Polymer solid electrolyte membrane and preparation method thereof, solid-state battery and electric device

By using a specific mass ratio of zinc salt, imide lithium salt and polymer matrix for hot pressing treatment in solid-state batteries, a polymer solid-state electrolyte membrane with a three-dimensional network block structure is formed, which solves the problem of ion conductivity and ion conductivity in solid-state batteries. The problem of insufficient mechanical strength has significantly improved the cycle performance and safety performance of the battery.

CN118738539AInactive Publication Date: 2024-10-01CHINA FAW CO LTD

Patent Information

Application Number
CN202410660513.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polymer solid electrolytes have low ionic conductivity and poor mechanical strength in solid-state batteries, which affect electrical performance and safety performance, limiting their commercial application.

Method used

A specific mass ratio of zinc salt, lithium imide salt and polymer matrix are used for hot-pressing treatment to form a polymer solid electrolyte membrane with a three-dimensional network block structure to improve its mechanical properties and ionic conductivity.

Benefits of technology

It effectively improves the cycle performance and safety performance of solid-state batteries, improves long- and short-term electrical performance, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738539A_ABST
    Figure CN118738539A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer solid electrolyte membrane and a preparation method thereof, a solid-state battery and an electric device, and belongs to the field of batteries. The preparation method comprises the following steps: mixing a zinc salt, an imide lithium salt, a polymer matrix and an organic solvent, drying, carrying out pre-pressing molding, and then carrying out hot pressing for 35-45 minutes at the pressure of 10-15 Mpa and the temperature of 100-120 DEG C; wherein the decomposition temperature of the imide lithium salt is higher than the hot pressing temperature, the polymer matrix contains polar functional groups, the melting temperature is lower than or equal to 100 DEG C, the glass transition temperature is lower than or equal to-15 DEG C, the imide lithium salt and the polymer matrix are jointly used as a main body, and the mass ratio of the zinc salt to the main body is (0.8-1.2): 100. The prepared polymer solid electrolyte membrane has a block structure in which flexible chain segments and rigid chain segments are alternated, and the polymer solid electrolyte membrane can effectively improve the cycle performance of a solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of solid-state batteries, and more specifically, to a polymer solid electrolyte membrane and a preparation method thereof, a solid-state battery and an electrical device. Background Art

[0002] Polymer electrolytes have the advantages of good safety, high interfacial compatibility, low cost, and easy processing, and are ideal materials for the next generation of solid-state batteries. Compared with traditional liquid electrolytes, solid electrolytes can effectively reduce the risk of leakage and electrolyte volatilization, while avoiding the problems of poor thermal stability of traditional diaphragms and poor electrolyte wettability.

[0003] The commonly used polymer frameworks of existing polymer solid electrolytes include: polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN) and multi-component copolymer materials. The currently used polymer electrolytes have the advantages of good flexibility, low interface impedance with electrode materials, good film-forming properties and low cost. However, their low ionic conductivity and poor mechanical strength seriously affect the electrical properties and safety performance of solid-state batteries, especially the cycle life, and also restrict their commercial and industrial applications. Summary of the invention

[0004] The present application provides a polymer solid electrolyte membrane and a preparation method thereof, a solid-state battery and an electrical device. The polymer solid electrolyte membrane has both good mechanical properties and ion conductivity properties. When the polymer solid electrolyte membrane is applied to a solid-state battery, it can effectively improve the cycle performance of the solid-state battery and enable the solid-state battery to have good long-term and short-term electrical properties and safety performance.

[0005] The embodiment of the present application is implemented as follows:

[0006] In a first aspect, the present application provides a method for preparing a polymer solid electrolyte membrane, which comprises the following steps:

[0007] The zinc salt, the lithium imide salt, the polymer matrix and the organic solvent for dissolving the polymer matrix are mixed and dried to obtain a precursor;

[0008] After the precursor is pre-pressed, the obtained green body is hot-pressed for 35 minutes to 45 minutes under the conditions of a hot-pressing pressure of 10 MPa to 15 MPa and a hot-pressing temperature of 100° C. to 120° C.;

[0009] The decomposition temperature of the imide lithium salt is greater than the hot pressing temperature, the melting temperature of the polymer matrix is ​​≤100°C and the glass transition temperature is ≤-15°C, the polymer matrix contains polar functional groups, the polar functional groups include -OH and / or -COC-, the imide lithium salt and the polymer matrix are used as the main body, and the mass ratio of the zinc salt to the main body is (0.8-1.2):100.

[0010] The preparation method provided in the present application is simple and controllable to operate, and utilizes the coordination of raw materials in a specific mass ratio and specific hot pressing conditions, so that the polymer solid electrolyte membrane has zinc ion agglomerate particles with a scale of nanometers and micrometers as cross-linking points, and the formed flexible segments and rigid segments alternate with each other to present a three-dimensional network block structure, so that the polymer solid electrolyte membrane can effectively improve the cycle performance of the solid-state battery when applied to the solid-state battery.

