Spherical zinc deposition growth regulator and electrolyte for concentrated alkaline zinc-based battery

By using polydimethyldiallylammonium chloride as a spherical zinc deposition growth regulator in alkaline zinc-based batteries to adjust the electrolyte state, the problems of zinc anode instability and uneven deposition are solved, and the battery is realized High cycle stability and long life.

CN118738596APending Publication Date: 2024-10-01XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953184.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In alkaline zinc-based batteries, the instability of the zinc anode and the random diffusion of zincate ions lead to uneven deposition, resulting in short-circuit failure of the battery and low utilization of active materials. It is difficult to effectively control this problem with existing technology.

Method used

Polydimethyldiallylammonium chloride (PDA) containing strong cationic groups is added to the alkaline electrolyte of an alkaline zinc-based battery as a spherical zinc deposition growth regulator to adjust the physical and chemical state of the electrolyte and reduce zinc The diffusion rate of salt ions promotes their uniform and orderly migration and induces dense spherical growth.

Benefits of technology

By adjusting the distribution of zincate ions to avoid space charge effects and achieve uniform nucleation and dense spherical growth of zinc, the cycle stability of the battery and the utilization rate of active materials are significantly improved, and the life of the battery is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738596A_ABST
    Figure CN118738596A_ABST
Patent Text Reader

Abstract

The invention provides a spherical zinc deposition growth regulator for a concentrated alkaline zinc-based battery and an electrolyte. Polydimethyldiallylammonium chloride (PDA) containing strong cation groups is used as the spherical zinc deposition growth regulator to be added into the alkaline electrolyte of the alkaline zinc-based battery. The spherical zinc deposition growth regulator can regulate the physical and chemical state of the alkaline electrolyte to reduce the diffusion rate of zincate ions [Zn (OH) 4] 2-and promote uniform and ordered migration of [Zn (OH) 4] 2-, so that uniform nucleation of zinc is regulated and controlled, and compact spherical growth is induced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alkaline zinc-based batteries, and in particular to a spherical zinc deposition growth regulator and an electrolyte for concentrated alkaline zinc-based batteries. Background Art

[0002] In recent years, the booming development of electric vehicles, microelectronics, and grid energy storage has increased the urgent demand for advanced energy storage devices with excellent performance and safety. Low cost, abundant mineral reserves, environmental friendliness, and especially high safety and reliability make aqueous zinc-based batteries one of the competitive candidates. Depending on the pH of the electrolyte, aqueous zinc-based batteries are divided into conventional aqueous zinc-ion batteries and alkaline zinc-based batteries. At present, various aqueous alkaline zinc-based batteries have been reported and partially commercialized, such as nickel-zinc batteries, zinc-silver batteries, zinc-manganese batteries, and zinc-air batteries.

[0003] In alkaline zinc-based batteries, the instability of the zinc negative electrode has hindered its large-scale practical application. Different from the alkaline electrolyte of conventional aqueous zinc-ion batteries, the zinc ions in the concentrated alkaline electrolyte system are mostly zincate ions [Zn(OH)4] 2- It exists in the form of Zn-ZnO deposition product conversion intermediate. During the electrodeposition process, the dissolved [Zn(OH)4] 2- In alkaline electrolyte, it diffuses randomly, resulting in uneven ion distribution at the electrode / alkaline electrolyte interface, large concentration gradient difference and space charge layer, so [Zn(OH)4] 2- They tend to aggregate and deposit at the tips. The uneven, fluffy deposition structure then grows into moss-shaped dendrites, accelerating the short-circuit failure of the battery. In addition, due to the particularity of the alkaline electrolyte system, zinc dendrites on the electrode interface are easily passivated by contact with the alkaline electrolyte to form "dead zinc", reducing the utilization rate of active substances. Therefore, regulating the deposition growth morphology of zinc negative electrodes in alkaline electrolytes is crucial for further applications.

