Increasing reactant utilization in FE / V flow batteries
Through the Fe/V redox chemical flow battery, controlling the V5+ ion concentration and optimizing the electrolyte ratio solves the problem of vanadium ion precipitation in flow batteries at high temperatures, achieving high energy density and low-cost battery performance, which is suitable for the Middle East and thermal environments such as North Africa.
Patent Information
- Application Number
- CN202380022123.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-15
- Filing Date
- 2023-02-14
- Publication Date
- 2024-10-01
AI Technical Summary
Existing flow batteries have vanadium ion precipitation problems in high-temperature environments, which affects their stability and energy density. They are also costly and difficult to meet the needs of thermal environments such as the Middle East and North Africa.
Fe/V redox chemical flow battery is used to limit the precipitation of V5+ ions by controlling the concentration ratio of V5+ ions to V4+ ions, using iron ions instead of vanadium ions as the reactant on the positive electrode side, and optimizing the anolyte and cathode electrolysis Liquid volume ratio, improve reactant utilization and energy density.
It achieves a high-energy-density battery that is stable at high temperatures, reduces material costs, meets operating requirements in thermal environments, and improves the long-term cycle performance and energy density of flow batteries.
Smart Images

Figure BDA0004995258830000031 
Figure BDA0004995258830000041 
Figure BDA0004995258830000061
Abstract
Description
[0001] Priority declaration
[0002] This application claims priority to U.S. patent application No. 17 / 651,116 filed on February 15, 2022, the entire contents of which are hereby incorporated by reference. Technical Field
[0003] The present disclosure relates to increasing reactant utilization and energy density in Fe / V mixed chloride and sulfonate flow batteries. Background Art
[0004] Energy storage is increasingly needed in the deployment of renewable energy and in improving grid reliability and efficiency. It is considered a key enabler in the transition from the current fossil-based economy to a zero-carbon economy.
[0005] Almost all countries in the Middle East and North Africa (MENA) region have abundant renewable energy due to their unique geographical location. For example, direct solar radiation (insolation) in the MENA region exceeds 6kWh / m 2 . However, these renewable energy sources are intermittent and require large-scale energy storage systems for continuous and reliable power output. The overall development plan should adopt and focus on appropriate energy storage technologies that will suit the needs and climate of the MENA region. Long-lasting batteries with capacities up to multi-megawatt levels, such as flow batteries, are considered suitable options for timely transfer of this high power as needed.
[0006] Flow batteries are energy storage technologies that store power as chemical energy in flowing solutions (called catholyte and anolyte) from separate storage tanks. Flow batteries are one of the most promising storage options and have the potential to be cheaper and more flexible than other competitors, for example due to their low cost and scalability. In a flow battery, an electrolyte circulates through electrochemical cells where they are separated by ion exchange membranes (IEMs). Electricity is converted into chemical energy in the electrochemical cells for storage and then released during discharge. What makes flow batteries unique is the ability to vary energy and power capacity independently. The energy capacity is defined by the volume of the electrolyte stored in the tanks and the concentration of the redox pairs, while the power rating is defined by the size of the electrodes and the number of cells in the stack. Summary of the invention
[0007] The embodiments described in the examples herein provide a flow battery. The flow battery includes an electrochemical cell unit, wherein the electrochemical cell unit includes an ion exchange membrane, an anode current collector, and a cathode current collector. The space between the ion exchange membrane and the anode current collector forms a first channel, and the space between the ion exchange membrane and the cathode current collector forms a second channel. The ion exchange membrane is configured to allow ions to pass between the first channel and the second channel. The flow battery includes a first tank and a second tank, the first tank being configured to allow an anolyte to flow through the first channel at a first rate, and the second tank being configured to allow a cathode electrolyte to flow through the second channel at a second rate. The cathode electrolyte, or both the cathode electrolyte and the anolyte, contain a mixture of iron ions and vanadium ions.
[0008] Another embodiment described in the examples herein provides a method for generating an electric current. The method includes flowing an anolyte through a first channel in an electrochemical cell, wherein the first channel is formed in a space between an anode current collector and an ion exchange membrane. Flowing a cathode electrolyte through a second channel in an electrochemical cell, wherein the second channel is formed in a space between a cathode current collector and an ion exchange membrane, wherein the first channel and the second channel are separated by an ion exchange membrane, and wherein the cathode electrolyte includes a mixed electrolyte comprising both iron ions and vanadium ions. Flowing ions through the ion exchange membrane to oxidize the anolyte and reduce the cathode electrolyte. Generating an electric current between the anode current collector and the cathode current collector. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 is a diagram of a flow battery using two electrolytes.