[0011] In some embodiments, the zinc salt comprises a zinc halide, and the zinc halide comprises at least one of zinc fluoride, zinc chloride, zinc bromide, and zinc iodide.

[0012] In some embodiments, the polymer matrix includes at least one of polyvinyl alcohol, polyethylene oxide, polypropylene oxide, and polybutylene oxide.

[0013] In some embodiments, the molecular weight of the polymer matrix is ​​10,000-18,000.

[0014] In some embodiments, the molecular weight of the polymer matrix is ​​12,000 to 15,000.

[0015] In some embodiments, the lithium imide salt includes lithium bis(trifluoromethanesulfonyl)imide.

[0016] In some embodiments, the mass ratio of the imide lithium salt to the polymer matrix is ​​(25-35):(65-75).

[0017] In some embodiments, the organic solvent includes at least one of anisole, ethylene dichloride, chloroform, and dimethylformamide.

[0018] In some embodiments, the pre-pressing includes: pressing at a pressure of 10 MPa to 15 MPa for 10 to 15 minutes.

[0019] In some embodiments, the step of mixing comprises:

[0020] Dissolving the polymer matrix in an organic solvent to obtain a polymer solution;

[0021] The zinc salt and the lithium imide salt are mixed with the polymer solution under stirring.

[0022] In some embodiments, the drying is performed under vacuum at a low temperature of 50°C to 80°C.

[0023] In a second aspect, the present application provides an example of a polymer solid electrolyte membrane, which is prepared by the preparation method provided in the first aspect of the present application.

[0024] The present application provides a polymer solid electrolyte membrane having a block structure in which flexible segments and rigid segments alternate with each other to present a three-dimensional network. When the polymer solid electrolyte membrane is applied to a solid-state battery, it can effectively improve the cycle performance of the solid-state battery and enable the solid-state battery to have good long-term and short-term electrical properties and safety performance.

[0025] In a third aspect, the present application provides a polymer solid electrolyte membrane, wherein the solid electrolyte membrane has a block structure in which rigid segments and flexible segments are alternately connected to form a three-dimensional network;

[0026] The rigid chain segments are crosslinked with nanometer-scale zinc ion aggregate particles as crosslinking points, and the zinc ion aggregate particles react with polar functional groups on the polymer matrix to form a tangled body with a certain rigidity by crosslinking multiple polymer molecular chains, and the polar functional groups include -OH and / or -COC-;

[0027] The flexible chain segments are free polymer molecular chains in a free state.

[0028] In a fourth aspect, the present application provides a solid-state battery, which includes the polymer solid electrolyte membrane provided in the second aspect or the third aspect of the present application.

[0029] In a fifth aspect, the present application example provides an electrical device comprising the solid-state battery provided in the fourth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 The preparation process and principle diagram of the polymer solid electrolyte membrane prepared by the preparation method provided in this application;

[0032] Figure 2 Schematic diagram of lithium ion transport in the polymer solid electrolyte prepared in this application. DETAILED DESCRIPTION

[0033] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0034] The following is a detailed description of the polymer solid electrolyte membrane and its preparation method, solid-state battery and electrical device according to the embodiments of the present application:

[0035] The present application provides a method for preparing a polymer solid electrolyte membrane, which comprises the following steps:

[0036] The zinc salt, the lithium imide salt, the polymer matrix and the organic solvent for dissolving the polymer matrix are mixed and dried to obtain a precursor;

[0037] After the precursor is pre-pressed, the obtained green body is hot-pressed for 35 minutes to 45 minutes under the conditions of a hot-pressing pressure of 10 MPa to 15 MPa and a hot-pressing temperature of 100° C. to 120° C.;

[0038] The decomposition temperature of the imide lithium salt is greater than the hot pressing temperature, the melting temperature of the polymer matrix is ​​≤100°C and the glass transition temperature is ≤-15°C, the polymer matrix contains polar functional groups, the polar functional groups include -OH and / or -COC-, the imide lithium salt and the polymer matrix are used as the main body, and the mass ratio of the zinc salt to the main body is (0.8-1.2):100.

[0039] Figure 1 The preparation process and principle diagram of the polymer solid electrolyte membrane prepared by the preparation method provided in this application; Figure 1 Part (a) shows that the precursor is cured by heat pressing to crosslink the polymer solid electrolyte; Figure 1 Part (b) is the design mechanism of the polymer solid electrolyte block structure.

