Deep sea cable convenient to observe and preparation process method thereof
By using a design that combines fluorescent substances and thermoplastic elastomers in deep-sea cables, the problem of reduced fluorescence in the marine environment is solved, achieving significant fluorescence effects and long life in seawater, and is suitable for the identification and monitoring of submarine equipment. .
Patent Information
- Application Number
- CN202410842649.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
AI Technical Summary
Factors such as salt, chloride ions, pH value, temperature and light in the marine environment have adverse effects on the fluorescence effect of fluorescent cables, resulting in a reduction in fluorescence and affecting the cable's observability and service life.
A yellow thermoplastic elastomer containing fluorescent substances is used as a protective sheath, combined with a TPE or Teflon insulation layer and a fluorescent agent, and through specific process conditions and material combinations, a deep-sea cable that can glow eye-catchingly under ultraviolet light is prepared. .
The deep-sea cable maintains good fluorescence effects in fresh water or sea water, has excellent visual effects and long service life. It can be deployed in deep sea water for a long time and still maintain significant fluorescence effects.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of marine technology, and in particular relates to a deep-sea cable that is easy to observe and a preparation method thereof. Background Art
[0002] In the field of marine technology, when testing marine environmental parameters, such as temperature, salinity or flow rate, or exploring marine resources using seabed drills and samplers, it is necessary to connect the seabed equipment to the cable. Fluorescent cables can emit fluorescence in deep sea environments, making them easier to identify and locate in underwater environments. This is very helpful for cable maintenance, repair and management, especially in dark seabed environments. In addition, cables can be used to build seabed earthquake monitoring networks and marine disaster observation and warning systems in the field of marine disaster warning and emergency rescue, which requires cables to emit obvious light signals.
[0003] However, factors such as salt, chloride ions, pH value, temperature, light and microorganisms in seawater will have an adverse effect on the fluorescent effect of the cable. After using the fluorescent cable for a period of time, the fluorescence will decrease. Summary of the invention
[0004] The object of the present invention is to provide a deep-sea cable that is easy to observe and a manufacturing method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A deep-sea cable which is easy to observe comprises a plurality of conductors, all of which are wrapped with insulating layers to form a conductor bundle, and the conductor bundle is surrounded by a protective sheath which is a yellow thermoplastic elastomer containing fluorescent material.
[0007] Preferably, the fluorescent substance includes one or more of fluorescent masterbatch and color masterbatch; the material of the insulating layer is TPE or Teflon.
[0008] Preferably, the thermoplastic elastomer is TPE, and the specific gravity of TPE is 0.9-1.0 g / cm3.
[0009] Preferably, both the TPE and Teflon are limited foaming materials.
[0010] Preferably, the raw material of the protective cover includes a stabilizer, and the stabilizer includes modified citrate.
[0011] Preferably, the preparation steps of the modified citrate include:
[0012] A1: Add appropriate amount of citric acid, n-butanol and aminosulfonic acid into the reactor, set process condition 1, and finally filter to obtain the intermediate product;
[0013] A2: Add appropriate amount of intermediate product 1, acetic anhydride, vanadium pentoxide and methanesulfonic acid into a reactor, set process condition 2, and finally filter to obtain modified citrate.
[0014] Preferably, process condition 1 is a temperature of 60-130°C and a time of 1-6h; process condition 2 is a temperature of 50-100°C and a time of 30min-5h.
[0015] A method for preparing a deep-sea cable that is easy to observe includes the following steps:
[0016] B1: Add appropriate amount of insulation layer material and foaming agent into a mixer, set process condition b1, prepare blend G01, inject blend G01 into an injection mold, pull the conductor core evenly through the injection mold, and then cool, shape and coil to prepare a semi-finished cable;
[0017] B2: passing the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; taking an appropriate amount of insulating layer material, masterbatch, and foaming agent into a mixer, setting process conditions b2, preparing a blend G02, injecting the blend G02 into a hollow tube, passing the prepared optical fiber assembly through the hollow tube and evenly pulling it out, then cooling and shaping and winding it to prepare a semi-finished optical cable;
[0018] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0019] B4: passing the composite cable core semi-finished product prepared in B3 through a hot air tube and setting process conditions b3 to obtain a composite cable core;
[0020] B5: Add TPE, fluorescent agent, yellow masterbatch and foaming agent into the mixer, set process condition b4, and prepare blend G3. Set process condition b5, pass the composite cable core through the hot air tube, and then inject blend G3 into the hot air tube through the injection mold, set process condition b6, blend G3 wraps the composite cable core, and pulls it out under constant tension and cools it to prepare a cable.
