addition, in the manufacture of display panels LCD, the use of i-line (365nm) exposure with a shorter wavelength instead of the g-line (436nm) exposure used in the manufacture of LCDs in the past may improve resolution. Accordingly, the positive photoresist composition of the present invention using a non-benzophenone compound as the (B) component and the optional (C) component can suppress the absorption of the i-line caused by the (B) component and the (C) component, and is therefore suitable for i-line exposure processing, and can achieve further high resolution.

[0106] In the modulation of the positive photoresist composition of the present invention, the following modulation methods can be listed as methods for making the molecular weight of the resist fall within the above-mentioned appropriate range: (1) a method in which component (A) is subjected to a fractionation operation before mixing so as to make the Mw of all components after mixing fall within the above-mentioned range, thereby pre-adjusting the Mw of component (A) to an appropriate range; (2) a method in which a plurality of components (A) having different Mw are prepared and appropriately combined to adjust the Mw of the solid component to fall within the above-mentioned range.

[0107] In particular, the modulation method (2) is more preferable in that the molecular weight of the photoresist and the sensitivity can be easily adjusted.

[0108] 《Method for forming resist pattern》

[0109] The following is an example of a preferred method for forming a resist pattern when a display panel LCD is manufactured using the positive photoresist composition of the present invention.

[0110] First, the positive photoresist composition of the present invention is coated on a substrate using a spin coater to form a coating film. A glass substrate is preferred as the substrate. Amorphous silicon is generally used as the glass substrate, and in the field of display panels LCD, low-temperature polycrystalline silicon is preferred. Since the positive photoresist composition of the present invention has excellent resolution under low NA conditions, a large substrate of 550 mm × 650 mm or more can be used as the glass substrate.

[0111] Next, the glass substrate with the coating film formed thereon is subjected to a heating treatment (pre-baking) at 100-140° C. to remove the remaining solvent and form a resist film. A preferred pre-baking method is proximity baking with a space between the hot plate and the substrate.

[0112] Then, the resist film is selectively exposed using a mask having a mask pattern drawn thereon.

[0113] In order to form a fine pattern, i-line (365 nm) is preferably used as a light source. In addition, the exposure treatment used in the exposure is preferably exposure under low NA conditions with NA of 0.3 or less, preferably 0.2 or less, and more preferably 0.15 or less.

[0114] Next, the selectively exposed resist film is subjected to a heat treatment (post-exposure baking: PEB). Examples of PEB methods include proximity baking with a gap between the hot plate and the substrate and direct baking without a gap. In order to prevent the substrate from warping and obtain the diffusion effect produced by PEB, it is best to perform proximity baking followed by direct baking. In addition, the heating temperature is preferably 90 to 150°C, particularly preferably 100 to 140°C.

[0115] The resist film after PEB is developed using a developer, for example, an alkaline aqueous solution such as a 1 to 10 mass % tetramethylammonium hydroxide aqueous solution, and the exposed portion is dissolved and removed, so that a resist pattern for the integrated circuit and a resist pattern for the liquid crystal display portion can be formed on the substrate at the same time.

[0116] Then, the developer remaining on the surface of the resist pattern is washed away with a rinse solution such as pure water to form a resist pattern.

[0117] In the method for forming the resist pattern, in the process of performing the above-mentioned selective exposure when manufacturing the display panel LCD, it is preferred to use as the mask a mask having a resist pattern forming mask pattern of less than 2.0 μm or a resist pattern forming mask pattern of more than 2.0 μm.

[0118] The positive photoresist composition for LCD of the present invention has excellent resolution, so that a resist pattern with a fine pattern faithfully reproducing the mask pattern can be obtained. Therefore, in the process of simultaneously forming the resist pattern, a resist pattern for an integrated circuit with a pattern size of 2.0 μm or less or a resist pattern for a liquid crystal display portion with a pattern size of more than 2.0 μm can be simultaneously formed on the substrate. Example

[0119] The present invention is described in detail below with reference to examples.

[0120] Resist patterns were formed by the following procedures using the positive photoresist compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 2, and were evaluated.