[0010] Figure 2 It is a method for operating Fe / V flow battery cells to obtain higher energy density.
[0011] Figure 3 is a schematic diagram of the charge and discharge operation of an electrochemical cell including a mixture of iron ions and vanadium ions in both the catholyte and the anolyte in equal volume ratios, with a charge voltage of up to 1.4V.
[0012] Figure 4 yes Figure 3 Performance curve of liquid flow battery.
[0013] Figure 5 is a schematic diagram of the operation of a flow battery containing a mixture of iron and vanadium ions in both the catholyte and the anolyte, showing the operational changes caused by higher charging voltage and different volume ratios.
[0014] Figure 6 yes Figure 5 Performance curve diagram of an electrochemical battery cell.
[0015] Figure 7 is a graph comparing the energy density of electrolytic cells of the two schemes over multiple charge / discharge cycles.
[0016] Figure 8 It is a cycle efficiency curve of the Fe / V electrolytic cell after 200 cycles.
[0017] Fig. 9 It is the capacity curve of Fe / V battery after 200 cycles. DETAILED DESCRIPTION
[0018] The examples described herein provide a flow battery utilizing an electrolyte mixture of iron ions and vanadium ions as both the anolyte and the catholyte. The charging voltage was increased from 1.4V to 1.6V to increase the energy density.
[0019] Specifically, the higher charging voltage will cause a portion of the cathode electrolyte to 4+ Ions are oxidized to form V 5+ ions. During charging, Fe in the catholyte at voltages up to 1.4 V 2+ The ion is oxidized to Fe 2+ , at higher voltages V 4+ The ions are oxidized to form V 5+ ion.
[0020] However, as described in this article, higher temperatures may cause V 5+ The precipitation of these compounds occurs on the positive side of the battery and at a 100% ratio of V 5+ ions start to drop at about 40°C. This is harmful to the flow battery. This can be solved by limiting V 5+ Ion and V 4+ The concentration ratios of the ions prevent this damage, as described with respect to Table 1.
[0021] The data in Table 1 show that the battery has a high voltage at about 50%, about 60%, about 70%, and about 80% V at temperatures above about 40°C, such as about 55°C and about 60°C. 5+ Ion and V 4+ ions. Tests at about 60°C show that V 5+ Ion and V 4+ The concentration ratio of the ions decreased to about 60%, at which concentration the flow battery showed stable behavior.
[0022] Table 1: At V 5+ With V 4+ Stability test at different concentration ratios
[0023]
[0024]
[0025] Therefore, in the embodiments described herein, the V formed in the catholyte is controlled 5+ ions in an amount to ensure that no more than about 50% to about 60% of the V 4+ ions into V 5+ ions. V 5+ Limiting the proportion of ions to less than about 60% of the total vanadium ions present reduces the V 5+ The possibility of precipitation of ions at operating temperatures up to about 40°C is reduced, and the temperature range is increased to meet the operating requirements in hot environments such as the Middle East and North African countries (MENA). In addition, iron ions are more stable than vanadium ions at higher temperatures, and therefore the presence of iron ions does not affect the stability of the electrolyte.
[0026] To take advantage of the increased energy density, the ratio of anolyte to catholyte was changed from 1:1 to 3:2, which improved the reactant utilization of ions in the catholyte. During discharge, the V 5+ The ion is first reduced to V 4+ ions, then Fe 3+ ions are reduced to Fe 2+ In the anolyte, iron ions do not participate in the reaction, which uses V 3+ / V 2+ Half battery cell.
[0027] Therefore, higher energy density batteries that are stable at higher temperatures can be made. Since the cost of iron is lower than vanadium, it also reduces the capital cost of Fe / V mixed acid flow batteries.
[0028] Figure 1 is a diagram of a flow battery 100 using two electrolytes. In the flow battery 100, energy is stored in electrolytes 102 and 104, which are referred to herein as anolyte 102 and catholyte 104. The electrolytes 102 and 104 are stored in tanks 106 and 108 and are pumped from the tanks 106 and 108, respectively, to the electrochemical cell 110 by dedicated pumps 112.