[0004] Existing zinc anode optimization methods mainly focus on surface area modification and three-dimensional structure design of zinc anode to reduce electrode passivation, improve zinc utilization and inhibit dendrites. These strategies usually adopt a "passive defense" tactic and do not fundamentally regulate [Zn(OH)4] 2- Therefore, a spherical zinc deposition growth regulator is developed to alleviate the problem of random diffusion and tip deposition in alkaline electrolyte [Zn(OH)4] 2- The concentration gradient distribution and change of the uneven deposition morphology of zinc have important research significance. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a spherical zinc deposition growth regulator and an electrolyte for a concentrated alkaline zinc-based battery. Polydimethyldiallylammonium chloride (PDA) containing a strong cationic group is added as a spherical zinc deposition growth regulator to the alkaline electrolyte of the alkaline zinc-based battery. The spherical zinc deposition growth regulator can adjust the physical and chemical state of the alkaline electrolyte to reduce the zincate ion [Zn(OH) 4 ] 2- The diffusion rate of [Zn(OH) 4 ] 2- Uniform and orderly migration, thereby regulating the uniform nucleation of zinc and inducing dense spherical growth.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries, wherein the pH of the alkaline electrolyte of the concentrated alkaline zinc-based battery is ≈ 14, and the spherical zinc deposition growth regulator is polydimethyldiallylammonium chloride containing a strong cationic group.

[0007] Further, the structural formula of polydimethyldiallylammonium chloride is:

[0008]

[0009] Furthermore, the spherical zinc deposition growth regulator is added to the alkaline electrolyte of the concentrated alkaline zinc-based battery for use, and the concentration range of the spherical zinc deposition growth regulator is 1% to 10% based on the total weight of the alkaline electrolyte solvent.

[0010] Furthermore, the spherical zinc deposition growth regulator is added to the alkaline electrolyte of the concentrated alkaline zinc-based battery for use, and the concentration range of the spherical zinc deposition growth regulator is 5% based on the total weight of the alkaline electrolyte solvent.

[0011] The present invention also provides an alkaline electrolyte for a concentrated alkaline zinc-based battery. A spherical zinc deposition growth regulator is added to the alkaline electrolyte. The spherical zinc deposition growth regulator is polydimethyldiallylammonium chloride containing a strong cationic group.

[0012] Furthermore, the concentration of the spherical zinc deposition growth regulator added is in the range of 1% to 10% based on the total weight of the alkaline electrolyte solvent.

[0013] Furthermore, the concentration range of the spherical zinc deposition growth regulator added is 5%, based on the total weight of the alkaline electrolyte solvent.

[0014] Furthermore, the electrolyte of the alkaline electrolyte comprises an aqueous solvent and an alkaline electrolyte, and the alkaline electrolyte is an inorganic base - potassium hydroxide.

[0015] The present invention also provides a concentrated alkaline zinc-based battery, wherein the alkaline electrolyte of the concentrated alkaline zinc-based battery is the alkaline electrolyte mentioned above.

[0016] Furthermore, the concentration of the alkaline electrolyte is 3 mol / L to 8 mol / L.

[0017] Compared with the prior art, the present invention has at least the following beneficial effects:

[0018] The present invention provides a spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries - polydimethyldiallyl ammonium chloride containing strong cationic groups. An appropriate amount of the spherical zinc deposition growth regulator is added to an alkaline electrolyte to adjust the physicochemical state of the alkaline electrolyte to reduce the zincate ion [Zn(OH) 4 ] 2- The diffusion rate of [Zn(OH) 4 ] 2- In addition, the spherical zinc deposition growth regulator has a strong zinc affinity, buffering between the electrode and the alkaline electrolyte, further reconstructing the [Zn(OH) 4 ] 2- concentration arrangement and promote their orderly transport and movement along the polymer chain.

[0019] The spherical zinc deposition growth regulator used in the present invention can enrich the uniform [Zn(OH) 4 ] 2- Ion flow avoids space charge effect, regulates uniform zinc nucleation and induces dense spherical growth. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a deposition growth morphology of the zinc negative electrode in the concentrated alkaline zinc-based battery electrolyte of Comparative Example 1.

[0021] Figure 2 It is a deposition growth morphology of zinc negative electrode in concentrated alkaline zinc-based battery electrolyte containing Examples 1 to 3 as spherical zinc deposition growth regulator.