[0021] A method for preparing a deep-sea cable that is easy to observe includes the following steps:
[0022] C1: Add appropriate amount of citric acid, n-butanol and aminosulfonic acid into the reactor, set process conditions c1, and finally filter and dry to obtain intermediate product 1;
[0023] C2: Add appropriate amount of intermediate product 1, acetic anhydride, vanadium pentoxide and methanesulfonic acid into the reactor, set process condition c2, and finally filter to obtain modified citrate;
[0024] C3: Add appropriate amounts of insulating layer material, foaming agent, modified citrate, and dibutyltin dilaurate into a mixer, set process conditions c3, prepare blend G1, inject blend G1 into an injection mold, pull the conductor core evenly through the injection mold, and then cool, shape, and coil to prepare a semi-finished cable;
[0025] C4: passing the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; taking an appropriate amount of insulating layer material, masterbatch, and foaming agent into a mixer, setting process conditions c4, preparing a blend G2, injecting the blend G2 into a hollow tube, passing the prepared optical fiber assembly through the hollow tube and evenly pulling it out, then cooling and shaping and winding it to prepare a semi-finished optical cable;
[0026] C5: Twisting the semi-finished cable and the semi-finished optical cable prepared in B1 and B2 in order, and winding them into a coil to obtain a composite cable core semi-finished product;
[0027] C6: passing the composite cable core semi-finished product prepared in C5 through a hot air tube and setting process conditions c5 to obtain a composite cable core;
[0028] C7: Put TPE, fluorescent agent, yellow masterbatch and foaming agent into the mixer, set process condition c6, and prepare blend G3. Set process condition c7, pass the composite cable core through the hot air tube, and then inject blend G3 into the hot air tube through the injection mold, set process condition c8, blend G3 wraps the composite cable core, and pulls it out and cools it under constant tension to prepare a cable.
[0029] Preferably,
[0030] The insulation layer material is TPE or Teflon;
[0031] The fluorescent agent is one or more of phenyldiazines, thiophenes, carbazoles, fluorenes, benzodiazines, etc.;
[0032] The raw material of the protective cover is TPE, and the specific gravity of TPE is 0.9-1.0g / cm3;
[0033] Process conditions b1, b2 and b4 are all heating temperature 200-280°C and pressure 1-2 MPa;
[0034] Process conditions b3 and b5 are both at a temperature of 210-240°C;
[0035] The mixer is one or more of an extruder or an internal mixer;
[0036] The cooling method is water cooling.
[0037] Preferably,
[0038] The process condition c1 is a temperature of 60-130°C and a time of 1-6h;
[0039] The process condition c2 is a temperature of 50-100°C and a time of 30 min-5 h;
[0040] The insulating layer material is TPE or Teflon;
[0041] The fluorescent agent is one or more of phenyldiazines, thiophenes, carbazoles, fluorenes, and benzodiazines;
[0042] The process conditions c3, c4 and c6 are all heating temperature 200-280°C and pressure 1-2 MPa;
[0043] The process conditions c5 and c7 are temperatures of 210-240°C, and the injection mold temperature of c8 is 200-280°C;
[0044] The mixer is one or more of an extruder or an internal mixer;
[0045] The cooling method is water cooling.
