Transparent conductive film, method for preparing transparent conductive film, and photoelectric device

Through the laminated structure and plasma enhanced chemical vapor deposition technology, the organic-inorganic hybrid layer is formed, which solves the problems of high resistance and poor flexibility of traditional transparent conductive films, and achieves a transparent conductive film with high stability and moisture and heat resistance, which is suitable for Flexible optoelectronic devices.

CN118737531APending Publication Date: 2024-10-01CHINA LUCKY GROUP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410862120.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Due to performance limitations such as high resistance and poor flexibility, traditional ITO transparent conductive films are difficult to meet the needs of flexible optoelectronic technology. Moreover, the metal silver layer has poor moisture and heat resistance, which can easily lead to apparent defects and performance degradation.

Method used

A transparent conductive film with a laminated structure of a transparent substrate, a first transparent dielectric layer, a metal layer, a hybrid layer and a second transparent dielectric layer is used. The hybrid layer is composed of organic silicon oxide and inorganic silicon oxide, and is deposited through plasma enhanced chemical vapor deposition. A hybrid layer is formed, and the dielectric layer is prepared by combining magnetron sputtering to improve the bonding force and stability of the film layer.

Benefits of technology

A transparent conductive film with low resistance, high transparency, and good flexibility is achieved, which significantly improves the stability and moisture and heat resistance of the film. The resistance does not increase by more than 30% after aging for 1,000 hours in an environment of 60°C and 90% RH.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737531A_ABST
    Figure CN118737531A_ABST
Patent Text Reader

Abstract

The invention discloses a transparent conductive film, a method for preparing the transparent conductive film and a photoelectric device. The transparent conductive film comprises a transparent substrate, a first transparent dielectric layer, a metal layer, a hybrid layer and a second transparent dielectric layer which are sequentially stacked, the hybrid layer is made of organic silicon oxide and inorganic silicon oxide, and the second transparent dielectric layer is made of inorganic matter. Therefore, the hybrid layer contains an organic matter and an inorganic matter, polar groups, free radicals and the like in the organic matter can improve the cohesiveness of the film layer and an adjacent film layer, inorganic silicon oxide in the hybrid layer and the second transparent dielectric layer belong to inorganic matter, the binding force is matched, the binding strength is higher, and therefore the overall fastness of the transparent conductive film can be improved; the hybrid layer can prevent small-molecule free substances from permeating and diffusing in the inner layer of the conductive film, can prevent the metal layer from migrating to damage the fastness of the film layer, and is beneficial to improving the stability of the transparent conductive film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite conductive films, and in particular to a transparent conductive film, a method for preparing the transparent conductive film, and a photoelectric device. Background Art

[0002] With the rapid development of flexible optoelectronic technology, the traditional ITO transparent conductive film has been unable to meet the needs of applications due to performance limitations such as high resistance and poor flexibility. In recent years, some transparent conductive films that can serve as substitutes for ITO have emerged, such as carbon nanotubes, graphene, conductive polymers, metal films, metal nanowires, metal grids, flexible multilayer conductive films, etc. Among them, the dielectric layer / metal layer / dielectric layer structure laminated transparent conductive film has attracted widespread attention because the metal layer has excellent conductivity and ductility, and the transmittance of the film can be improved by regulating the dielectric layer, so that it has the characteristics of low resistance, high transmittance, and high flexibility. Metallic silver has the lowest optical loss in the visible light band and the lowest resistivity (1.62×10 -8 Ω·m), and is often used as a metal layer in laminated transparent conductive films. However, metallic silver itself is highly active and unstable, and since a silver layer reaches a certain thickness, it will lead to high reflectivity. Therefore, the silver layer of the laminated transparent conductive film needs to be as thin as possible, resulting in poor moisture and heat resistance of the metallic silver layer, and prone to problems such as apparent defects and performance degradation, which seriously affects the practical application of the laminated transparent conductive film.

[0003] Therefore, the current transparent conductive film, method for preparing the transparent conductive film and optoelectronic device still need to be improved. Summary of the invention

[0004] The present invention aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.

[0005] In one aspect of the present invention, the present invention proposes a transparent conductive film. In some embodiments of the present invention, the transparent conductive film includes a transparent substrate, a first transparent dielectric layer, a metal layer, a hybrid layer and a second transparent dielectric layer stacked in sequence, the material of the hybrid layer includes organic silicon oxide and inorganic silicon oxide, and the material of the second transparent dielectric layer is inorganic. Thus, the hybrid layer contains organic and inorganic substances, and the polar groups, free radicals, etc. in the organic substances can improve the adhesion between the film layer and the adjacent film layer. The inorganic silicon oxide in the hybrid layer and the second transparent dielectric layer belong to the same inorganic substance, and the binding force matches, and the binding strength is higher, which is conducive to improving the overall fastness of the transparent conductive film; the hybrid layer can block the penetration and diffusion of small molecular free substances in the inner layer of the conductive film, and can prevent the migration of the metal layer from damaging the fastness of the film layer, which is conducive to improving the stability of the transparent conductive film.

