Titanium and titanium alloy L-shaped profile forming method
Through the stamping forming method, the problem of defects such as bending and twisting of titanium and titanium alloy profiles during the extrusion forming process is solved, and high-quality forming of titanium and titanium alloy L-shaped profiles is achieved to meet the requirements of high-wall thickness, thin, and Weight requirements, improved mechanical properties and economic benefits.
Patent Information
- Application Number
- CN202411010066.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-08
AI Technical Summary
Titanium and titanium alloy profiles are prone to defects such as bending and twisting during the extrusion forming process, and lack production specifications and quality inspections, resulting in unstable product quality and difficulty in meeting the high-quality needs of aerospace and other industries.
Stamping forming methods are adopted, including making square slabs, heat treatment, stamping forming, vacuum annealing, heat calibration and surface treatment, to achieve uniform forming of titanium and titanium alloy L-shaped profiles through L-shaped profile molds and profile equipment to ensure structural uniformity and dimensional accuracy.
It improves the structural uniformity and appearance quality of titanium and titanium alloy profiles, eliminates defects such as cracks, meets the high wall thickness and weight requirements of aerospace and other industries, shortens the molding cycle, and improves mechanical properties and economic benefits.
Smart Images

Figure CN118744190A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of profile production, and in particular relates to a method for forming a titanium and titanium alloy L-shaped profile. Background Art
[0002] Titanium and titanium alloy profiles are important aircraft structural materials and are widely used in wings, wall panels, bulkheads, etc. Since titanium has a close-packed hexagonal crystal structure at room temperature, it has high strength and is difficult to deform, so the extrusion process of titanium and titanium alloy profiles must be carried out under high temperature conditions. When extruding titanium and titanium alloy profiles, the metal flow differences at different parts of the profile cross section are large, which eventually causes the profile to have defects such as bending and twisting. The twisting or bending of titanium and titanium alloy profiles after extrusion is a problem that cannot be completely avoided, especially in thin-walled asymmetric cross-section titanium and titanium alloy profiles.
[0003] Traditional titanium and titanium alloy extruded profiles have very broad application prospects in aerospace and other fields, but the extrusion process is extremely difficult due to problems such as sticking or distortion. At present, although some production technologies of titanium and titanium alloy profiles have been mastered, the production specifications of titanium and titanium alloy profiles have not yet been formed. The long-term lack of standardized technical requirements and consistent quality inspections has resulted in uneven product quality of titanium and titanium alloy profiles and a lack of competitiveness in the application market.
[0004] Therefore, it is necessary to propose a titanium and titanium alloy L-shaped profile forming method that can effectively improve the quality of titanium and titanium alloy profile products and promote the development of aerospace, weapons and other industries. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for forming L-shaped profiles of titanium and titanium alloys in view of the deficiencies in the above-mentioned prior art. The method adopts a stamping forming method to improve the uniformity of the formed structure of the obtained L-shaped profiles of titanium and titanium alloys. The method is simple to operate, has no welds, has high dimensional accuracy, and improves the appearance quality of the titanium and titanium alloy profiles, effectively solving the problems of high weight requirements, thin wall thickness, and great forming difficulty in the aerospace, weapons and other industries.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for forming a titanium and titanium alloy L-shaped profile, characterized in that the method comprises the following steps:
[0007] Step 1: Making square slabs: According to the target L-shaped profile, titanium sheets or titanium alloy sheets are selected and cut to obtain square slabs;
[0008] Step 2: Heat treatment of the square slab: heat treatment of the square slab is performed using a profile heating device;
[0009] Step 3: stamping to produce an L-shaped profile: installing an L-shaped profile die on a profile stamping device, using the profile stamping device to set a pressing speed and a set pressing force to stamp the heat-treated square slab to obtain an L-shaped profile;
[0010] Wherein, the L-shaped profile mold comprises an L-shaped profile lower mold with an L-shaped groove and an L-shaped profile impact upper mold matching the L-shaped profile lower mold;
[0011] Step 4: Vacuum annealing of profile: vacuum annealing of the L-shaped profile;
[0012] Step 5: Profile thermal correction: Use profile straightening equipment to perform thermal correction on the L-shaped profile after vacuum annealing;
[0013] Step 6: Profile surface treatment: Surface treatment is performed on the L-shaped profile after heat calibration to obtain a finished L-shaped profile.