[0029] In some embodiments, an ion exchange membrane 114 is used in the electrochemical cell 110. The ion exchange membrane 114 separates the electrolytes 102 and 104 to prevent energy loss caused by short circuits, while allowing protons or other ions to pass between the two sides during the charge and discharge cycles and maintain electrical neutrality. In some embodiments, the ion exchange membrane 114 is sulfonated tetrafluoroethylene, such as DuPont Chemical of Wilmington, Virginia, and is available as The ion exchange membrane 114 generally controls the efficiency of the flow battery 100 and is a significant factor affecting the cost of the flow battery 100. Accordingly, in some embodiments, the ion exchange membrane 114 is omitted and the electrolytes 102 and 104 are generally prevented from mixing by laminar flow or made unnecessary by the battery design, such as when a single electrolyte solution is used.
[0030] As electrolytes 102 and 104 are pumped through electrochemical cell 110, they pass through channels 116 and 118. Channels 116 and 118 may include porous electrode materials (such as felt or Raney nickel, etc.) to allow ions and electrons to flow between electrolytes 102 and 104. In some embodiments, for example, when ion exchange membrane 114 is omitted, channels 116 and 118 may be narrow to enhance laminar flow.
[0031] During power generation, ions in the anolyte 102 are oxidized, thereby showing electrons entering the anode current collector 120. The electrons are transferred to the load 124 via line 122. After powering the load 124, the electrons return to the electrochemical cell 110 via another line 126. The electrons re-enter the electrochemical cell 110 from the cathode current collector 128, reducing the ions in the cathode electrolyte 104.
[0032] One of the most mature technologies for flow batteries is based on vanadium redox chemistry and is known as vanadium redox flow battery (VFB). In VFB, vanadium ions are dissolved in an aqueous acid-supported electrolyte. VFB is typically based on V 2+ / V 3+ and V 4+ / V 5+ Redox couple.
[0033] For a vanadium ion flow battery, during discharge, the reaction of the anolyte 102 at the anode current collector 120 is as shown in Equation 1.
[0034] V 2+ →V 3+ +e - , E 0 = -0.25V, relative to SHE (1)
[0035] During discharge, the catholyte 104 reacts at the cathode current collector 128 as shown in Equation 2.
[0036] VO2 + +2H + +e - →VO 2+ +H2O,E 0 = +1.01V, relative to SHE (2)
[0037] Anolyte 102 and catholyte 104 are regenerated during a charging cycle. During a charging cycle, power source 130 removes electrons from cathode current collector 128 through line 132, oxidizing ions in cathode electrolyte 104 to their original state, for example, in the reverse process of Equation 2. Electrons are provided from power source 130 to anode current collector 120 through another line 134, reducing ions in anolyte 102 to their original state, for example, in the reverse process of Equation 1.
[0038] In a VFB, vanadium ions are dissolved in an aqueous acid-supported electrolyte.Since the first demonstration of a VFB, several studies have been conducted to investigate the effects of various electrochemical, chemical, and physical variables in order to optimize the relevant system operating parameters with negligible capacity reduction.
[0039] Although VFB is currently used commercially, there are problems associated with its performance at temperatures above about 40°C, where V 5+ The ions tend to precipitate, which can damage flow batteries. These problems could limit their use in hot environments such as those in MENA countries.
[0040] Therefore, this paper presents flow batteries based on Fe / V redox chemistry as an option for reducing the cost of large-scale energy storage due to the utilization of Fe ions instead of V on the cathode side. 5+ The ion could lead to a significant improvement in the operating temperature window over all vanadium flow batteries. In addition, iron costs less than vanadium, reducing the material cost of flow batteries.
[0041] In a Fe / V flow battery, during a discharge cycle of the flow battery, the catholyte 104 contains Fe 3+ , which is reduced to Fe at the cathode current collector 128 2+ (+), and the anolyte 102 contains V 2+ , which is oxidized to V at the anode current collector 120 H (-), according to the reaction shown below:
[0042]
[0043] However, Fe / V flow batteries may be difficult to commercialize. Cross-contamination of the electrolytes of the two half-cells due to the passage of iron and vanadium ions across the membrane may lead to discharge decay, thereby reducing the life of the electrolyte.