[0006] In some embodiments of the present invention, the thickness of the hybrid layer is 10 nm-30 nm. Thus, the film layer has good light transmittance and good water vapor barrier effect, which is conducive to further improving the stability of the transparent conductive film.

[0007] In some embodiments of the present invention, the metal layer is made of an alloy of silver and at least one element selected from copper, palladium, niobium, tin, indium, antimony, aluminum, titanium, nickel and chromium; and / or the thickness of the metal layer is 3nm-20nm. Thus, the metal layer has excellent electrical conductivity and high light transmittance.

[0008] In some embodiments of the present invention, the material of the first transparent dielectric layer and the material of the second transparent dielectric layer independently include one or more of metal oxide, metal oxide dopant, metal sulfide, metal fluoride, silicon oxide and silicon nitride; and / or the thickness of the first transparent dielectric layer and the thickness of the second transparent dielectric layer independently range from 5nm to 100nm. Thus, it is beneficial to improve the light transmittance of the transparent conductive film and can protect the intermediate film layer.

[0009] In some embodiments of the present invention, the transparent conductive film satisfies at least one of the following conditions: the material of the first transparent dielectric layer and the material of the second transparent dielectric layer independently include one or more of indium tin oxide, niobium pentoxide, titanium dioxide, bismuth oxide, tungsten trioxide, nickel oxide, zinc oxide, gallium zinc oxide, indium zinc oxide, silicon dioxide, hafnium dioxide, zirconium oxide, aluminum-doped zinc oxide, aluminum oxide, indium oxide, tin dioxide, zinc sulfide, silicon nitride and magnesium fluoride; the material of the transparent substrate includes one or more of polyethylene terephthalate, polyimide, polyethylene naphthalate, polycarbonate, polystyrene and cellulose triacetate; the thickness of the transparent substrate is 1 μm-500 μm; after aging for 1000 hours at 60°C and 90% RH, the resistance of the transparent conductive film does not increase by more than 30%.

[0010] In another aspect of the present invention, the present invention proposes a method for preparing the transparent conductive film described above. In some embodiments of the present invention, the method for preparing the transparent conductive film described above includes: providing a transparent substrate; sequentially forming a first transparent dielectric layer, a metal layer, a hybrid layer and a second transparent dielectric layer on one side of the transparent substrate; wherein the hybrid layer is formed by the following steps: placing the transparent substrate formed with the first transparent dielectric layer and the metal layer in a plasma enhanced chemical vapor deposition device, introducing organic silicon, oxygen-containing gas and inert gas, and performing plasma enhanced chemical vapor deposition to form a hybrid layer on the surface of the metal layer away from the transparent substrate. Thus, plasma enhanced chemical vapor deposition can utilize glow discharge to decompose organic silicon, generate active groups to promote plasma reaction, deposit thin films at a lower temperature, and will not cause damage to the metal layer. Moreover, this method can significantly improve the bonding quality between the metal film layer and the second transparent dielectric layer, and significantly improve the bonding strength between the film layers.

[0011] In some embodiments of the present invention, the organosilicon includes one or more of tetramethyldisiloxane, hexamethyldisiloxane, vinyltrimethylsilane, hexamethyldisilane, methylsilane, dimethylsilane, trimethylsilane, diethylsilane, propylsilane, phenylsilane, vinyltriethoxysilane, vinyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane and octamethylcyclotetrasiloxane; and / or, the oxygen-containing gas includes one or more of oxygen, carbon monoxide and ozone; and / or, the inert gas includes argon. The above-mentioned organosilicon can be cracked under glow discharge conditions and react with the oxygen-containing gas to deposit and form a hybrid layer having both organic silicon oxide and inorganic silicon oxide.

[0012] In some embodiments of the present invention, the organosilicon includes at least one of tetraethoxysilane and hexamethyldisiloxane; and / or the oxygen-containing gas includes oxygen.

[0013] In some embodiments of the present invention, the first transparent dielectric layer and the second transparent dielectric layer are both formed by magnetron sputtering. The dielectric layer formed by magnetron sputtering has good film uniformity and high light transmittance, which is beneficial to improving the overall performance of the transparent conductive film.