[0046] Compared with the prior art, the beneficial effects of the present invention are: the cable prepared by the present invention glows strikingly under ultraviolet light in fresh water or sea water, has a very excellent visual effect, maintains an excellent fluorescent effect, and can still maintain a good fluorescent effect and a long service life when deployed in deep sea water for a long time. DETAILED DESCRIPTION
[0047] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0048] Embodiment 1:
[0049] B1: 100 parts of TPE and 3 parts of azodicarbonamide were put into a mixer, the temperature was set to 200°C, and the pressure was 1 MPa to prepare a blend G01, and the blend G01 was injected into an injection mold. The conductor core was evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0050] B2: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; take an appropriate amount of 100 parts of TPE and 3 parts of ammonium bicarbonate and put them into a mixer, set the temperature to 200°C, pressurize to 1 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0051] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0052] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 210°C to obtain a composite cable core;
[0053] B5: 100 parts of TPE, 0.01 parts of fluorescent agent DMS, 1 part of yellow masterbatch, and 3 parts of azodicarbonamide were added to a mixer, heated to 200°C, and pressurized to 1 MPa to prepare blend G3. The composite cable core was preheated to 210°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 200°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0054] Embodiment 2:
[0055] B1: 100 parts of Teflon, an insulating layer material, and 5 parts of sodium bicarbonate are put into a mixer, the temperature is set to 280°C, and the pressure is 2 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0056] B2: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon and 5 parts of ammonium bicarbonate into a mixer, set the temperature to 280°C, pressurize to 2 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0057] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0058] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 240°C to obtain a composite cable core;
[0059] B5: 100 parts of TPE, 1 part of 2.5-bis(5-tert-butyl-2-benzoxazolyl)thiophene, 5 parts of yellow masterbatch, and 5 parts of ammonium bicarbonate were added to a mixer, heated to 280°C, and pressurized to 2 MPa to prepare blend G3. The composite cable core was preheated to 240°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 280°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0060] Embodiment 3:
[0061] B1: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0062] B2: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; take an appropriate amount of 100 parts of TPE, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate and put them into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0063] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0064] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0065] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0066] Embodiment 4:
[0067] C1: Take 5 parts of citric acid, 20 parts of n-butanol and 0.5 parts of aminosulfonic acid and put them into a reactor at 60°C for 1 hour, and finally filter and dry to obtain intermediate product 1;
[0068] C2: Add 10 parts of the intermediate product 1, 20 parts of acetic anhydride, 0.5 parts of vanadium pentoxide and 0.5 parts of methanesulfonic acid into a reaction kettle at a temperature of 50-100°C for 30 minutes, and finally filter to obtain the modified citrate;
[0069] C3: 100 parts of TPE, 4 parts of azodicarbonamide, 2 parts of modified citrate, and 1 part of dibutyltin dilaurate are put into a mixer, heated to 250° C., pressurized to 1.5 MPa, to prepare a blend G1, and the blend G1 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0070] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0071] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0072] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0073] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0074] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0075] Embodiment 5:
[0076] C1: Take appropriate amounts of 10 parts of citric acid, 60 parts of n-butanol and 2 parts of aminosulfonic acid and put them into a reactor at 130°C for 6 hours, and finally filter and dry to obtain intermediate product 1;
[0077] C2: Add 20 parts of the intermediate product 1, 60 parts of acetic anhydride, 2 parts of vanadium pentoxide and 1 part of methanesulfonic acid into a reaction kettle at 100°C for 5 hours, and finally filter to obtain the modified citrate;
[0078] C3: 100 parts of TPE, 4 parts of azodicarbonamide, 5 parts of modified citrate, and 2 parts of dibutyltin dilaurate are put into a mixer, heated to 250° C., pressurized to 1.5 MPa, to prepare a blend G1, and the blend G1 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0079] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0080] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0081] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0082] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0083] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0084] Embodiment 6:
[0085] C1: 8 parts of citric acid, 50 parts of n-butanol and 1.6 parts of aminosulfonic acid were added to a reactor at 100°C for 4 hours, and then filtered and dried to obtain intermediate product 1;
[0086] C2: Add 14 parts of the intermediate product, 140 parts of acetic anhydride, 1.3 parts of vanadium pentoxide and 0.8 parts of methanesulfonic acid into a reactor at 80°C for 2 hours, and finally filter to obtain the modified citrate;
[0087] C3: 100 parts of TPE, 4 parts of azodicarbonamide, 3 parts of modified citrate, and 1.6 parts of dibutyltin dilaurate are put into a mixer, heated to 250° C., pressurized to 1.5 MPa, to prepare a blend G1, and the blend G1 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0088] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0089] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0090] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0091] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0092] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0093] Embodiment 7:
[0094] A deep-sea cable that is easy to observe, including several conductors, all of which are wrapped with an insulating layer to form a conductor bundle, and the conductor bundle is surrounded by a protective sleeve, which is a yellow thermoplastic elastomer containing fluorescent material. The fluorescent material includes one or more of fluorescent masterbatch and color masterbatch; the material of the insulating layer is TPE or Teflon; the thermoplastic elastomer is TPE, and the specific gravity of TPE is 0.9-1.0g / cm 3 . Both TPE and Teflon are limited foaming materials.