[0044] In addition, Fe / V redox flow batteries have lower energy density than VFB systems due to lower cell operating voltages across the cathode and anode, and inefficient utilization of reactants in the catholyte 104. This is generally due to lower reactant concentrations in the electrolyte than in VFBs. Fe ions have low solubility in hydrochloric acid and sulfuric acid, which limits the total concentration of Fe and V ions in the Fe / V / HCl cell to approximately 1.5 mol L -1 .
[0045] Figure 2 The method 200 for operating a Fe / V flow battery cell to obtain higher energy density is provided. The method begins at box 202, where a solution of iron ions and vanadium ions is prepared. This can be done by dissolving iron metal in a strong acid (such as concentrated HCl), for example, to form a solution with a maximum concentration of 1.5 M based on solubility. Vanadium metal is then dissolved in the acid, for example, to form a mixed ion solution having about 1.5 M vanadium ions in addition to Fe ions.
[0046] At block 204, an anolyte tank in a flow battery is filled with a mixed ion solution. At block 206, a catholyte tank is filled with a mixed ion solution.
[0047] At block 208, the anolyte and catholyte are flowed through the electrochemical cell to generate electricity. In the embodiments described herein, the power output is controlled by the total charging voltage and the volume ratio of the catholyte to the anolyte (e.g., a ratio of 2:3 of catholyte to anolyte). This can be adjusted by controlling the flow rate through the electrochemical cell. At block 210, the load is powered by the electricity generated from the flow battery.
[0048] In addition to Fe 2+ / Fe 3+ In addition to the half-cell reactions, V is also utilized on the positive side of the hybrid V / Fe chloride / sulfide flow battery (i.e., in its catholyte) 4+ / V 5+ Half-cell reactions allow the energy density of Fe / V flow batteries to be increased by about 30%, for example by optimizing the flow rate to volume ratio. Figure 5 and Figure 6 As described above, the flow rate or volume ratio of the cathode electrolyte to the anode electrolyte is 3:2. Fe 2+ Ions and V 4+ions. Improvements in energy density and reagent utilization could reduce the capital cost of Fe / V mixed acid flow batteries by 25% to 30% or more. 4+ To V 5+ The conversion of is limited to 60%, so the tolerance to high temperatures (such as 40°C or higher) is high compared to VFB. This allows the flow battery to meet the operating requirements in the MENA region.
[0049] Examples
[0050] experiment
[0051] Preparation of electrolyte
[0052] A mixed ion solution containing Fe ions and V ions was prepared as described herein. The mixed reactant solution contained 1.25-1.5M Fe / 1.25-1.5MV and 6.6-8.6M Cl - The preparation was performed by dissolving 1.25-1.5 M iron (II) chloride (FeCl2) powder into 6.6-8.6 M hydrochloric acid (HCl) solution at ambient temperature (20°C-25°C) and then stirring for 24 hours.
[0053] After this time, a 50 / 50 molar ratio mixture of V2O3 and V2O5 was added to the FeCl2 solution. The solution was heated to 60°C and stirred for 12 hours. The resulting electrolyte solution was V 3.5+ / Fe 2+ A mixed solution consisting of 50% V 4+ and 50% of V 3+ Add Fe 2+ Solution composition.
[0054] Electrochemical testing of battery cells
[0055] The mixed reactant solution is used as both the catholyte and the anolyte in an electrochemical test cell. Even though these solutions do not flow, the terms catholyte and anolyte remain consistent. Figure 1 , the catholyte 104 is on the positive side during discharge, accepting electrons from the load, while the anolyte 102 is on the negative side during discharge, providing electrons to the load. The volume ratio is determined by the amount added to each side of the test cell. The test cells were separated by a sulfonated polytetrafluoroethylene membrane, which was purchased from Chemours, Wilmington, DE, USA, with a Trademarks available.
[0056] Example 1: Mixed Fe / V electrolyte with 0% vanadium utilization in the catholyte.
[0057] Initial testing used a charge voltage of 1.4V and a 1:1 volume ratio of catholyte to anolyte. Using this charge voltage, only the iron ions in the catholyte reacted, and only the vanadium ions in the anolyte reacted. This will refer to Figure 3 Further explanation.