[0022] Figure 3 It is a deposition growth morphology of the zinc negative electrode in a concentrated alkaline zinc-based battery electrolyte containing Comparative Example 2 as a spherical zinc deposition growth regulator.

[0023] Figure 4 The results are calculated under molecular dynamics simulation in the concentrated alkaline zinc-based battery electrolyte containing Example 2 and Comparative Example 1 [Zn(OH) 4 ] 2- RMS-time plot of migration.

[0024] Figure 5The zinc-zinc symmetric battery assembled by the electrolyte of Example 1 of the present invention is 1 mA cm -2 The time-voltage curve below.

[0025] Figure 6 The zinc-zinc symmetric battery assembled by the electrolyte of Example 2 of the present invention is 1 mA cm -2 The time-voltage curve below.

[0026] Figure 7 The zinc-zinc symmetric battery assembled by the electrolyte of Example 3 of the present invention is 1 mA cm -2 The time-voltage curve below.

[0027] Figure 8 The zinc-zinc symmetrical battery assembled with the electrolyte of Comparative Example 1 of the present invention at 1 mA cm -2 The time-voltage curve below.

[0028] Fig. 9 The zinc-zinc symmetrical battery assembled with the electrolyte of Comparative Example 2 of the present invention at 1 mA cm -2 The time-voltage curve below.

[0029] Fig.10 The alkaline zinc-air battery assembled with the electrolytes of Example 2 and Comparative Example 1 at different current densities (0.5-1-2-5-8-10-20-2-1 mA cm -2 )’s rate curve.

[0030] Fig.11 The symmetrical battery assembled by the electrolyte of Example 2 of the present invention and Comparative Example 1 is an alkaline zinc-air battery at 10 mA cm -2 Cycle life curve.

[0031] Fig.12 It is the cycle life curve of the symmetrical battery assembled by the electrolyte of Example 2 of the present invention and the comparative example 1 in the alkaline nickel-zinc battery. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0033] Unless otherwise defined, the professional terms used below have the same meanings as those understood by professionals in the field; unless otherwise specified, the raw materials and reagents involved in this article can be purchased from the market or prepared by known methods.

[0034] The present invention provides a spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries, wherein the pH of the concentrated alkaline zinc-based batteries is approximately 14, and a polydimethyldiallylammonium chloride (PDA) containing a strong cationic group is specifically selected. The specific structural formula of the spherical zinc deposition growth regulator is shown in Formula 1:

[0035] Formula 1:

[0036]

[0037] The spherical zinc deposition growth regulator is added to an alkaline electrolyte for use. The concentration of the spherical zinc deposition growth regulator is in the range of 1% to 10% based on the total weight of the alkaline electrolyte solvent.

[0038] Preferably, the concentration of the spherical zinc deposition growth regulator added to the alkaline electrolyte is 5%. In an embodiment, the alkaline electrolyte comprises an aqueous solvent and an alkaline electrolyte.

[0039] Preferably, the aqueous solvent is pure water.

[0040] Preferably, the electrolyte is an inorganic base - potassium hydroxide (KOH), and the concentration of the prepared alkaline electrolyte is 3 mol / L to 8 mol / L.

[0041] The present invention also provides a concentrated alkaline zinc-based battery, in which 1% to 10% of a spherical zinc deposition growth regulator is added to the alkaline zinc-based battery electrolyte. The above-mentioned concentrated alkaline zinc-based battery can be a zinc-zinc symmetrical battery composed of commercial zinc foil, glass fiber separator and concentrated alkaline zinc-based battery electrolyte containing a spherical deposition growth regulator; or an alkaline zinc-air battery composed of commercial zinc foil as the negative electrode, air catalytic material as the positive electrode, and concentrated alkaline zinc-based battery electrolyte containing a spherical deposition growth regulator; or an alkaline nickel-zinc battery composed of commercial zinc oxide as the negative electrode, commercial nickel hydroxide as the positive electrode, and concentrated alkaline zinc-based battery electrolyte containing a spherical deposition growth regulator. The above-mentioned concentrated alkaline zinc-based battery is subjected to a cycle performance test, and the life of the zinc-zinc symmetrical battery exceeds 500 hours. Both the alkaline zinc-air full battery and the alkaline nickel-zinc battery show excellent long-cycle stability.