[0040] Combination Figure 1 The above-mentioned preparation method provided in the present application is to heat-press the raw materials with specific mass ratios with specific parameters, so that the polymer is in a molten state in the early stage of hot pressing (initial stage of curing), and the Zn on the surface of the fully dispersed zinc salt is 2+The ether oxygen groups on the polymer chain segments react before the polymer matrix, so that the zinc salt slowly dissolves in the molten polymer and continues to react to form nanometer-scale particles. As the hot pressing time increases, the viscosity of the electrolyte continues to increase, and the continuously reacting zinc salt particles will agglomerate in the gaps of the molecular chains to form zinc ion agglomerate particles with a scale of nanometers. As the particle size of the zinc ion agglomerate particles increases, the number of coordination reaction binding sites provided around increases. Therefore, the zinc ion agglomerate particles are used as crosslinking points, and the zinc ion agglomerate particles and the polar functional groups on the polymer matrix react to form a tangled body with a certain rigidity formed by crosslinking multiple polymer molecular chains, as rigid segments; at the same time, the distance between the crosslinking points is extended, and a flexible segment is formed between the two crosslinking points, and the flexible segment is a free polymer molecular chain. That is, after the polymer solid electrolyte membrane is solidified due to hot pressing, the rigid segment is crystalline, giving the polymer solid electrolyte strong mechanical properties; the flexible segment is amorphous, giving the molecular chain good relaxation and mobility. The flexible segments and rigid segments alternate with each other to form a three-dimensional network block structure.

[0041] Figure 2 The schematic diagram of lithium ion transport in the polymer solid electrolyte membrane prepared in this application is shown in Figure 1. In the polymer solid electrolyte membrane, lithium ions are complexed with polar groups (-OH, COC, etc.) on the polymer molecular chains, decomplexed during the charge and discharge process of the battery cell, and then complexed with adjacent molecular chains as the polymer molecular chains move, repeating this process to achieve lithium ion migration.

[0042] Combination Figure 1 as well as Figure 2 The block polymer solid electrolyte prepared by the above preparation method can not only construct a stable lithium ion transmission network by utilizing the unique structure of alternating rigid and flexible segments, effectively inhibiting the battery capacity attenuation and the generation of lithium dendrites, but also Zn 2+ In addition to serving as a crosslinking point, it can also capture some TFSI - , so that more Li + It can migrate on the polymer chain to improve the conductivity, and has good mechanical properties and a certain degree of ductility, which can effectively prevent external factors or lithium dendrites from damaging the electrolyte structure.

[0043] Among them, choosing imide lithium salt as the electrolyte salt is beneficial to improving the cycle performance of the solid-state battery, and by controlling the decomposition temperature of the imide lithium salt to be greater than the hot pressing temperature, it is beneficial to inhibit the decomposition of the imide lithium salt during the process of hot pressing to form the polymer solid electrolyte membrane, which is beneficial to maintaining high ionic conductivity of the polymer solid electrolyte membrane.

[0044] By limiting the melting temperature of the polymer matrix to ≤100°C and the glass transition temperature to ≤-15°C, that is, the melting temperature of the polymer matrix is ​​lower than the hot pressing temperature, it is beneficial for the polymer matrix to remain in a molten state during the hot pressing process, for the zinc salt and lithium imide salt to be dispersed in the polymer matrix, for the polymer matrix to fully react with the zinc salt, and for improving the ionic conductivity of the polymer solid electrolyte membrane. The presence of polar functional groups is beneficial for zinc ions to react with polar functional groups on polymer segments first, thereby slowly dissolving in the molten polymer and continuing to react to form nanometer-sized particles.

[0045] If the mass ratio between zinc salt and the main body is too large or too small, it will affect the smooth construction of the block structure of the polymer solid electrolyte, resulting in low cycle performance of the solid-state battery. Therefore, controlling the mass ratio of zinc salt and the main body to (0.8~1.2):100 and performing hot pressing with specific parameters can effectively construct the above-mentioned flexible segments and rigid segments alternating with each other to present a three-dimensional network block structure.

[0046] Illustratively, the mass ratio of the zinc salt to the host is any value of 0.8:100, 0.9:100, 1.0:100, 1.1:100, 1.2:100, or between any two values.

[0047] Pre-pressing means pressing a precursor into a green body at room temperature, and the precursor is a mixture of zinc salt, lithium imide salt, and polymer matrix. The present application adopts a method of hot pressing a pre-formed green body. On the one hand, during the process of pre-pressing the green body, it is beneficial for the zinc salt and lithium imide salt to move along with the movement of the polymer matrix, which is beneficial for the zinc salt and lithium imide salt to be evenly dispersed, thereby improving the performance of the polymer solid electrolyte membrane. On the other hand, it is more conducive to shaping than directly hot pressing the precursor.

[0048] The hot pressing pressure, hot pressing temperature and hot pressing time all affect the effective construction of a three-dimensional network block structure in which flexible segments and rigid segments alternate with each other. Therefore, the hot pressing pressure is 10Mpa~15Mpa and the hot pressing temperature is 100℃~120℃ for 35min~45min. The selection of raw materials is conducive to the preparation of a polymer solid electrolyte membrane with a three-dimensional network block structure, thereby effectively improving the cycle performance and other electrochemical properties of the solid-state battery.

[0049] Exemplarily, the hot pressing pressure is any value among 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa, 15 MPa or between any two values.