[0095] Comparative Example 1:
[0096] C1: 8 parts of citric acid, 50 parts of n-butanol and 1.6 parts of aminosulfonic acid were added to a reactor at 100°C for 4 hours, and then filtered and dried to obtain intermediate product 1;
[0097] C2: Add 14 parts of the intermediate product, 140 parts of acetic anhydride and 1.3 parts of vanadium pentoxide into a reactor at 80°C for 2 hours, and finally filter to obtain the modified citrate;
[0098] C3: 100 parts of TPE, 4 parts of azodicarbonamide, 3 parts of modified citrate, and 1.6 parts of dibutyltin dilaurate are put into a mixer, heated to 250° C., pressurized to 1.5 MPa, to prepare a blend G1, and the blend G1 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0099] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0100] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0101] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0102] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0103] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0104] Comparative Example 2:
[0105] C1: 8 parts of citric acid, 50 parts of n-butanol and 1.6 parts of aminosulfonic acid were added to a reactor at 100°C for 4 hours, and then filtered and dried to obtain intermediate product 1;
[0106] C2: Add 14 parts of the intermediate product, 140 parts of acetic anhydride and 0.8 parts of methanesulfonic acid into a reaction kettle at 80°C for 2 hours, and finally filter to obtain the modified citrate;
[0107] C3: 100 parts of TPE, 4 parts of azodicarbonamide, 3 parts of modified citrate, and 1.6 parts of dibutyltin dilaurate are put into a mixer, heated to 250° C., pressurized to 1.5 MPa, to prepare a blend G1, and the blend G1 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0108] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0109] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0110] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0111] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0112] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0113] Comparative Example 3:
[0114] C1: 8 parts of citric acid, 50 parts of n-butanol and 1.6 parts of aminosulfonic acid were added to a reactor at 100°C for 4 hours, and then filtered and dried to obtain intermediate product 1;
[0115] C2: Add 14 parts of the intermediate product, 140 parts of acetic anhydride, 1.3 parts of vanadium pentoxide and 0.8 parts of methanesulfonic acid into a reactor at 80°C for 2 hours, and finally filter to obtain the modified citrate;
[0116] C3: 100 parts of TPE, 4 parts of azodicarbonamide, and 3 parts of modified citrate are put into a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare a blend G1, which is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0117] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0118] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0119] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0120] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0121] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0122] Comparative Example 4:
[0123] B1: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0124] B2: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; take an appropriate amount of 100 parts of TPE, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate and put them into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0125] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0126] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0127] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0128] Comparative Example 5:
[0129] C1: 8 parts of citric acid, 50 parts of n-butanol and 1.6 parts of aminosulfonic acid were added to a reactor at 100°C for 4 hours, and then filtered and dried to obtain intermediate product 1;
[0130] C2: Add 14 parts of the intermediate product, 140 parts of acetic anhydride, 1.3 parts of vanadium pentoxide and 0.8 parts of methanesulfonic acid into a reactor at 80°C for 2 hours, and finally filter to obtain the modified citrate;
[0131] C3: 100 parts of TPE, 4 parts of azodicarbonamide, 3 parts of modified citrate, and 1.6 parts of dibutyltin dilaurate are put into a mixer, heated to 250° C., pressurized to 1.5 MPa, to prepare a blend G1, and the blend G1 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0132] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0133] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0134] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0135] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0136] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was pulled out and cooled under constant tension to prepare a cable.