[0014] In another aspect of the present invention, the present invention provides a photoelectric device. In some embodiments of the present invention, the photoelectric device includes a transparent electrode, and the transparent electrode includes the transparent conductive film described above. Therefore, the photoelectric device has all the characteristics and advantages of the transparent conductive film described above, which will not be repeated here. In general, the photoelectric device has good stability and a long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0016] Figure 1 A schematic structural diagram of a transparent conductive film according to an embodiment of the present invention is shown;

[0017] Figure 2 A schematic diagram of the structure of a transparent conductive film in related art is shown.

[0018] Description of reference numerals:

[0019] 11: transparent substrate; 12: first transparent dielectric layer; 13: metal layer; 14: hybrid layer; 15: second transparent dielectric layer. DETAILED DESCRIPTION

[0020] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0021] In one aspect of the present invention, the present invention provides a transparent conductive film. In some embodiments of the present invention, reference Figure 1 The transparent conductive film may include a transparent substrate 11, a first transparent dielectric layer 12, a metal layer 13, a hybrid layer 14 and a second transparent dielectric layer 15 stacked in sequence, wherein the material of the hybrid layer 14 may include organic silicon oxide and inorganic silicon oxide, and the material of the second transparent dielectric layer 15 is inorganic. A hybrid layer is arranged between the metal layer and the second transparent dielectric layer, and the main components of the hybrid layer are organic silicon oxide and inorganic silicon oxide. The hybrid layer contains organic chain breakers such as -CH 3 Groups, etc. These polar groups, free radicals, etc. can make the hybrid layer have high adhesion with the adjacent film layer. At the same time, the inorganic silicon oxide contained in the hybrid layer and the second transparent dielectric layer are both inorganic substances, and the bonding force is matched, which is beneficial to further improve the fastness of the transparent conductive film; in addition, the Si-O atomic distance (about 0.1nm) is smaller than the equivalent kinetic diameter of water vapor molecules (about 0.3nm), which can block the penetration and diffusion of small molecular free substances (including water and oxygen) in the inner layer of the transparent conductive film, and can at least prevent the migration of the metal layer from damaging the fastness of the transparent conductive film to a certain extent, which is beneficial to improve the stability of the transparent conductive film.

[0022] In some embodiments of the present invention, the hybrid layer has more Si-O bonds, which is beneficial to improving the water and oxygen barrier properties of the transparent conductive film. In some embodiments of the present invention, the hybrid layer has more C (carbon) elements, which is beneficial to improving the adhesion of the hybrid layer, thereby improving the bonding strength between the hybrid layer and the metal layer and the second transparent dielectric layer.

[0023] In some embodiments of the present invention, the thickness of the hybrid layer 14 can be 10nm-30nm. For example, the thickness of the hybrid layer 14 can be 10nm, 15nm, 20nm, 25nm, 30nm, etc. Therefore, the hybrid layer is a continuous film layer, which has a good barrier effect on water, oxygen, etc., and the hybrid layer has good light transmittance and a thin thickness, and has no obvious adverse effect on the conductivity of the transparent conductive layer.

[0024] In some preferred embodiments of the present invention, the thickness of the hybrid layer 14 may be 10 nm-25 nm, so that the hybrid layer has a higher light transmittance and can play a better water and oxygen barrier effect, thereby helping to further improve the overall performance of the transparent conductive layer.

[0025] In some embodiments of the present invention, the material of the transparent substrate 11 may include one or more of polyethylene terephthalate (PET), polyimide (PI), polyethylene naphthalate (PEN), polycarbonate (PC), polystyrene (PS) and triacetyl cellulose (TAC). The transparent substrate of the above materials has good light transmittance and good flexibility, which is conducive to improving the flexibility of the transparent conductive film so that the transparent conductive film can be applied to flexible optoelectronic devices. In some specific embodiments of the present invention, the transparent substrate 11 may be a PET film layer, a PI film layer, a PEN film layer, a PC film layer, a PS film layer or a TAC film layer. In other embodiments of the present invention, the transparent substrate 11 may also be a composite film layer composed of at least two of the PET film layer, the PI film layer, the PEN film layer, the PC film layer, the PS film layer and the TAC film layer.

[0026] In some embodiments of the present invention, the thickness of the transparent substrate 11 can be 1μm-500μm. For example, the thickness of the transparent substrate 11 can be 1μm, 10μm, 50μm, 100μm, 300μm, 500μm, etc. Therefore, the transparent substrate has certain light transmittance and flexibility, which is beneficial to improving the overall performance of the transparent conductive film.