[0121] Evaluation Method

[0122] (1) Formation of resist pattern

[0123] A positive photoresist composition was coated on a glass substrate (550 mm × 650 mm) with a Ti film formed thereon using a large-scale resist coating apparatus for substrates (apparatus name: TR36000, manufactured by Tokyo Ohka Industry Co., Ltd.). The temperature of the hot plate was then raised to 100°C, and the first drying was performed for 90 seconds by adjacent drying at an interval of about 1 mm. The temperature of the hot plate was then lowered to 90°C, and the second drying was performed for 90 seconds by adjacent drying at an interval of about 0.5 mm, thereby forming a resist film with a thickness of 1.5 μm.

[0124] Then, using a test pattern mask (レチクル) having mask patterns for simultaneously reproducing a 3.0μm L&S resist pattern and a 1.5μm L&S resist pattern, selective exposure was performed using an i-line exposure device (device name: FX-702J, manufactured by Nikon; NA=0.14) with an exposure amount (Eop exposure amount) that can faithfully reproduce a 1.5μm L&S.

[0125] Next, the hot plate was heated to 120° C., and a heating treatment was performed for 30 seconds by proximity drying with a gap of 0.5 mm, and then a heating treatment was performed for 60 seconds by direct drying without a gap at the same temperature.

[0126] Then, using a developing device with a slit coater nozzle (device name: TD-39000 Developer, manufactured by Tokyo Ohka Industry Co., Ltd.), a 23°C, 2.38 mass % TMAH aqueous solution was evenly spread on the substrate over 10 seconds, maintained for 55 seconds, washed with water for 30 seconds, and spin dried.

[0127] (2) Evaluation of sensitivity and residual film rate

[0128] Photoresist composition stability test:

[0129] The photoresist compositions prepared in the examples and comparative examples were stored in a constant temperature oven at 25° C., and samples were taken for testing on the 20th, 30th and 40th days;

[0130] Spin-coat the photoresist on the silicon wafer, dry it in a vacuum oven (VCD), and bake it on a hot plate at 110°C for 90 seconds to form a photoresist coating. The coating thickness is about 1.5 μm as measured by a film thickness meter.

[0131] Then, the photoresist layer was exposed to different energies using an exposure machine containing g+h+i wavelengths. After exposure, it was developed with 2.38wt% tetramethylammonium hydroxide (TMAH) for 70s, washed with water for 25s, and then dried to remove the exposed part to form a photoresist pattern.

[0132] Evaluation of the stability of the photoresist composition: The thickness of the photoresist layer before and after exposure was checked by a film thickness meter, and the residual film rate of the photoresist was calculated;

[0133] Record the energy required for complete exposure and development, and calculate the sensitivity of the photoresist.

[0134] The stability of photoresist is evaluated based on sensitivity and residual film rate. (Resist composition)

[0135] The following materials were prepared as components (A) to (D).

[0136] (A)Ingredients:

[0137] (A1) A novolac resin having Mw=20000 and Mw / Mn=5.2 synthesized by a conventional method using 1 mol of a mixed phenol of m-cresol / 3,4-xylenol=8 / 2 (mol ratio) and 0.82 mol of formaldehyde

[0138] (B) Ingredients:

[0139] Nitrogen was introduced into a 500 mL four-necked flask, and 270 mL of 1,4-dioxane, a raw material polyhydroxyphenol (I) and diazonaphthoquinonesulfonyl chloride (II) were added in a nitrogen atmosphere in a ratio of 1:3.7 mol, and the mixture was stirred and mixed evenly, and the system temperature was maintained at 25-30° C.; the temperature was raised to 30° C., and 10.0 g of triethylamine was slowly added dropwise, and the addition was completed within 3.0 hours; the system temperature was maintained at 30-33° C., and the stirring reaction was continued for about 1.0 hour, and the reaction was completed; the precipitated solid in the system was filtered out, and the mother liquor was slowly added into 1000 mL of pre-prepared 1.0 wt% dilute hydrochloric acid, stirred for crystallization for 1.0 hour, and filtered; the filter cake was washed three times with pure water and filtered; the wet filter cake was dried at 150 mbar and 40° C. to obtain a light yellow solid product.

[0140] The following product B was obtained by the above method.