[0050] Exemplarily, the hot pressing temperature is any one of 100° C., 105° C., 110° C., 115° C., 120° C., or between any two values.

[0051] Exemplarily, the hot pressing time is any value among 35min, 37min, 39min, 40min, 43min, 45min or between any two values. The hot pressing time can be adjusted within the above range according to the selection of the above specific hot pressing pressure and hot pressing temperature.

[0052] In summary, the preparation method provided in the present application is simple and controllable to operate, and utilizes the coordination of raw materials in a specific mass ratio and specific hot pressing conditions to make the polymer solid electrolyte membrane have a block structure in which flexible segments and rigid segments alternate with each other to present a three-dimensional network. When the polymer solid electrolyte membrane is used in a solid-state battery, it can effectively improve the cycle performance of the solid-state battery, and enable the solid-state battery to have good long-term and short-term electrical properties and safety performance.

[0053] Among them, zinc salt is used to provide zinc ions.

[0054] Zinc salts include, but are not limited to, zinc trifluoromethanesulfonate, zinc perchlorate, propineb, zinc dimethacrylate, zinc trifluoromethanesulfonylimide, zinc stearate, zinc sulfide or zinc halide and the like.

[0055] In some embodiments, the zinc salt comprises a zinc halide, and the zinc halide comprises at least one of zinc fluoride, zinc chloride, zinc bromide, and zinc iodide.

[0056] By selecting zinc halide as zinc salt, not only zinc ions can be provided, but free halogen ions can also participate in SEI film formation during the first charging process of the solid-state battery, which is beneficial to improving the density of the SEI film and the cycle performance of the solid-state battery.

[0057] In some embodiments, the polymer matrix includes at least one of polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide (PPO), and polybutylene oxide (PBO).

[0058] When the polymer solid electrolyte membrane prepared using the above-mentioned polymer matrices is used in solid-state batteries, it is beneficial to improve the cycle performance of the solid-state batteries.

[0059] Optionally, the polymer matrix includes at least one of polyethylene oxide (PEO), polypropylene oxide (PPO), and polybutylene oxide (PBO). The above selection is conducive to further improving the cycle performance of the solid-state battery.

[0060] In some embodiments, the molecular weight of the polymer matrix is ​​10,000-18,000.

[0061] Within the above range, when the prepared polymer solid electrolyte membrane is applied to a solid-state battery, the solid-state battery has better cycle performance.

[0062] Illustratively, the molecular weight of the polymer matrix is ​​any value of 10000, 11000, 12000, 13000, 14000, 15000, 16000, 17000, 18000 or between any two values.

[0063] In some embodiments, the molecular weight of the polymer matrix is ​​12,000 to 15,000.

[0064] Within the above range, when the prepared polymer solid electrolyte membrane is used in a solid-state battery, it is beneficial to further improve the cycle performance of the solid-state battery.

[0065] Illustratively, the molecular weight of the polymer matrix is ​​any one of 12000, 12500, 13000, 13500, 14000, 14500, 15000 or between any two values.

[0066] In some embodiments, the lithium imide salt includes but is not limited to at least one of lithium bis(fluorosulfonyl)imide salt and lithium bis(trifluoromethanesulfonyl)imide.

[0067] In some embodiments, the lithium imide salt is lithium bis(trifluoromethanesulfonyl)imide.

[0068] When the polymer solid electrolyte membrane prepared from the above-mentioned lithium bis(trifluoromethanesulfonyl)imide is used in a solid-state battery, it is beneficial to improve the cycle performance of the solid-state battery.

[0069] In some embodiments, in the main body, the mass ratio of the imide lithium salt to the polymer matrix is ​​(25-35):(65-75).

[0070] Under the above ratio, when the prepared polymer solid electrolyte membrane is applied to a solid-state battery, the solid-state battery has good cycle performance.

[0071] Exemplarily, the mass ratio of the imide lithium salt to the polymer matrix is ​​any one of 25:75, 28:72, 30:70, 33:67, 35:65, or between any two values.

[0072] Organic solvents are used to dissolve the polymer matrix.

[0073] In some embodiments, the organic solvent includes at least one of anisole, ethylene dichloride, chloroform, and dimethylformamide.

[0074] The above organic solvents have good solubility for the polymer matrix, which is conducive to uniform mixing of the zinc salt, the lithium imide salt and the polymer matrix.

[0075] In some embodiments, the pre-pressing includes: pressing at a pressure of 10 MPa to 15 MPa for 10 to 15 minutes.

[0076] The above operation is conducive to pressing the precursor into a blank, which is conducive to the subsequent hot pressing and shaping.

[0077] Exemplarily, the pre-pressing pressure is any value among 10Mpa, 11Mpa, 12Mpa, 13Mpa, 14Mpa, 15MPa or between any two values, and the pre-pressing time is any value among 10min, 11min, 12min, 13min, 14min, 15min or between any two values.