[0137] Comparative Example 6:
[0138] C1: 8 parts of citric acid, 50 parts of n-butanol and 1.6 parts of aminosulfonic acid were added to a reactor at 100°C for 4 hours, and then filtered and dried to obtain intermediate product 1;
[0139] C2: Add 14 parts of the intermediate product, 140 parts of acetic anhydride, 1.3 parts of vanadium pentoxide and 0.8 parts of methanesulfonic acid into a reactor at 80°C for 2 hours, and finally filter to obtain the modified citrate;
[0140] C3: 100 parts of TPE, 4 parts of azodicarbonamide, 3 parts of modified citrate, and 1.6 parts of tribasic lead sulfate are put into a mixer, heated to 250° C., pressurized to 1.5 MPa, to prepare a blend G1, and the blend G1 is injected into an injection mold, and the conductor core is evenly pulled out through the injection mold, and then cooled, shaped, and wound to prepare a semi-finished cable;
[0141] C4: 100 parts of insulating layer material TPE and 4 parts of azodicarbonamide are put into a mixer, the temperature is set to 250°C, and the pressure is 1.5 MPa to prepare a blend G01, and the blend G01 is injected into an injection mold. The conductor core is evenly pulled out through the injection mold, and then cooled, shaped and wound to prepare a semi-finished cable;
[0142] C5: Pass the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; put an appropriate amount of 100 parts of Teflon, 4 parts of azodicarbonamide, and 2 parts of ammonium bicarbonate into a mixer, set the temperature to 260°C, pressurize to 1.5 MPa, prepare a blend G02, inject the blend G02 into the hollow tube, pass the prepared optical fiber assembly through the injection-molded hollow tube and evenly pull it out, then cool it to shape and coil it to prepare a semi-finished optical cable;
[0143] B3: The semi-finished cable and the semi-finished optical cable prepared in B1 and B2 are twisted in order and wound into a coil to obtain a composite cable core semi-finished product.
[0144] B4: The composite cable core semi-finished product prepared in B3 is passed through a hot air tube at a set temperature of 220°C to obtain a composite cable core;
[0145] B5: 100 parts of TPE, 0.5 parts of 4-(9-carbazolyl)phenylacetic acid, 3 parts of yellow masterbatch, and 4 parts of ammonium bicarbonate were added to a mixer, heated to 250°C, and pressurized to 1.5 MPa to prepare blend G3. The composite cable core was preheated to 230°C and passed through a hot air tube, and then blend G3 was injected into the hot air tube through an injection mold. The temperature of the injection mold was 250°C. Blend G3 wrapped the composite cable core and was placed under constant tension.
[0146] The cables are prepared by cooling down the pull-down.