[0027] In some preferred embodiments of the present invention, the thickness of the transparent substrate 11 can be 100μm-188μm. For example, the thickness of the transparent substrate 11 can be 120μm, 130μm, 150μm, 160μm, 180μm, etc. The thickness of the transparent substrate is within the above range, the light transmittance is high, the flexibility is good, and it can also provide good support for the film layer thereon, which is beneficial to further improve the overall performance of the transparent conductive film.

[0028] In some embodiments of the present invention, the material of the metal layer 13 may be an alloy of silver and at least one element selected from copper, palladium, niobium, tin, indium, antimony, aluminum, titanium, nickel and chromium. The metal layer of the above material has excellent electrical conductivity and good stability, which is conducive to improving the overall performance of the transparent conductive film. In some specific embodiments of the present invention, the material of the metal layer 13 may be a silver-copper alloy, a silver-palladium alloy, a silver-niobium alloy, a silver-tin alloy, a silver-indium alloy, a silver-antimony alloy, a silver-aluminum alloy, a silver-titanium alloy, a silver-nickel alloy or a silver-chromium alloy. In other embodiments of the present invention, the material of the metal layer 13 may also be an alloy of silver and at least two elements selected from copper, palladium, niobium, tin, indium, antimony, aluminum, titanium, nickel and chromium.

[0029] In some embodiments of the present invention, the thickness of the metal layer 13 can be 3nm-20nm. For example, the thickness of the metal layer 13 can be 3nm, 5nm, 10nm, 15nm, 20nm, etc. Thus, the metal layer has a suitable thickness, low resistance, and high light transmittance.

[0030] In some preferred embodiments of the present invention, the thickness of the metal layer 13 may be 6 nm-16 nm. For example, the thickness of the metal layer 13 may be 6 nm, 8 nm, 11 nm, 12 nm, 14 nm, 16 nm, etc.

[0031] In some embodiments of the present invention, the material of the first transparent dielectric layer 12 and the material of the second transparent dielectric layer 15 can independently include one or more of metal oxides, metal oxide dopants, metal sulfides, metal fluorides, silicon oxides, and silicon nitrides. The first transparent dielectric layer and the second transparent dielectric layer made of the above materials can protect the intermediate film layer and have good light transmittance.

[0032] In some embodiments of the present invention, the material of the first transparent dielectric layer 12 and the material of the second transparent dielectric layer 15 can independently include one or more of indium tin oxide, niobium pentoxide, titanium dioxide, bismuth oxide, tungsten trioxide, nickel oxide, zinc oxide, gallium zinc oxide, indium zinc oxide, silicon dioxide, hafnium dioxide, zirconium oxide, aluminum-doped zinc oxide, aluminum oxide, indium oxide, tin dioxide, zinc sulfide, silicon nitride and magnesium fluoride.

[0033] In some embodiments of the present invention, the material of the first transparent dielectric layer 12 may be the same as the material of the second transparent dielectric layer 15. In other embodiments of the present invention, the material of the first transparent dielectric layer 12 may be different from the material of the second transparent dielectric layer 15.

[0034] In some embodiments of the present invention, the thickness of the first transparent dielectric layer 12 and the thickness of the second transparent dielectric layer 15 can be 5nm-100nm independently. For example, the thickness of the first transparent dielectric layer 12 and the thickness of the second transparent dielectric layer 15 can be 5nm, 10nm, 20nm, 50nm, 70nm, 100nm, etc. independently. When the thickness of the first transparent dielectric layer and the thickness of the second transparent dielectric layer are within the above range, the light transmittance is high, and the intermediate film layer can be well protected. In some preferred embodiments, the thickness of the first transparent dielectric layer 12 and the thickness of the second transparent dielectric layer 15 can be 20nm-80nm independently. In the present invention, the thickness of the first transparent dielectric layer 12 and the thickness of the second transparent dielectric layer 15 can be the same or different.

[0035] The transparent conductive film of the present invention is aged for 1000 hours in an environment of 60° C. and 90% RH, and the resistance increase does not exceed 30%, and the appearance is good.

[0036] In another aspect of the present invention, the present invention provides a method for preparing the transparent conductive film described above. In some embodiments of the present invention, the method for preparing the transparent conductive film described above may include the following steps: providing a transparent substrate; sequentially forming a first transparent dielectric layer, a metal layer, a hybrid layer, and a second transparent dielectric layer on one side of the transparent substrate.

[0037] In some embodiments of the present invention, the hybrid layer is formed by the following steps: placing a transparent substrate having a first transparent dielectric layer and a metal layer in a plasma enhanced chemical vapor deposition device, introducing organic silicon, oxygen-containing gas and inert gas, performing plasma enhanced chemical vapor deposition, and forming a hybrid layer on the surface of the metal layer away from the transparent substrate.