[0078] The step of mixing the zinc salt, the lithium imide salt, the polymer matrix and the organic solvent for dissolving the polymer matrix can be performed by adding the zinc salt, the lithium imide salt and the polymer matrix into the organic solvent and stirring to mix them, or the polymer matrix can be first dissolved in the organic solvent and then mixed with the zinc salt and the lithium imide salt.

[0079] In some embodiments, the step of mixing comprises:

[0080] Dissolving the polymer matrix in an organic solvent to obtain a polymer solution;

[0081] The zinc salt and the lithium imide salt are mixed with the polymer solution under stirring.

[0082] The method of first dissolving the polymer matrix in an organic solvent and then mixing it with the zinc salt and lithium imide salt is beneficial for fully and evenly mixing the three and for uniform distribution of the components in the precursor obtained by drying, thereby improving the uniformity of the reaction between zinc ions and the polymer matrix during the subsequent hot pressing reaction and improving the performance of the polymer solid electrolyte membrane.

[0083] After mixing, the precursor is dried to obtain the precursor. It is understood that the drying temperature should be less than the minimum hot pressing temperature, and the zinc ions and the polymer matrix do not chemically react during the drying process. Therefore, the drying can be vacuum drying, wherein the vacuum drying temperature is less than the minimum hot pressing temperature.

[0084] In some embodiments, the drying is performed under vacuum at a low temperature of 50°C to 80°C.

[0085] By using the above-mentioned low-temperature vacuum drying method, on the basis of achieving the purpose of drying, chemical reactions between the components and the air, or between the components, such as zinc ions and the polymer matrix, can be effectively avoided, which is beneficial to improving the performance of the polymer solid electrolyte membrane.

[0086] Exemplarily, the temperature of low-temperature vacuum drying is any one of 50° C., 60° C., 70° C., 80° C., or between any two values.

[0087] The present application also provides a polymer solid electrolyte membrane, which is prepared by the preparation method provided by the present application.

[0088] The present application provides a polymer solid electrolyte membrane having a block structure in which flexible segments and rigid segments alternate with each other to present a three-dimensional network. When the polymer solid electrolyte membrane is applied to a solid-state battery, it can effectively improve the cycle performance of the solid-state battery and enable the solid-state battery to have good long-term and short-term electrical properties and safety performance.

[0089] Exemplarily, the thickness of the polymer solid electrolyte membrane is 1 μm-1000 μm.

[0090] The present application also provides a polymer solid electrolyte membrane, which has a block structure in which rigid segments and flexible segments are alternately connected to present a three-dimensional network;

[0091] The rigid chain segments are crosslinked with nanometer-scale zinc ion aggregate particles as crosslinking points, and the zinc ion aggregate particles react with polar functional groups on the polymer matrix to form a tangled body with a certain rigidity by crosslinking multiple polymer molecular chains, and the polar functional groups include -OH and / or -COC-;

[0092] The flexible chain segments are free polymer molecular chains in a free state.

[0093] Among them, the polymer solid electrolyte with the above block structure can not only use the unique structure of alternating rigid and flexible segments to build a stable lithium ion transmission network, effectively inhibiting the battery capacity decay and the generation of lithium dendrites, but also Zn 2+ In addition to serving as a crosslinking point, it can also capture some TFSI-, making more Li + It can migrate on the polymer chain to improve the conductivity, and has good mechanical properties and a certain degree of ductility, which can effectively prevent external factors or lithium dendrites from damaging the electrolyte structure.

[0094] That is, the polymer solid electrolyte membrane provided in the present application can effectively improve the cycle performance of the solid-state battery when applied to the solid-state battery, and enable the solid-state battery to have good long-term and short-term electrical properties and safety performance.

[0095] The present application also provides a solid-state battery, which includes the polymer solid electrolyte membrane provided by the present application.

[0096] Solid-state batteries are lithium batteries. Generally, solid-state batteries include a positive electrode, a negative electrode, and a polymer solid electrolyte membrane. During the charge and discharge process of solid-state batteries, active lithium ions are embedded and extracted back and forth between the positive electrode and the negative electrode. The polymer solid electrolyte membrane plays the role of conducting lithium ions between the positive electrode and the negative electrode.

[0097] The solid-state battery may be a full battery or a half battery. The outer packaging of the solid-state battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc., or a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0098] The present application has no particular limitation on the shape of the solid-state battery, which may be cylindrical, square, or any other shape.

[0099] The present application also provides an electrical device, which includes a solid-state battery.

[0100] Solid-state batteries can be used as power sources for electrical devices or as energy storage units for electrical devices. Electrical devices can be, but are not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc.; mobile devices can include, but are not limited to, at least one of mobile phones and laptops; electric vehicles can include, but are not limited to, at least one of pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.

[0101] The polymer solid electrolyte membrane and its preparation method, solid-state battery and electrical device of the present application are further described in detail below in conjunction with the embodiments.