[0058] Figure 3 1 is a schematic diagram of the charging and discharging operation of an electrochemical cell 302 that includes a mixture of iron ions and vanadium ions in both the catholyte 104 and the anolyte 102 in equal volume ratios. In this example, the cell is charged at a voltage of 1.4 V. During charging, Fe in the catholyte 104 2+ Oxidized to Fe 3 + In the anolyte 102, the charge V 3+ Restore to V 2+ When charged at 1.4 V, the vanadium ions in the cathode electrolyte 104 do not participate in the reaction. Also, the iron ions in the anode electrolyte 102 do not participate in the reaction.
[0059] During discharge, Fe in the catholyte 104 3+ ions are reduced to Fe 2+ , and V in the anolyte 102 2+ ions are oxidized to V 3+ As during charging, the iron ions in the anolyte 102 do not participate in the reaction.
[0060] Figure 4 yes Figure 3 Figure 2 shows the charging performance curve of the flow battery. Charging at 1.4V provides a charging capacity of about 3.3 ampere-hours (Ah).
[0061] Example 2: Mixed Fe / V electrolyte with 50% vanadium utilization in the catholyte.
[0062] Figure 5 1 is a schematic diagram of the operation of an electrochemical cell containing a mixture of iron ions and vanadium ions in both the catholyte 104 and the anolyte 102, which shows the operational changes caused by the higher charging voltage of 1.6V. This increases the energy density of the flow battery. The increase in energy density can be achieved by increasing the reactant utilization in the electrolyte. Since the vanadium component is a more expensive component of the Fe / V flow battery system, the increase in vanadium utilization not only increases the energy density but also reduces the electrolyte cost.
[0063] In order to take advantage of the increased energy density in the catholyte 104, the catholyte / anolyte volume ratio is set to 2:3. Specifically, the catholyte 104 contains two molar volumes of iron ions and two molar volumes of vanadium ions, for a total of four molar volumes. The anolyte 102 contains three molar volumes of iron ions and three molar volumes of vanadium ions, for a total of six molar volumes. This saves 3 / 8 of the total amount of vanadium used compared to a cell without mixed electrolytes.
[0064] In this example, during charging, Fe 2+ First, it is oxidized to Fe 3+ In Fe 2+ After the ions are completely oxidized, V 4+ is oxidized to form V 4+ and V 5+ ions. The charge is controlled to transfer only 50% to 60% of V 4+ ions into V 5+ ions. This maintains the stability of the solution at higher temperatures, for example, reducing the V 5+ The possibility of ion precipitation. In the anolyte 102, charging V 3+ Restore to V 2+ As with Example 1, the iron ions in the anolyte 102 do not participate in the reaction.
[0065] During discharge, V in the catholyte 104 5+ The ion is first reduced to V 4+ ions. Once V 5+ ions are reduced, and Fe in the cathode electrolyte 104 3+ ions are reduced to Fe 2+ During discharge, V in the anolyte 102 3+ ions are reduced to V 2+ As during charging, the iron ions in the anolyte 102 do not participate in the reaction.
[0066] As a result of the higher charging voltage and the change in volume ratio, more than 50% vanadium in the positive electrolyte (catholyte) can be utilized and thus compared to Fe / V cells operating at lower charging voltages (such as with respect to Figure 3 and Figure 4 Compared with the above, a 30% increase in the energy density of Fe / V battery cells was achieved.
[0067] Figure 6 yes Figure 5 The charge curve of the electrochemical cell is shown in Figure 1. 2 The effective area 212 membrane, this test was conducted at an electrolyte volume of 192 mL. The electrolytes used for both the anolyte and catholyte were 1.25 molar (M)V, 1.25M Fe, 6.6M Cl - and 0.8M SO4 2- During charging, Fe in the catholyte 2+ Oxidized to Fe 3+ Once all the Fe 2+ has been converted, and a higher charging voltage drives the cathode electrolyte V 4+ Oxidized to V 5+ As described herein, charging is controlled to avoid less than about 60% of V 4+ Convert to V 5+ , thereby increasing thermal stability. In the anolyte, V 3+ During charging, it is restored to V 2+ .
[0068] Figure 7 is a graph comparing the energy density of the electrolytic cell of the two schemes over multiple charge / discharge cycles. In these tests, the catholyte, anolyte and membrane are as described in relation to Figure 6 described.