[0038] The hybrid layer is prepared by plasma enhanced chemical vapor deposition (PECVD). On the one hand, due to the strong concave-convex tracking and flattening of chemical vapor deposition, the surface of the metal layer can be perfectly covered, even defects and peaks can be well covered, thus playing a good passivation protection role for the metal layer, and the interlayer bonding force between the metal layer and the hybrid layer will be stronger; on the other hand, the organic silicon will be decomposed to form active groups under the action of glow discharge, and oxygen-containing gas will participate in the reaction, and a hybrid layer containing both organic silicon oxide and inorganic silicon oxide will be deposited at a lower temperature. The hybrid layer contains organic chain-breaking -CH3 These polar groups, free radicals, etc. can improve the adhesion between the hybrid layer and the adjacent film layer. In addition, the inorganic silicon oxide in the hybrid layer and the second transparent dielectric layer are both inorganic substances, and the bonding force is matched, which significantly improves the adhesion between the second transparent dielectric layer and the hybrid layer.

[0039] In some embodiments of the present invention, the organosilicon may include one or more of tetramethyldisiloxane, hexamethyldisiloxane, vinyltrimethylsilane, hexamethyldisilane, methylsilane, dimethylsilane, trimethylsilane, diethylsilane, propylsilane, phenylsilane, vinyltriethoxysilane, vinyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane and octamethylcyclotetrasiloxane. The above organosilicon can be cracked under the action of glow discharge and react with oxygen-containing gas to obtain a hybrid layer having both organic silicon oxide and inorganic silicon oxide.

[0040] In some embodiments of the present invention, the organosilicon may include at least one of tetraethoxysilane and hexamethyldisiloxane.

[0041] In some embodiments of the present invention, the oxygen-containing gas may include one or more of oxygen, carbon monoxide and ozone. The oxygen-containing gas may participate in the reaction, which is beneficial to increase the content of Si-O in the hybrid layer, thereby improving the water-oxygen barrier performance of the hybrid layer.

[0042] In some embodiments of the present invention, the oxygen-containing gas may include oxygen, which is environmentally friendly and does not have adverse effects on the health of operators.

[0043] In some embodiments of the present invention, the inert gas may include argon. In some specific embodiments of the present invention, the inert gas may be argon. Argon can form plasma and transfer energy. Gaseous substances are ionized under the action of plasma to form excited active groups, which diffuse to the substrate surface and then undergo chemical reactions to complete film growth.

[0044] In the present invention, deposition of films with different elemental components and properties can be achieved by adjusting process parameters such as the flow ratio of organic silicon and oxygen-containing gas, power, and working gas pressure.

[0045] In some embodiments of the present invention, when preparing the hybrid layer, the power may be 200W-800W, for example, the power may be 200W, 300W, 500W, 600W, 800W, etc.

[0046] In some embodiments of the present invention, when preparing the hybrid layer, the working pressure may be 0.5Pa-5Pa, for example, the working pressure may be 0.5Pa, 0.8Pa, 1Pa, 2Pa, 3Pa, 5Pa, etc.

[0047] In some embodiments of the present invention, when preparing the hybrid layer, the flow ratio of the organosilicon and the oxygen-containing gas can be 1:30-1:15, for example, the flow ratio of the organosilicon and the oxygen-containing gas can be 1:30, 1:25, 1:20, 1:15, etc.

[0048] The power, working pressure, and flow ratio of the organosilicon and the oxygen-containing gas satisfying the above conditions are conducive to obtaining a hybrid layer with excellent performance.

[0049] In some embodiments of the present invention, the first transparent dielectric layer and the second transparent dielectric layer can be formed by magnetron sputtering. The first transparent dielectric layer and the second transparent dielectric layer are formed by magnetron sputtering, and the film uniformity is good, which can play a better role in protecting the intermediate film layer.

[0050] In some embodiments of the present invention, a transparent substrate can be placed in a chamber, argon and oxygen are introduced to sputter the target material, and a first transparent dielectric layer is formed on the surface of the transparent substrate. The steps of forming the second transparent dielectric are the same as the steps of forming the first transparent dielectric layer, and are not repeated here. The specific conditions for forming the first transparent dielectric layer and the second transparent dielectric layer are not particularly limited in the present invention, and those skilled in the art can select and set them according to actual conditions.

[0051] The present invention does not specifically limit the method for preparing the metal layer, and those skilled in the art may select the method according to actual conditions.