[0102] Example 1

[0103]

Polymer solid electrolyte membrane

[0104] 1) 50 g of polyethylene oxide (PEO) polymer with a molecular weight of 13,000 was placed in 200 g of anisole and stirred at 300 r / min for 50 min to fully dissolve the PEO to obtain a polymer solution;

[0105] 2) Take 0.8 g of zinc fluoride (ZnF2) and 22 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), put them into the above polymer solution, and stir at 400 r / min for 18 min to fully mix the polymer matrix, lithium salt and cross-linking agent to obtain a polymer precursor solution.

[0106] 3) The polymer precursor solution obtained in step 2) is placed in a vacuum oven, evacuated to -0.1 MPa, and dried at 60° C. for 12 h, and the solvent is completely removed to obtain a uniformly mixed precursor of PEO, LiTFSI and ZnF2.

[0107] 4) The precursor was placed in a 100 μm deep mold and pressed at 13 MPa for 12 min at 25 °C to obtain a thin and uniform green body;

[0108] 5) placing the green body obtained in step 4) in a mold with a depth of 100 μm, placing it in a double-plate hot press, adjusting the hot pressing temperature of the upper and lower plates to 110°C, and after the hot pressing temperature stabilizes, hot pressing is performed at a hot pressing pressure of 13 MPa for 40 minutes, and the polymer film obtained by hot pressing is taken out and naturally cooled to 25°C to obtain a block polymer polymer solid electrolyte membrane with a stable cross-linked network.

[0109]

Button-type semi-solid battery

[0110] LiNi 0.9 Co 0.05 Mn 0.05 , conductive agent SP and binder PVDF are mixed in a ratio of 90:5:5 and homogenized in NMP system, the slurry is coated on aluminum foil, and then dried and rolled to obtain LiNi 0.9 Co 0.05 Mn 0.05 Pole piece.

[0111] Take lithium sheet as negative electrode and LiNi 0.9 Co 0.05 Mn 0.05 The pole piece is used as the positive pole piece, the nickel foam is used as the buffer gasket, and the block polymer solid electrolyte is assembled to obtain a button-type semi-solid battery.

[0112] Example 2

[0113] The only difference between it and Example 1 is that the polymer matrix PEO is replaced by polyvinyl alcohol (PVA), and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as in Example 1.

[0114] Example 3

[0115] The only difference between it and Example 1 is that the polymer matrix PEO is replaced by polypropylene oxide (PPO), and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as those in Example 1.

[0116] Example 4

[0117] The only difference between it and Example 1 is that the polymer matrix PEO is replaced by polybutylene oxide (PBO), and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as those in Example 1.

[0118] Example 5

[0119] The only difference between it and Example 1 is that zinc fluoride is replaced by zinc chloride (ZnCl2), and the other parameters such as the content of each component, degree of polymerization, preparation conditions, etc. are the same as those in Example 1.

[0120] Example 6

[0121] The only difference between it and Example 1 is that zinc fluoride is replaced by zinc bromide (ZnBr2), and the other parameters such as the content of each component, degree of polymerization, preparation conditions, etc. are the same as those in Example 1.

[0122] Example 7

[0123] The only difference between it and Example 1 is that the cross-linking agent is changed to zinc bromide (ZnI2), and the other parameters such as the content of each component, degree of polymerization, preparation conditions, etc. are the same as those in Example 1.

[0124] Example 8

[0125] The only difference between it and Example 1 is that in step 5), the hot pressing temperature is changed to 120° C., the hot pressing pressure is 13 MPa, and the hot pressing time is 40 min. The other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as in Example 1.

[0126] Example 9

[0127] The only difference between it and Example 1 is that in step 5), the hot pressing pressure is changed to 15 MPa, the hot pressing temperature is set to 110° C., the hot pressing time is 40 min, and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as in Example 1.

[0128] Example 10

[0129] The only difference between it and Example 1 is that the hot pressing time in step 5) is changed to 45 min, the hot pressing temperature is set to 110° C., the hot pressing pressure is 13 MPa, and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as in Example 1.

[0130] Embodiment 11

[0131] The only difference between it and Example 1 is that the molecular weight of PEO is 10000, and the contents of other components, degree of polymerization, preparation conditions and other parameters are the same as those in Example 1.

[0132] Example 12

[0133] The only difference between it and Example 1 is that the molecular weight of PEO is 18000, and the contents of other components, degree of polymerization, preparation conditions and other parameters are the same as those in Example 1.

[0134] Comparative Example 1

[0135] The only difference between it and Example 1 is that the amount of zinc fluoride added is replaced by 0.36 g, and the contents of other components, degree of polymerization, preparation conditions and other parameters are the same as in Example 1.

[0136] Comparative Example 2

[0137] The only difference between it and Example 1 is that the amount of zinc fluoride added is replaced by 1.08 g, and the contents of other components, degree of polymerization, preparation conditions and other parameters are the same as in Example 1.

[0138] Comparative Example 3

[0139] The only difference between it and Example 1 is that the hot pressing time is adjusted to 30 minutes, and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as those in Example 1.