[0069] As described herein, the first or common approach ( Figure 3 and Figure 4 ) uses a 1:1 volume ratio of catholyte to anolyte and produces a voltage of up to 1.4V. Figure 7 As shown in , the energy density of a common solution is about 12 Watt-hours / liter (Wh / l).
[0070] New Solution( Figure 5 and Figure 6 ) uses a higher volume ratio of 2:3 of catholyte to anolyte and produces voltages up to 1.6 V. Figure 7 As shown in , the energy density of the new solution is slightly lower than 16Wh / 1.
[0071] Figure 8 The graph shows the cycle efficiency of the Fe / V electrolytic cell after 200 cycles. 2 -Long-term cycling performance of Fe / V redox flow battery cells with a 2.5-kcal electrolyte. In these tests, the catholyte, anolyte and membrane were Figure 6 The coulombic, voltage and energy efficiency remained constant over 200 cycles.
[0072] Fig. 9 This is the capacity curve of the Fe / V battery after 200 cycles. Fig. 9As shown in Figure 2, the Fe / V battery cell also exhibits excellent capacity retention, with no significant capacity loss over 200 cycles. The discharge energy density also remains constant over 200 cycles, indicating that the Fe / V flow battery can be reliably operated over a long period of time. The excellent stability of the Fe / V flow battery over long-term cycles enables the system to be operated with minimal system maintenance.
[0073] Example
[0074] The embodiments described in the examples herein provide a flow battery. The flow battery includes an electrochemical cell unit, wherein the electrochemical cell unit includes an ion exchange membrane, an anode current collector, and a cathode current collector. The space between the ion exchange membrane and the anode current collector forms a first channel, and the space between the ion exchange membrane and the cathode current collector forms a second channel. The ion exchange membrane is configured to allow ions to pass between the first channel and the second channel. The flow battery includes a first tank and a second tank, the first tank being configured to allow an anolyte to flow through the first channel at a first rate, and the second tank being configured to allow a cathode electrolyte to flow through the second channel at a second rate. The cathode electrolyte, or both the cathode electrolyte and the anolyte, contain a mixture of iron ions and vanadium ions.
[0075] In one aspect, the mixture is an equimolar mixture of iron ions and vanadium ions.
[0076] In one aspect, the first rate is greater than the second rate. In one aspect, the ratio between the first rate and the second rate is 3:2. In one aspect, the flow battery includes a pump configured to flow an anolyte through a first channel at a first rate and a pump for flowing a catholyte through a second channel at a second rate.
[0077] In one aspect, the cathode electrolyte comprises both vanadium ions and iron ions. In one aspect, the anolyte comprises both vanadium ions and iron ions. In one aspect, the cathode electrolyte comprises 1.25 moles (M) V, 1.25 MFe, 6.6 MCl-, and 0.8 MSO4 2 -. In one aspect, the catholyte is the same as the anolyte.
[0078] In one aspect, the anode current collector is a carbon-based electrode. In one aspect, the cathode current collector is a carbon-based electrode.
[0079] In one aspect, the first channel comprises a porous electrode material. In one aspect, the porous electrode material is felt or Raney nickel.
[0080] In one aspect, the second channel comprises a porous electrode material. In one aspect, the porous electrode material is felt or Raney nickel.
[0081] In one aspect, the flow battery includes a load connected between the anode current collector and the cathode current collector. In one aspect, the flow battery includes a power source connected to the anode current collector and the cathode current collector.
[0082] In one aspect, the catholyte comprises between 50% and 60% 5+ Oxidized vanadium ion.
[0083] Another embodiment described in the example provides a method for generating an electric current. The method includes flowing an anolyte through a first channel in an electrochemical cell, wherein the first channel is formed in a space between an anode current collector and an ion exchange membrane. Flowing a cathode electrolyte through a second channel in an electrochemical cell, wherein the second channel is formed in a space between a cathode current collector and an ion exchange membrane, wherein the first channel and the second channel are separated by an ion exchange membrane, and wherein the cathode electrolyte includes a mixed electrolyte comprising both iron ions and vanadium ions. Flowing ions through the ion exchange membrane to oxidize the anolyte and reduce the cathode electrolyte. Generating an electric current between the anode current collector and the cathode current collector.