[0052] The material and thickness of the transparent substrate, the material and thickness of the metal layer, the thickness of the hybrid layer, the material and thickness of the first transparent dielectric layer and the second transparent dielectric layer have been described in detail above and will not be repeated here.

[0053] In general, the method proposed in the present invention for preparing a transparent conductive film has the following beneficial effects: (1) A hybrid layer is formed between the metal layer and the second transparent dielectric layer by a plasma enhanced chemical vapor deposition (PECVD) method. Due to the strong concave-convex tracking and flattening of the chemical vapor deposition method, the hybrid layer can perfectly cover the surface of the metal layer, thereby providing a good passivation protection for the metal layer, and at the same time, the interlayer bonding force between the metal layer and the hybrid layer will be stronger. (2) Since the inorganic silicon oxide contained in the hybrid layer and the second transparent dielectric layer are both inorganic substances, the bonding force matches, which significantly improves the adhesion between the second transparent dielectric layer and the hybrid layer. (3) In the hybrid layer, the components of organic silicon oxide and inorganic silicon oxide have a barrier effect on small molecular free substances (including water and oxygen, etc.), which can effectively prevent the upper small molecular free substances (including water and oxygen) from corroding the metal layer, thereby improving the moisture and heat resistance of the transparent conductive film. (4) Furthermore, after a hybrid layer is added between the metal layer and the second transparent dielectric layer, the second transparent dielectric layer is prepared on its surface by a magnetron sputtering process. Since the hybrid layer has etching resistance, the damage to the metal layer surface caused by the magnetron sputtering process of the second transparent dielectric layer can be significantly reduced.

[0054] In another aspect of the present invention, the present invention provides a photoelectric device. In some embodiments of the present invention, the photoelectric device may include a transparent electrode, and the transparent electrode may include the transparent conductive film described above. Therefore, the photoelectric device has all the features and advantages of the transparent conductive film described above, which will not be described in detail here.

[0055] In some embodiments of the present invention, the optoelectronic device may be a touch screen, a liquid crystal dimming film, an electrochromic device, a thin-film solar cell, an organic electroluminescent device, or the like.

[0056] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment used are all commercially available. If in the following examples, specific processing conditions and processing methods are not clearly described, then conditions and methods known in the art can be used to process.

[0057] Example 1

[0058] On a transparent substrate, a magnetron sputtering method is first used to introduce argon and oxygen into the chamber to sputter the target material and plate the first transparent dielectric layer; then a metal layer is plated; then, a plasma enhanced chemical vapor deposition method is used to introduce organic silicon (tetraethoxysilane), oxygen, and argon, with a power of 500W, a working pressure of 3Pa, and a flow ratio of organic silicon to oxygen of 1:20 to deposit a hybrid layer; then, a magnetron sputtering method is used to introduce argon and oxygen into the chamber to sputter the target material and plate the second transparent dielectric layer to obtain a transparent conductive film with a structure as shown in FIG. Figure 1 shown.

[0059] The transparent conductive film of Example 1 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of ITO with a thickness of 50 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 10 nm; the hybrid layer 14 has organic silicon oxide and inorganic silicon oxide, and the thickness of the hybrid layer 14 is 10 nm; the second transparent dielectric layer 15 is made of ITO with a thickness of 50 nm.

[0060] Example 2

[0061] The preparation steps are the same as those in Example 1. The structure of the prepared transparent conductive film is as follows: Figure 1 shown.

[0062] The transparent conductive film of Example 2 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of ITO with a thickness of 60 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 10 nm; the hybrid layer 14 has organic silicon oxide and inorganic silicon oxide, and the thickness of the hybrid layer 14 is 20 nm; the second transparent dielectric layer 15 is made of ITO with a thickness of 20 nm.

[0063] Example 3

[0064] On a transparent substrate, a magnetron sputtering method is first used to introduce argon and oxygen into the chamber to sputter the target material and plate the first transparent dielectric layer; then a metal layer is plated; then, a plasma chemical vapor deposition method is used to introduce organic silicon (hexamethyldisiloxane), oxygen, and argon to deposit a hybrid layer, with a power of 800W, a working pressure of 5Pa, and a flow ratio of organic silicon to oxygen of 1:30; then, a magnetron sputtering method is used to introduce argon and oxygen into the chamber to sputter the target material and plate the second transparent dielectric layer to obtain a transparent conductive film, the structure of which is shown in FIG. Figure 1 shown.