[0140] Comparative Example 4

[0141] The only difference between it and Example 1 is that the hot pressing time is adjusted to 50 minutes, and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as those in Example 1.

[0142] Comparative Example 5

[0143] The only difference between it and Example 1 is that the hot pressing temperature is adjusted to 80° C., and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as those in Example 1.

[0144] Comparative Example 6

[0145] The only difference between it and Example 1 is that the hot pressing temperature is adjusted to 150° C., and the other parameters such as the content of each component, degree of polymerization, and preparation conditions are the same as those in Example 1.

[0146] Comparative Example 7

[0147] The only difference between it and Example 1 is that lithium bis(trifluoromethanesulfonyl)imide is replaced with lithium hexafluorophosphate (LiPF6), and the contents of other components, degree of polymerization, preparation conditions and other parameters are the same as those in Example 1.

[0148] Test Example 1

[0149] The performance of the polymer solid electrolyte membrane and button-type solid-state battery prepared in each embodiment and comparative example was tested respectively, and the specific testing method included:

[0150] [Short-term power test] refers to the peak power test result of the button-type semi-solid-state battery obtained by charging the button-type semi-solid-state battery for 10 seconds at an ambient temperature of 25°C and a state of charge (SOC) of 50%. The peak power test result is expressed in Table 1 as 25°C@50%SOC 10s DCR.

[0151] [Rate performance 2C / 0.2C] The battery is tested at different rates of 2C and 0.2C on the LAND battery test system (CT2001A) charge and discharge tester. The test conditions are constant current charge and discharge. At a constant temperature of 20°C, the voltage range is 2.5-4.2V, and the test rate performance is 2C / 0.2C.

[0152] [Number of Cycles] In a 45°C oven, the button-type semi-solid-state battery is cyclically charged and discharged at a current of 1C in a specified potential range, and the discharge capacity of each cycle is recorded. The test is terminated when the solid-state battery capacity reaches 80% of the first cycle capacity, and the number of cycles at this time is recorded, which is recorded as the number of cycles corresponding to 45°C 80% SOH in Table 1.

[0153] [Capacity retention rate] At an ambient temperature of -10°C, the button-type semi-solid-state battery was cycled for 500 cycles at a current of 0.33C in a specified potential range, and the capacity retention rate at this time was recorded, which is recorded as -10°C 0.33C capacity retention rate in Table 1.

[0154] [Ionic conductivity] At 25°C, a 10mm diameter cylindrical stainless steel current collector is used to tightly clamp the polymer solid electrolyte membrane under mechanical pressure in the battery mold, and then the current collector is connected to the electrochemical workstation to perform electrochemical impedance testing on the polymer solid electrolyte membrane at a bias voltage of 10mV and a frequency range of 106Hz to 0.1Hz. The Z' coordinate value of the point closest to the Z' axis from right to left in the low-frequency band of the curve in the electrochemical impedance spectrum is taken as the resistance value R, and the ionic conductivity σ is calculated using the formula: σ=D / AR, where D is the thickness of the polymer solid electrolyte membrane, A is the contact area between the polymer solid electrolyte membrane and the current collector, and R is the impedance. It is recorded as 25°C ionic conductivity in Table 1.

[0155] [Young's modulus] The Young's modulus of the polymer solid electrolyte membrane with a size of 70mm×20mm×0.05mm was tested using a universal tensile machine. The tensile rate during the test was 0.1min -1 .

[0156] The results are shown in Table 1.

[0157] Table 1 Test results

[0158]

[0159]

[0160] It can be seen from Table 1 that the polymer solid electrolyte membrane provided in the present application has both good mechanical properties and ion conductivity properties. The solid-state battery using the polymer solid electrolyte membrane has good long-term and short-term electrical properties and safety performance, especially increasing the number of cycles corresponding to 80% SOH of the solid-state battery and improving its cycle life.

[0161] It can be seen from Example 1 and Comparative Examples 1-2 that the mass ratio between the zinc salt and the main body is too large or too small, which affects the smooth construction of the block structure of the polymer solid electrolyte, resulting in low cycle performance of the solid-state battery. Controlling the mass ratio of the zinc salt and the main body to (0.8-1.2):100 and performing hot pressing with specific parameters can effectively construct the above-mentioned flexible segments and rigid segments alternating with each other to present a three-dimensional network block structure, effectively improving the number of cycles corresponding to 80% SOH of the solid-state battery.

[0162] According to Example 1 and Comparative Examples 3-6, it can be seen that the hot pressing pressure, hot pressing temperature and hot pressing time all affect the effective construction of a three-dimensional network block structure in which the flexible segments and the rigid segments alternate with each other. The present application selects a hot pressing pressure of 10Mpa to 15Mpa and a hot pressing temperature of 100°C to 120°C for 35min to 45min. The selection of the raw materials is conducive to the preparation of a polymer solid electrolyte membrane with a three-dimensional network block structure, thereby effectively improving the cycle performance and other electrochemical properties of the solid-state battery.