[0084] In one aspect, the method includes flowing the catholyte through the second channel at a rate that is 3 / 2 the rate at which the anolyte flows through the first channel.
[0085] In one aspect, the method includes preparing a mixed electrolyte as an equimolar solution comprising between about 1.25 moles (M) and 1.5 M of vanadium ions and between about 1.25 M and 1.5 M of iron ions, and using the mixed electrolyte as a cathode electrolyte. In one aspect, the method includes using the mixed electrolyte as an anode electrolyte.
[0086] In one aspect, the method includes forming a mixed electrolyte solution comprising about 6.6 MCl - ions and about 0.8M SO4 2- ion.
[0087] Other implementations are within the scope of the following claims.
Claims
1. A flow battery comprising: An electrochemical cell, wherein the electrochemical cell comprises: Ion exchange membranes; Anode current collector; a cathode current collector, wherein the space between the ion exchange membrane and the anode current collector forms a first channel, the space between the ion exchange membrane and the cathode current collector forms a second channel, and wherein the ion exchange membrane is configured to allow ions to pass between the first channel and the second channel: a first tank configured to flow anolyte through the first passage at a first rate; and A second tank is configured to flow a catholyte through the second passage at a second rate, wherein the catholyte, or both the catholyte and the anolyte, comprises a mixture of iron ions and vanadium ions.
2. The flow battery according to claim 1, wherein: The mixture is an equimolar mixture of iron ions and vanadium ions.
3. The flow battery according to claim 1, wherein: The first rate is greater than the second rate.
4. The flow battery according to claim 1, wherein: The ratio between the first rate and the second rate is 3:
2.
5. The flow battery of claim 1, further comprising a pump configured to flow the anolyte through the first channel at the first rate and a pump for flowing the catholyte through the second channel at the second rate.
6. The flow battery according to claim 1, wherein: The catholyte contains both vanadium ions and iron ions.
7. The flow battery according to claim 1, wherein: The anolyte contains both vanadium ions and iron ions.
8. The flow battery according to claim 6, wherein: The catholyte contained 1.25 M V, 1.25 M Fe, 6.6 M Cl - and 0.8M SO4 2- .
9. The flow battery according to claim 8, wherein: The catholyte is the same as the anolyte.
10. The flow battery according to claim 1, wherein: The anode current collector is a carbon-based electrode.
11. The flow battery according to claim 1, wherein: The cathode current collector is a carbon-based electrode.
12. The flow battery according to claim 1, wherein: The first channel includes a porous electrode material.
13. The flow battery according to claim 12, wherein: The porous electrode material is felt or Raney nickel.
14. The flow battery according to claim 1, wherein: The second channel includes a porous electrode material.
15. The flow battery according to claim 14, wherein: The porous electrode material is felt or Raney nickel.
16. The flow battery of claim 1, further comprising a load connected between the anode current collector and the cathode current collector.
17. The flow battery of claim 1, further comprising a power source connected to the anode current collector and the cathode current collector.
18. The flow battery according to claim 1, wherein: The catholyte contains between 50% and 60% of V 5+ Oxidized vanadium ion.
19. A method of generating an electric current, comprising: flowing an anolyte through a first channel in the electrochemical cell, wherein the first channel is formed in a space between an anode current collector and an ion exchange membrane; flowing a catholyte through a second channel in the electrochemical cell, wherein the second channel is formed in a space between a cathode current collector and the ion exchange membrane, wherein the first channel and the second channel are separated by the ion exchange membrane, and wherein the catholyte comprises a mixed electrolyte comprising both iron ions and vanadium ions; flowing ions through the ion exchange membrane to oxidize the anolyte and reduce the catholyte; as well as An electric current is generated between the anode current collector and the cathode current collector.
20. The method of claim 19, comprising flowing the catholyte through the second channel at a rate that is 3 / 2 the rate at which the anolyte flows through the first channel.
21. The method of claim 19, comprising: The mixed electrolyte is prepared as an equimolar solution including between about 1.25 moles (M) and 1.5 M of vanadium ions and between about 1.25 M and 1.5 M of iron ions; and The mixed electrolyte was used as the cathode electrolyte.
22. The method of claim 21, comprising using the mixed electrolyte as the anolyte.
23. The method of claim 21, comprising forming the mixed electrolyte to contain about 6.6 M Cl- ions and about 0.8 M SO4 2 -ion.