[0042] Preferably, the positive electrode active material of the alkaline zinc-air battery is an air catalyst, preferably at least one of a platinum-carbon catalyst or an oxidized noble metal catalyst (iridium oxide, ruthenium oxide, etc.).

[0043] Preferably, the positive electrode active material of the alkaline nickel-zinc battery is nickel hydroxide.

[0044] Example 1

[0045] The invention discloses a spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries. The spherical zinc deposition growth regulator is polydimethyldiallylammonium chloride (PDA). The concentration of the spherical zinc deposition growth regulator in alkaline electrolyte is 1%, which is recorded as 1PDA.

[0046] Example 2

[0047] The invention discloses a spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries. The spherical zinc deposition growth regulator is polydimethyldiallylammonium chloride (PDA). The concentration of the spherical zinc deposition growth regulator in alkaline electrolyte is 5%, which is recorded as 5PDA.

[0048] Example 3

[0049] The invention discloses a spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries. The spherical zinc deposition growth regulator is polydimethyldiallylammonium chloride (PDA). The concentration of the spherical zinc deposition growth regulator in alkaline electrolyte is 10%, which is recorded as 10PDA.

[0050] Comparative Example 1

[0051] An alkaline electrolyte without an alkaline zinc-based battery spherical zinc deposition growth regulator, wherein the concentration of the spherical zinc deposition growth regulator is 0%, recorded as 0PDA.

[0052] Example 4

[0053] Study on the optimal concentration of spherical zinc deposition growth regulator to regulate the growth of spherical zinc deposition:

[0054] The deposition growth morphology of the zinc negative electrode in the concentrated alkaline zinc-based battery alkaline electrolyte using the above Examples 1 to 3 as spherical zinc deposition growth regulators and Comparative Example 1 was microscopically photographed using a scanning electron microscope.

[0055] Figure 1 This is a deposition growth morphology of the zinc negative electrode in the concentrated alkaline zinc-based battery electrolyte of Comparative Example 1. The electroplated zinc deposition morphology in Comparative Example 1 is loose, randomly grown moss-like zinc dendrites with an average height of more than 500 μm.

[0056] Figure 2 It is a deposition growth morphology of zinc negative electrode in concentrated alkaline zinc-based battery electrolyte containing spherical zinc deposition growth regulator of Examples 1 to 3. It can be seen from the figure that the zinc deposition morphology changes significantly when using spherical zinc deposition growth regulators with different concentrations. However, the concentrations of Examples 1 and 3 cannot stably regulate the spherical deposition growth of zinc, and larger protrusions are generated. When the spherical zinc deposition growth regulator is added in an appropriate amount (Example 2), zinc balls can be stably deposited and the growth morphology is very uniform, with a maximum height of only 200μm.

[0057] This indicates that the introduction of an appropriate amount of the spherical zinc deposition growth regulator significantly regulates the growth morphology of the spherical deposition of the negative electrode of concentrated alkaline zinc-based batteries.

[0058] Comparative Example 2

[0059] A spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries, wherein the spherical zinc deposition growth regulator is dimethyldiallyl ammonium chloride (DA), and the concentration of the spherical zinc deposition growth regulator in the alkaline electrolyte is 5%, denoted as 5DA, wherein the specific structural formula of dimethyldiallyl ammonium chloride is shown in Formula 2:

[0060] Formula 2:

[0061]

[0062] Example 5

[0063] Study on the role of polymer segments in PDA spherical zinc deposition growth regulator:

[0064] The deposition growth morphology of the zinc negative electrode in the concentrated alkaline zinc-based battery electrolyte containing the above-mentioned comparative example 2 as a spherical zinc deposition growth regulator was microscopically photographed using a scanning electron microscope.

[0065] Figure 3 This is a deposition growth morphology of the zinc negative electrode in the concentrated alkaline zinc-based battery electrolyte containing Comparative Example 2. The electroplated zinc deposition morphology in Comparative Example 2 is also relatively random, similar to Comparative Example 1, indicating that the polymer segment of the PDA spherical zinc deposition growth regulator has a very important regulatory effect on the spherical deposition of the zinc negative electrode in the concentrated alkaline zinc-based battery electrolyte.