[0163] It can be seen from Example 1 and Comparative Example 7 that the selection of lithium salt will significantly affect the ionic conductivity of the polymer solid electrolyte membrane and the performance of the final battery. Among them, the selection of imide lithium salt as the electrolyte salt in the polymer solid electrolyte membrane of the present application is beneficial to improving the ionic conductivity of the polymer solid electrolyte membrane and the battery cycle life.

[0164] In summary, the polymer solid electrolyte membrane provided in the present application has both good mechanical properties and ion conductivity properties. When the polymer solid electrolyte membrane is applied to a solid-state battery, it can effectively improve the cycle performance of the solid-state battery and enable the solid-state battery to have good long-term and short-term electrical properties and safety performance.

[0165] The above are only specific embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a polymer solid electrolyte membrane, characterized in that: The following steps are involved: Mixing zinc salt, lithium imide salt, polymer matrix and an organic solvent for dissolving the polymer matrix, and drying to obtain a precursor; After the precursor is pre-pressed, the obtained green body is hot-pressed for 35 minutes to 45 minutes under the conditions of a hot-pressing pressure of 10 MPa to 15 MPa and a hot-pressing temperature of 100° C. to 120° C.; The decomposition temperature of the lithium imide salt is greater than the hot pressing temperature, the melting temperature of the polymer matrix is ​​≤100°C and the glass transition temperature is ≤-15°C, the polymer matrix contains polar functional groups, and the polar functional groups include -OH and / or -COC-. The lithium imide salt and the polymer matrix are used as the main body, and the mass ratio of the zinc salt to the main body is (0.8-1.2):

100.

2. The preparation method according to claim 1, characterized in that: The zinc salt includes zinc halide, and the zinc halide includes at least one of zinc fluoride, zinc chloride, zinc bromide and zinc iodide.

3. The preparation method according to claim 1, characterized in that: The polymer matrix includes at least one of polyvinyl alcohol, polyethylene oxide, polypropylene oxide, and polybutylene oxide.

4. The preparation method according to claim 1, characterized in that: The molecular weight of the polymer matrix is ​​10,000-18,000.

5. The preparation method according to claim 1, characterized in that: The molecular weight of the polymer matrix is ​​12,000 to 15,000.

6. The preparation method according to claim 1, characterized in that: The lithium imide salt includes lithium bis(trifluoromethanesulfonyl)imide.

7. The preparation method according to any one of claims 1 to 6, characterized in that: In the main body, the mass ratio of the imide lithium salt to the polymer matrix is ​​(25-35):(65-75).

8. The preparation method according to any one of claims 1 to 6, characterized in that: The organic solvent includes at least one of anisole, ethylene dichloride, chloroform and dimethylformamide.

9. The preparation method according to any one of claims 1 to 6, characterized in that: The pre-pressing comprises: pressing for 10 min to 15 min under the condition of 10 MPa to 15 MPa.

10. The preparation method according to any one of claims 1 to 6, characterized in that: The mixing step comprises: dissolving the polymer matrix in the organic solvent to obtain a polymer solution; The zinc salt, the lithium imide salt and the polymer solution are mixed under stirring conditions.

11. The preparation method according to any one of claims 1 to 6, characterized in that: The drying is performed at a low temperature of 50°C to 80°C in vacuum.

12. A polymer solid electrolyte membrane, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 11.

13. A polymer solid electrolyte membrane, characterized in that: The solid electrolyte membrane has a block structure in which rigid segments and flexible segments are alternately connected to form a three-dimensional network; The rigid chain segments are cross-linked with nanometer-scale zinc ion aggregate particles as cross-linking points, and the zinc ion aggregate particles react with polar functional groups on the polymer matrix to form a tangled body with a certain rigidity by cross-linking multiple polymer molecular chains, wherein the polar functional groups include -OH and / or -COC-; The flexible chain segment is a free polymer molecular chain in a free state.

14. A solid-state battery, characterized in that: It comprises the polymer solid electrolyte membrane according to claim 12 or 13.

15. An electrical device, characterized in that: It includes the solid-state battery as claimed in claim 14.

Citation Information

Patent Citations

  • Composite solid electrolyte membrane, preparation method thereof and all-solid-state lithium metal battery

    CN114927753A

  • Coordination polymer solid electrolyte, preparation method thereof and solid-state battery

    CN115332623A

  • Sodium ion composite polymer solid electrolyte and preparation method thereof

    CN116826152A

  • Polymer electrolyte and preparation method thereof, sulfide composite material and method and application thereof

    CN117199514A

  • Polymer solid electrolyte membrane and preparation method and application thereof

    CN117996206A

Cited By

  • Cross-linked polymer solid electrolyte and preparation method thereof

    CN120895725A

  • Polymer solid electrolyte membrane, preparation method therefor, solid-state battery, and electrical apparatus

    WO2025246146A1