[0147] The cables prepared in Examples 1-6 and Comparative Examples 1-6 were placed in 20-meter seawater and fresh water for 2 years, and placed in 100-meter seawater for 2 years. The cables were irradiated with ultraviolet light every six months, and the fluorescence phenomenon was observed. The test results are as follows:
[0148] Table 1 Brightness test results (20 meters under sea water)
[0149]
[0150] From the results in Table 1, it can be seen that after being placed in 20 meters of seawater for 1.5 years, the brightness of the ropes of Examples 1-6 and Comparative Examples 1-3 was very bright; however, after 2 years, each of Examples 1-3, Comparative Examples 6 and Comparative Examples 1-3 became darker than at the beginning, but Examples 4-6 were still very bright. In addition, the brightness of Comparative Example 4 at 0.5 years, 1 year, 1.5 years, and 2 years was darker than that of Example 3 at the corresponding time, and the brightness of Comparative Example 5 at 0.5 years, 1 year, 1.5 years, and 2 years was darker than that of Example 5 at the corresponding time. The effect of Comparative Example 6 was worse than that of Examples 4-6. The Comparative Example was darker at the second year than at the beginning,
[0151] Table 2 Brightness test results (20 meters under fresh water)
[0152]
[0153] From the results in Table 2, it can be seen that after being placed in 20 meters of seawater for 2 years, the brightness of the ropes of Examples 1-6, Comparative Examples 1-3 and Comparative Example 6 is very bright. By comparing the results of Examples 1-6 and Comparative Examples 1-3 in Table 1, it can be seen that seawater has a weakening effect on the intensity of the fluorescent agent, which also shows that Examples 4-6 are more resistant to the weakening effect of seawater on the intensity of the fluorescent agent than Examples 1-3. The brightness of Comparative Example 4 at 0.5 years, 1 year, 1.5 years, and 2 years is darker than that of Example 3 at the corresponding time. Comparative Example 6 has the same effect as Examples 4-6.
[0154] Table 3 Brightness test results (100 meters under sea water)
[0155]
[0156] The results of Examples 1-3 show that when Examples 1-3 are 100 meters underwater, in the first year, the brightness is slightly darker than the initial time, and in the 1.5 and 2 years, the brightness gradually becomes darker; however, in Examples 4-6, the brightness is basically unchanged in the 0.5-1.5 years, and only in the 2nd year, the brightness becomes darker than the initial time, while in Comparative Examples 1-3, there is no brightness change in the first year, but in the 1.5 year, the brightness gradually decreases every six months, and Comparative Examples 4 and Comparative Examples 5 also have a brightness difference similar to that at 20 meters underwater. Comparative Example 6 is slightly worse than Examples 4-6, and starts to become darker from 1.5 years.
[0157] Although embodiments of the present invention have been shown and described (see the above detailed description for details), it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A deep-sea cable that is easy to observe, comprising a plurality of conductors, characterized in that: The conductors are all wrapped with an insulating layer to form a conductor bundle, and the conductor bundle is surrounded by a protective sleeve, and the protective sleeve is a yellow thermoplastic elastomer containing fluorescent material.
2. The deep-sea cable that is easy to observe according to claim 1, characterized in that: The fluorescent substance includes one or more of fluorescent masterbatch and color masterbatch; the material of the insulating layer is TPE or Teflon; the thermoplastic elastomer is TPE, and the specific gravity of TPE is 0.9-1.0g / cm 3 .
3. The deep-sea cable that is easy to observe according to claim 2, characterized in that: Both TPE and Teflon are limited foaming materials.
4. The deep-sea cable that is easy to observe according to claim 1, characterized in that: The raw material of the protective cover includes a stabilizer, and the stabilizer includes modified citrate.
5. The deep-sea cable that is easy to observe according to claim 4, characterized in that: The preparation steps of the modified citrate include: A1: Add appropriate amount of citric acid, n-butanol and aminosulfonic acid into the reactor, set process condition 1, and finally filter to obtain the intermediate product; A2: Add appropriate amount of intermediate product 1, acetic anhydride, vanadium pentoxide and methanesulfonic acid into a reactor, set process condition 2, and finally filter to obtain modified citrate.
6. The deep-sea cable that is easy to observe according to claim 5, characterized in that: The process condition 1 is a temperature of 60-130°C and a time of 1-6h; the process condition 2 is a temperature of 50-100°C and a time of 30min-5h.