[0066] Example 6

[0067] Growth regulators of spherical zinc deposits regulate the zincate ion [Zn(OH) 4 ] 2- Diffusion research:

[0068] Molecular dynamics simulation was used to calculate the concentration of [Zn(OH) 4 ] 2- The RMS-time diagram of the migration diffusion. Figure 4 It can be seen that after the growth regulator of zinc negative electrode spherical deposits is added to the concentrated alkaline electrolyte, the electrolyte [Zn(OH) 4 ] 2- The slope of the RMS-time curve was significantly reduced, indicating that [Zn(OH) 4 ] 2- The random diffusion is effectively restricted.

[0069] Example 7

[0070] Assemble the zinc-zinc symmetric cell:

[0071] The electrolytes configured in the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 2 were used to prepare zinc foil as positive and negative electrodes, glass fiber as a separator, and a 2032-type battery shell. The concentrated alkaline zinc-zinc symmetrical battery was assembled in the order of negative electrode shell, tin foil current collector, zinc foil, separator, electrolyte, zinc foil, tin foil current collector, gasket, spring sheet, and positive electrode shell.

[0072] experiment:

[0073] The zinc-zinc symmetric button cells assembled in the embodiments and comparative examples were subjected to electrochemical tests. -2 The constant current charge and discharge test was carried out at a current density of 25°C on the Xinwei battery test system.

[0074] 1. Cycle life

[0075] Figures 5 to 9 Symmetrical cells assembled with the electrolytes in Examples 1 to 3 and Comparative Examples 1 to 2 at 1 mA cm -2 The current density and 0.5 mAh cm -2 The time-voltage curve under the capacity of . It can be seen from the figure that when the electrolyte of Comparative Example 1 or Comparative Example 2 is used, the zinc-zinc symmetric battery quickly short-circuits after dozens of cycles. When the electrolyte containing different concentrations of spherical zinc deposition growth regulator is used, the reversible long cycle stability of the symmetric battery is significantly improved. Among them, when the additive is appropriate (Example 2), the cycle can exceed 550h.

[0076] This shows that the introduction of an appropriate amount of polydimethyldiallylammonium chloride (PDA) significantly improves the cycle life of the symmetric battery.

[0077] 2. Reversible long cycle performance

[0078] The reversible long cycle performance of the zinc-zinc symmetrical batteries assembled in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 is shown in Table 1.

[0079] Table 1 Comparison of reversible long cycle performance between the embodiment and the comparative example

[0080] sample <![CDATA[Current density (mA cm -2 )]]> <![CDATA[Area capacity (mAh cm -2 )]]> Cycle time (h) Example 1 1 0.5 280 Example 2 1 0.5 550 Example 3 1 0.5 140 Comparative Example 1 1 0.5 105 Comparative Example 2 1 0.5 130

[0081] Example 8

[0082] Assembling an alkaline zinc-air battery:

[0083] A platinum-carbon catalyst is used as the positive electrode active material, zinc foil is used as the negative electrode, glass fiber is used as the separator, the electrolyte configured in the above-mentioned Example 2 and Comparative Example 1 is added, and a 2032-type air battery shell is used. The alkaline zinc-air battery is assembled in the order of negative electrode shell, tin foil current collector zinc foil, separator, electrolyte, positive electrode active material, gasket, spring sheet, and positive electrode shell.

[0084] experiment:

[0085] The alkaline zinc-air batteries assembled in Example 2 and Comparative Example 1 were subjected to electrochemical tests. -2 The constant current charge and discharge test was carried out at a current density of 25°C on the Xinwei battery test system.

[0086] 1. Rate performance

[0087] Fig.10 The alkaline zinc-air batteries assembled with the electrolytes in Example 2 and Comparative Example 1 were tested at different current densities (0.5-1-2-5-8-10-20-2-1 mA cm -2 )’s rate performance curve.

[0088] As can be seen from the figure, the addition of an appropriate amount of spherical zinc deposition growth regulator can significantly improve the rate performance of alkaline zinc-air batteries.