[0014] The above-mentioned titanium and titanium alloy L-shaped profile forming method is characterized in that: in step 2, before heat treating the square slab, an anti-oxidation coating is coated on the surface of the square slab.
[0015] The above-mentioned titanium and titanium alloy L-shaped profile forming method is characterized in that: in step two, the profile heating equipment is a heating furnace, and when the square slab is heat treated, the heat treatment temperature is lower than the phase change point of the square slab by 80°C to 120°C, and at the heat treatment temperature, the square slab is heated in the heating furnace for 2h to 3h.
[0016] The above-mentioned titanium and titanium alloy L-shaped profile forming method is characterized in that: the profile stamping equipment includes an upper workbench and a lower workbench capable of relative movement, the L-shaped profile lower die is installed on the lower workbench, and the L-shaped profile impact upper die is installed on the upper workbench.
[0017] The above-mentioned titanium and titanium alloy L-shaped profile forming method is characterized in that: the inner die surface of the L-shaped profile lower die includes the L-shaped profile lower die boss end face, the L-shaped profile lower die end face, the L-shaped profile lower die end face R angle, the L-shaped profile lower die groove side face and the L-shaped profile lower die groove bottom face, which are arranged in sequence from top to bottom, and the L-shaped profile lower die groove bottom face is a concave arc surface;
[0018] The bottom of the L-shaped profile impact upper die is provided with an L-shaped profile upper die R angle matching the bottom surface of the L-shaped profile lower die groove, and the L-shaped profile upper die R angle has the same size as the L-shaped profile inner R angle.
[0019] The above-mentioned titanium and titanium alloy L-shaped profile forming method is characterized in that: when using profile stamping equipment to hot stamp the heat-treated square slab, the square slab is placed on the end face of the lower die of the L-shaped profile, and the profile stamping equipment is started, so that the upper workbench drives the L-shaped profile to impact the upper die to hot stamp the square slab until the bottom of the square slab is stamped to the bottom surface of the groove of the lower die of the L-shaped profile to obtain an L-shaped profile.
[0020] The above-mentioned titanium and titanium alloy L-shaped profile forming method is characterized in that: in step four, the vacuum annealing temperature is 500°C to 800°C, and the vacuum annealing holding time is 1h to 2h.
[0021] The above-mentioned method for forming an L-shaped titanium and titanium alloy profile is characterized in that: in step 5, before heat-correcting the L-shaped profile, the profile is first heat-treated according to the method in step 2;
[0022] When the L-shaped profile is subjected to thermal profiling, one end of the L-shaped profile is clamped by the fixed end clamping assembly of the profile straightening equipment, and at the same time, the other end of the profile is clamped by the moving slide and power propulsion assembly of the profile straightening equipment, and the other end of the L-shaped profile is driven to move for straightening.
[0023] The above-mentioned titanium and titanium alloy L-shaped profile forming method is characterized in that: in step six, when the profile is subjected to surface treatment, the surface of the profile is shot peened, degreased, washed with water and dried in sequence.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1. The present invention breaks the traditional method of extrusion molding of titanium and titanium alloy profiles and proposes a new preparation method. The above method can improve the uniformity of the formed structure of the prepared titanium and titanium alloy L-shaped profiles, is simple to operate, has no welds, has high dimensional accuracy, and improves the appearance quality of the titanium and titanium alloy profiles. At the same time, defects such as cracks are eliminated, the molding accuracy is improved, the product quality of the titanium and titanium alloy profiles is improved, the molding cycle is shortened, and the mechanical properties of the profiles are improved.
[0026] 2. The present invention adopts a stamping forming method to obtain titanium and titanium alloy profiles with a wall thickness greater than 2 mm, and the mechanical properties and chemical composition of the titanium and titanium alloy profiles can meet the requirements of relevant standards, effectively solving the problems of high weight requirements, thin wall thickness and great forming difficulty in the aerospace, weapons and other industries.
[0027] 3. The present invention adopts a stamping forming method, which effectively improves the quality and yield rate of titanium and titanium alloy L-shaped profiles, and greatly reduces the production cost of the entire equipment during the manufacturing process of the entire product, thereby significantly improving the economic benefits.
[0028] In summary, the stamping forming method used in the present invention can improve the uniformity of the formed structure of the titanium and titanium alloy L-shaped profiles, is simple to operate, has no welds, has high dimensional accuracy, and improves the appearance quality of the titanium and titanium alloy profiles, effectively solving the problems of high weight requirements, thin wall thickness, and great forming difficulty in the aerospace, weapons and other industries.