[0141]

[0142]

[0143] Table 1

[0144] (C) Ingredients:

[0145] (C1) Bis(5-cyclohexyl-4-hydroxy-2-methylphenyl)-3,4-dihydroxyphenylmethane

[0146] (D) Ingredients:

[0147] (D1)PGMEA

[0148] (Examples 1 to 5, Comparative Examples 1 to 2)

[0149] The components (A) to (C) were used in the amounts shown in Table 2. A surfactant (product name: "Megafilter R-08"; manufactured by Dainippon Ink & Chemicals Co., Ltd.) was used in an amount equivalent to 450 ppm based on the total weight of the components (A) to (C). These components were dissolved in the component (D) shown in Table 2, and then filtered with a membrane filter having a pore size of 0.2 μm to prepare a positive photoresist composition. The molecular weight of the resist of the obtained positive photoresist composition is shown in Table 2.

[0150] The obtained positive photoresist composition was evaluated for each of the items (1) to (2). The results are shown in Table 3.

[0151]

[0152] Table 2

[0153] Wherein: compound (VI) is TPPA-PAC (Toyo Gosei Kogyo Co., Ltd., Japan); compound (VII) is THPE-PAC (Miwon Specialty Chemical Co., Ltd., South Korea).

[0154]

[0155]

[0156] Table 3

[0157] It can be seen from the above test results that, compared with Examples 1 to 5, as time goes by, the sensitivity and residual film rate of Comparative Examples 1 to 2 are increasingly different from the measurement results at 20 days, and the stability is poor; the photoresist compositions provided by Examples 1 to 5 within the scope of the present invention have excellent sensitivity and stability, and a high residual film rate, compared with the photoresist compositions prepared using photosensitizers that have been widely commercialized on the market.

[0158] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A positive photoresist composition, characterized in that: The invention comprises (A) an alkali-soluble resin, (B) a naphthoquinone diazide sulfonate, (C) a phenolic hydroxyl group-containing compound having a molecular weight of 1000 or less, and (D) an organic solvent, wherein the component (B) comprises a reaction product of a polyhydroxyphenol compound represented by the following general formula (I) and a naphthoquinone diazide sulfonyl chloride represented by (II), wherein R1, R2, and R3 each independently represent hydrogen, halogen, C1-C18 straight or branched alkyl, C6-C12 aryl, C1-C8 alkoxy, C1-C8 alkylthio, C2-C10 unsaturated hydrocarbon group, C3-C12 cycloalkyl group, C4-C12 cycloalkylalkyl group, C1-C9 alkanoyl, C7-C13 aromatic acyl, C3-C6 heterocyclic group in which carbon or hydrogen atoms are selectively substituted by O, S or N atoms, C1-C18 alkylamino or aromatic amino; a, b, c each independently represent an integer between 0 and 2; x, y, z each independently represent an integer between 0 and 3; the diazonaphthoquinonesulfonyl chloride (II) is one of the following structural compounds; 2. The positive photoresist composition according to claim 1, wherein the component (B) contains the reaction product of a polyhydroxyphenol represented by diazonaphthoquinonesulfonyl chloride, wherein R1, R2, and R3 in the general formula (I) each independently represent hydrogen, a C1-C6 straight chain or branched alkyl group, a C6-C12 aromatic group, a C1-C6 alkoxy group, and (II).

3. The positive photoresist composition according to claim 1, wherein the component (B) contains at least one polyhydroxyphenol compound (I) selected from the following structural compounds: 4 . The positive photoresist composition according to claim 1 , wherein the component (D) contains propylene glycol monoalkyl ether acetate and / or 2-heptanone. The positive photoresist composition according to claim 1 , which is used for i-line exposure process. The positive photoresist composition according to claim 1 , which is used for exposure processing with NA below 0.

3.

7. A method for forming an anti-etching pattern, comprising the following steps: (1) coating a substrate with a positive photoresist composition as described in any one of claims 1 to 6 to form a coating film; (2) heating the substrate on which the coating film is formed to form an anti-etching film on the substrate; (3) selectively exposing the anti-etching film using a mask having a mask pattern for forming an anti-etching pattern of less than 2.0 μm and a mask pattern for forming an anti-etching pattern of more than 2.0 μm; (4) heating the selectively exposed anti-etching film; (5) developing the heat-treated anti-etching film in (4) with an alkaline aqueous solution to simultaneously form an anti-etching pattern for an integrated circuit with a pattern size of less than 2.0 μm and an anti-etching pattern for a liquid crystal display portion with a pattern size of more than 2.0 μm on the substrate.

8. The method for forming a resist pattern according to claim 6, wherein the step of (3) performing selective exposure uses i-line as a light source and is performed by exposure treatment under a low NA condition of 0.3 or less.