[0089] 2. Cycle life

[0090] from Fig.11 It can be seen that at 10 mA cm -2 Under the conditions of high current density and poor electrolyte (<200 μL), the battery containing the electrolyte of Example 2 can stably cycle for 1400 min; while the battery assembled with the electrolyte of Comparative Example 1 fails quickly after 300 min of cycling. This indicates that the growth regulator containing spherical zinc deposits can withstand more severe test conditions, indicating its successful application in stabilizing concentrated alkaline zinc-based battery electrolytes.

[0091] Example 9

[0092] Assembling Alkaline Nickel Zinc Batteries:

[0093] Commercial nickel hydroxide is used as the positive electrode active material, commercial zinc oxide is used as the negative electrode active material, and a glass fiber separator is used as a separator. The electrolyte configured in the above Example 2 and Comparative Example 1 is added, and an alkaline nickel-zinc soft-pack battery is assembled in the order of negative electrode active material, separator, electrolyte, and positive electrode active material.

[0094] experiment:

[0095] Electrochemical tests were performed on the alkaline nickel-zinc batteries assembled in Example 2 and Comparative Example 1. Commercial constant voltage charge and discharge tests were performed on a Xinwei battery test system, and the test temperature was maintained at 25°C.

[0096] Long cycle test was carried out under ultra-high utilization rate (DOD 80%) conditions. Fig.12 As shown in Figure 2, the battery assembled with the electrolyte in Comparative Example 1 failed rapidly after 59 cycles, while the battery could stably cycle for 300 cycles after the introduction of polydimethyldiallylammonium chloride (PDA) regulator, with an average surface capacity of 10 mAh cm -2 , indicating that batteries assembled from electrolytes modified by spherical zinc deposition growth regulators provide a practical solution for achieving long-term stable and high-energy-density concentrated alkaline zinc-based batteries.

[0097] The above are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries, characterized in that: The pH of the concentrated alkaline zinc-based battery alkaline electrolyte is about 14, and the spherical zinc deposition growth regulator is polydimethyldiallylammonium chloride containing a strong cationic group.

2. The spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries according to claim 1, characterized in that: The structural formula of polydimethyldiallylammonium chloride is:

3. The spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries according to claim 1, characterized in that: The spherical zinc deposition growth regulator is added to the alkaline electrolyte of the concentrated alkaline zinc-based battery for use. The concentration range of the spherical zinc deposition growth regulator is 1% to 10% based on the total weight of the alkaline electrolyte solvent.

4. The spherical zinc deposition growth regulator for concentrated alkaline zinc-based batteries according to claim 1, characterized in that: The spherical zinc deposition growth regulator is added to the alkaline electrolyte of a concentrated alkaline zinc-based battery for use. The concentration range of the spherical zinc deposition growth regulator is 5% based on the total weight of the alkaline electrolyte solvent.

5. An alkaline electrolyte for a concentrated alkaline zinc-based battery, characterized in that: The alkaline electrolyte is added with a spherical zinc deposition growth regulator, and the spherical zinc deposition growth regulator is polydimethyldiallylammonium chloride containing a strong cationic group.

6. The alkaline electrolyte for a concentrated alkaline zinc-based battery according to claim 5, characterized in that: The concentration range of the spherical zinc deposition growth regulator added is 1% to 10% based on the total weight of the alkaline electrolyte solvent.

7. The alkaline electrolyte for a concentrated alkaline zinc-based battery according to claim 5, characterized in that: The concentration range of the spherical zinc deposition growth regulator added is 5%, based on the total weight of the alkaline electrolyte solvent.

8. The alkaline electrolyte for a concentrated alkaline zinc-based battery according to claim 5, characterized in that: The electrolyte of the alkaline electrolyte solution comprises an aqueous solvent and an alkaline electrolyte, and the alkaline electrolyte is an inorganic alkali-potassium hydroxide.

9. A concentrated alkaline zinc-based battery, characterized in that: The alkaline electrolyte of the concentrated alkaline zinc-based battery is the alkaline electrolyte described in any one of claims 5 to 8.

10. A concentrated alkaline zinc-based battery according to claim 1, characterized in that: The concentration of the alkaline electrolyte is 3 mol / L to 8 mol / L.