7. A method for preparing a deep-sea cable that is easy to observe, characterized in that: The process steps include: B1: Add appropriate amount of insulation layer material and foaming agent into a mixer, set process condition b1, prepare blend G01, inject blend G01 into an injection mold, pull the conductor core evenly through the injection mold, and then cool, shape and coil to prepare a semi-finished cable; B2: passing the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; taking an appropriate amount of insulating layer material, masterbatch, and foaming agent into a mixer, setting process conditions b2, preparing a blend G02, injecting the blend G02 into a hollow tube, passing the prepared optical fiber assembly through the hollow tube and evenly pulling it out, then cooling and shaping and winding it to prepare a semi-finished optical cable; B3: The semi-finished cables and optical cables prepared in B1 and B2 are sequentially twisted and coiled to obtain a composite cable core semi-finished product. B4: passing the composite cable core semi-finished product prepared in B3 through a hot air tube and setting process conditions b3 to obtain a composite cable core; B5: Add TPE, fluorescent agent, yellow masterbatch and foaming agent into the mixer, set process condition b4, and prepare blend G03. Set process condition b5, pass the composite cable core through the hot air tube, and then inject blend G03 into the hot air tube through the injection mold, set process condition b6, blend G03 wraps the composite cable core, and pulls it out under constant tension and cools it to prepare a cable.
8. A method for preparing a deep-sea cable that is easy to observe, characterized in that: The process steps include: C1: Add appropriate amount of citric acid, n-butanol and aminosulfonic acid into the reactor, set process conditions c1, and finally filter and dry to obtain intermediate product 1; C2: Add appropriate amount of intermediate product 1, acetic anhydride, vanadium pentoxide and methanesulfonic acid into the reactor, set process condition c2, and finally filter to obtain modified citrate; C3: Add appropriate amounts of insulating layer material, foaming agent, modified citrate, and dibutyltin dilaurate into a mixer, set process conditions c3, prepare blend G1, inject blend G1 into an injection mold, pull the conductor core evenly through the injection mold, and then cool, shape, and coil to prepare a semi-finished cable; C4: passing the optical fiber and the inner tensile fiber through the inner layer to form an optical fiber assembly; taking an appropriate amount of insulating layer material, masterbatch, and foaming agent into a mixer, setting process conditions c4, preparing a blend G2, injecting the blend G2 into a hollow tube, passing the prepared optical fiber assembly through the hollow tube and evenly pulling it out, then cooling and shaping and winding it to prepare a semi-finished optical cable; C5: Twisting the semi-finished cable and the semi-finished optical cable prepared in B1 and B2 in order, and winding them into a coil to obtain a composite cable core semi-finished product; C6: passing the composite cable core semi-finished product prepared in C5 through a hot air tube and setting process conditions c5 to obtain a composite cable core; C7: Put TPE, fluorescent agent, yellow masterbatch and foaming agent into the mixer, set process condition c6, and prepare blend G3. Set process condition c7, pass the composite cable core through the hot air tube, and then inject blend G3 into the hot air tube through the injection mold, set process condition c8, blend G3 wraps the composite cable core, and pulls it out and cools it under constant tension to prepare a cable.
9. The method for preparing a deep-sea cable that is easy to observe according to claim 7, characterized in that: The insulating layer material is TPE or Teflon; The fluorescent agent is one or more of phenyldiazines, thiophenes, carbazoles, fluorenes, benzodiazines, etc.; The raw material of the protective cover is TPE, and the specific gravity of the TPE is 0.9-1.0g / cm3; The process conditions b1, b2 and b4 are all heating temperature 200-280°C and pressure 1-2 MPa; The process conditions b3 and b5 are both at a temperature of 210-240°C, and the injection mold temperature of b6 is 200-280°C; The mixer is one or more of an extruder or an internal mixer; The cooling method is water cooling.
10. The method for preparing a deep-sea cable that is easy to observe according to claim 8, characterized in that: The process condition c1 is a temperature of 60-130°C and a time of 1-6h; The process condition c2 is a temperature of 50-100°C and a time of 30 min-5 h; The insulating layer material is TPE or Teflon; The fluorescent agent is one or more of phenyldiazines, thiophenes, carbazoles, fluorenes, and benzodiazines; The process conditions c3, c4 and c6 are all heating temperature 200-280°C and pressure 1-2 MPa; The process conditions c5 and c7 are temperatures of 210-240°C, and the injection mold temperature of c8 is 200-280°C; The mixer is one or more of an extruder or an internal mixer; The cooling method is water cooling.