[0065] The transparent conductive film of Example 3 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of AZO (aluminum-doped zinc oxide) with a thickness of 50 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 10 nm; the hybrid layer 14 has organic silicon oxide and inorganic silicon oxide, and the thickness of the hybrid layer 14 is 15 nm; the second transparent dielectric layer 15 is made of AZO with a thickness of 50 nm.

[0066] Example 4

[0067] The preparation steps are the same as those in Example 3. The structure of the prepared transparent conductive film is as follows: Figure 1 shown.

[0068] The transparent conductive film of Example 4 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of AZO (aluminum-doped zinc oxide) with a thickness of 50 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 10 nm; the hybrid layer 14 has organic silicon oxide and inorganic silicon oxide, and the thickness of the hybrid layer 14 is 20 nm; the second transparent dielectric layer 15 is made of ITO with a thickness of 30 nm.

[0069] Example 5

[0070] The preparation steps are the same as those in Example 1. The structure of the prepared transparent conductive film is as follows: Figure 1 shown.

[0071] The transparent conductive film of Example 5 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of ITO with a thickness of 50 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 12 nm; the hybrid layer 14 has organic silicon oxide and inorganic silicon oxide, and the thickness of the hybrid layer 14 is 20 nm; the second transparent dielectric layer 15 is made of ITO with a thickness of 50 nm.

[0072] Example 6

[0073] The preparation steps are the same as those in Example 1. The structure of the prepared transparent conductive film is as follows: Figure 1 shown.

[0074] The transparent conductive film of Example 6 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of ITO with a thickness of 50 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 11 nm; the hybrid layer 14 has organic silicon oxide and inorganic silicon oxide, and the thickness of the hybrid layer 14 is 22 nm; the second transparent dielectric layer 15 is made of ITO with a thickness of 50 nm.

[0075] Comparative Example 1

[0076] On a transparent substrate, a magnetron sputtering method is first used to introduce argon and oxygen into the chamber to sputter the target material, and a first transparent dielectric layer is plated; then a metal layer is plated; and then a magnetron sputtering method is used to introduce argon and oxygen into the chamber to sputter the target material, and a second transparent dielectric layer is plated to obtain a transparent conductive film, the structure of which is as follows: Figure 2 shown.

[0077] The transparent conductive film of Comparative Example 1 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of ITO with a thickness of 50 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 10 nm; the second transparent dielectric layer 15 is made of ITO with a thickness of 50 nm.

[0078] The difference between Comparative Example 1 and Example 1 is that no hybrid layer is formed in Comparative Example 1.

[0079] Comparative Example 2

[0080] On a transparent substrate, a magnetron sputtering method is first used to introduce argon and oxygen into the chamber to sputter the target material, and a first transparent dielectric layer is plated; then a metal layer is plated; and then a magnetron sputtering method is used to introduce argon and oxygen into the chamber to sputter the target material, and a second transparent dielectric layer is plated to obtain a transparent conductive film, the structure of which is as follows: Figure 2 shown.

[0081] The transparent conductive film of Comparative Example 2 is configured as follows from bottom to top: the transparent substrate 11 is made of PET with a thickness of 125 μm; the first transparent dielectric layer 12 is made of AZO (aluminum-doped zinc oxide) with a thickness of 50 nm; the metal layer 13 is made of silver-titanium alloy, the mass content of titanium in the metal layer 13 is 10%, and the thickness of the metal layer 13 is 10 nm; the second transparent dielectric layer 15 is made of AZO with a thickness of 50 nm.

[0082] The difference between Comparative Example 2 and Example 3 is that no hybrid layer is formed in Comparative Example 2.

[0083] The transparent conductive film samples prepared in Examples 1-6 and Comparative Examples 1-2 were subjected to relevant tests, including water vapor transmission rate, sheet resistance, moisture and heat resistance, etc. The specific test methods are as follows:

[0084] (1) Water vapor transmission rate:

[0085] The test was conducted using the Aquatran Model 1 moisture permeability tester from the American MOCON Company.

[0086] (2) Sheet resistance:

[0087] The test was conducted using an ST-21 sheet resistance tester at a temperature of 23±5°C and a relative humidity of (50%±10%) RH.

[0088] (3) Moisture and heat resistance:

[0089] The transparent conductive film samples were placed in an environment of 23±5℃ and relative humidity (50%±10%) RH for at least 2 hours. The square resistance was tested before and after aging for 1000 hours, and the square resistance change rate was calculated. The aging conditions are: 60℃ temperature, 90% relative humidity, square resistance change rate = (R 1 -R 0 ) / R 0 × 100%, where R 0 is the initially measured sheet resistance, R 1 It is the sheet resistance value measured after aging for 240 hours.

[0090] At the same time, after aging for 1000 hours, the appearance of the conductive film was observed with the naked eye (○ represents good, △ represents good, and × represents poor).

[0091] The test results are shown in Table 1:

[0092] Table 1 Test data table of Examples 1-6 and Comparative Examples 1-2

[0093]

[0094] Compared with Comparative Examples 1 and 2, in Examples 1-6, plasma enhanced chemical vapor deposition is used to form a hybrid layer between the metal layer and the second transparent dielectric layer, which can greatly improve the water vapor barrier performance, moisture and heat resistance and stability of the transparent conductive film.

[0095] In the description of the present invention, the orientation or position relationship indicated by the terms "upper" and "lower" etc. is based on the orientation or position relationship shown in the drawings and is only for the convenience of describing the present invention rather than requiring the present invention to be constructed and operated in a specific orientation. Therefore, it should not be understood as a limitation on the present invention.

[0096] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0097] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A transparent conductive film, characterized in that: The invention comprises a transparent substrate, a first transparent dielectric layer, a metal layer, a hybrid layer and a second transparent dielectric layer which are stacked in sequence. The material of the hybrid layer comprises organic silicon oxide and inorganic silicon oxide, and the material of the second transparent dielectric layer is inorganic.

2. The transparent conductive film according to claim 1, characterized in that: The thickness of the hybrid layer is 10nm-30nm.

3. The transparent conductive film according to claim 1, characterized in that: The material of the metal layer is an alloy of silver and at least one element selected from copper, palladium, niobium, tin, indium, antimony, aluminum, titanium, nickel and chromium; And / or, the thickness of the metal layer is 3nm-20nm.

4. The transparent conductive film according to claim 1, characterized in that: The material of the first transparent dielectric layer and the material of the second transparent dielectric layer independently include one or more of metal oxide, metal oxide dopant, metal sulfide, metal fluoride, silicon oxide and silicon nitride; And / or, the thickness of the first transparent dielectric layer and the thickness of the second transparent dielectric layer are each independently 5 nm-100 nm.

5. The transparent conductive film according to any one of claims 1 to 4, characterized in that: The transparent conductive film satisfies at least one of the following conditions: The material of the first transparent dielectric layer and the material of the second transparent dielectric layer independently include one or more of indium tin oxide, niobium pentoxide, titanium dioxide, bismuth oxide, tungsten trioxide, nickel oxide, zinc oxide, gallium zinc oxide, indium zinc oxide, silicon dioxide, hafnium dioxide, zirconium oxide, aluminum-doped zinc oxide, aluminum oxide, indium oxide, tin dioxide, zinc sulfide, silicon nitride and magnesium fluoride; The material of the transparent substrate includes one or more of polyethylene terephthalate, polyimide, polyethylene naphthalate, polycarbonate, polystyrene and triacetyl cellulose; The thickness of the transparent substrate is 1 μm-500 μm; After aging for 1000 hours in an environment of 60° C. and 90% RH, the resistance of the transparent conductive film increases by no more than 30%.

6. A method for preparing the transparent conductive film according to any one of claims 1 to 5, characterized in that: include: providing a transparent substrate; forming a first transparent dielectric layer, a metal layer, a hybrid layer and a second transparent dielectric layer in sequence on one side of the transparent substrate; The hybrid layer is formed by the following steps: placing a transparent substrate formed with the first transparent dielectric layer and the metal layer in a plasma enhanced chemical vapor deposition device, introducing organic silicon, oxygen-containing gas and inert gas, and performing plasma enhanced chemical vapor deposition to form a hybrid layer on the surface of the metal layer away from the transparent substrate.

7. The method according to claim 6, characterized in that The organosilicon includes one or more of tetramethyldisiloxane, hexamethyldisiloxane, vinyltrimethylsilane, hexamethyldisilane, methylsilane, dimethylsilane, trimethylsilane, diethylsilane, propylsilane, phenylsilane, vinyltriethoxysilane, vinyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane and octamethylcyclotetrasiloxane; and / or, the oxygen-containing gas comprises one or more of oxygen, carbon monoxide and ozone; And / or, the inert gas includes argon.

8. The method according to claim 7, characterized in that: The organosilicon includes at least one of tetraethoxysilane and hexamethyldisiloxane; And / or, the oxygen-containing gas comprises oxygen.

9. The method according to any one of claims 6 to 8, characterized in that: The first transparent dielectric layer and the second transparent dielectric layer are both formed by magnetron sputtering.

10. A photoelectric device, characterized in that: The invention comprises a transparent electrode, wherein the transparent electrode comprises the transparent conductive film according to any one of claims 1 to 5.