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a flowchart of the present invention.
[0031] Figure 2 It is a schematic structural diagram of the profile stamping equipment of the present invention.
[0032] Figure 3 It is a schematic diagram of the positional relationship between the square slab, the L-shaped profile lower die and the L-shaped profile impact upper die during hot stamping of the present invention.
[0033] Figure 4 It is a schematic diagram of the positional relationship between the L-shaped profile after hot stamping, the L-shaped profile lower die and the L-shaped profile impact upper die of the present invention.
[0034] Figure 5 It is a structural schematic diagram of the lower mold of the L-shaped profile of the present invention.
[0035] Figure 6 It is a structural schematic diagram of the L-shaped profile of the present invention.
[0036] Figure 7 It is a structural schematic diagram of the profile straightening device of the present invention.
[0037] Description of reference numerals:
[0038] 1—square slab; 3—profile stamping equipment; 3-1—upper workbench; 3-2—lower workbench; 6—L-shaped profile section; 9—profile straightening equipment; 9-1—movable slide; 9-2—power propulsion assembly; 9-4—fixed end clamping assembly; 10—L-shaped profile lower die; 10-1—L-shaped profile lower die boss end face; 10-2—L-shaped profile lower die end face; 10-3—L-shaped profile lower die end face R angle; 10-4—L-shaped profile lower die groove side face; 10-5—L-shaped profile lower die groove bottom face; 11—L-shaped profile impact upper die; 11-1—L-shaped profile upper die R angle; 12—L-shaped profile inner R angle; 13—L-shaped profile. DETAILED DESCRIPTION
[0039] like Figure 1 A method for forming a titanium and titanium alloy L-shaped profile is shown, the method comprising the following steps:
[0040] Step 1: Making a square slab: According to the target L-shaped profile, a titanium sheet or a titanium alloy sheet is selected and cut to obtain a square slab 1;
[0041] Step 2: Heat treatment of square slab: heat treatment of the square slab 1 is performed using a profile heating device;
[0042] Step 3: stamping to produce an L-shaped profile: installing an L-shaped profile mold on a profile stamping device 3, and using the profile stamping device 3 to set a pressing speed and a set pressing force to stamp the heat-treated square slab 1 to obtain an L-shaped profile 13;
[0043] Wherein, the L-shaped profile mold comprises an L-shaped profile lower mold 10 having an L-shaped groove and an L-shaped profile impact upper mold 11 matching the L-shaped profile lower mold 10;
[0044] Step 4: vacuum annealing of profile: vacuum annealing the L-shaped profile 13;
[0045] Step 5: Profile thermal correction: Use profile straightening equipment 9 to perform thermal correction on the L-shaped profile 13 after vacuum annealing;
[0046] Step 6: Profile surface treatment: Surface treatment is performed on the L-shaped profile 13 after heat calibration to obtain a finished L-shaped profile 13 .
[0047] In actual use, when cutting the sheet material, a water jet cutting method is adopted to obtain a square sheet blank 1 .
[0048] It should be noted that by using the profile stamping equipment 3 to hot stamp the square plate blank 1 after heat treatment to obtain the L-shaped profile 13, the uniformity of the formed structure of the titanium and titanium alloy profiles can be effectively improved. The operation is simple, there is no weld, the dimensional accuracy is high, and the appearance quality of the titanium and titanium alloy profiles is improved. At the same time, defects such as cracks are eliminated, the forming accuracy is improved, the product quality of the titanium and titanium alloy profiles is improved, the forming cycle is shortened, and the mechanical properties of the profile are improved.
[0049] In addition, the stamping method can be used for continuous production with a simple process. The preparation method has a high utilization rate of raw materials and can also significantly save energy, reduce processing costs, and improve production efficiency.
[0050] It should be noted that the stamping forming method can effectively improve the quality and yield rate of L-shaped profiles, and greatly reduce the production cost of the entire equipment during the manufacturing process of the whole product, significantly improving the economic benefits; it is easy to obtain L-shaped profiles with a wall thickness greater than 2mm, and the mechanical properties and chemical composition of the L-shaped profiles can meet the relevant standard requirements, effectively solving the problems of high weight requirements, thin wall thickness and high forming difficulty in the aerospace, weapons and other industries.
[0051] In particular, during hot stamping, by controlling the hot stamping temperature and pressure and applying high-temperature resistant and anti-oxidation coatings, the pressure is effectively reduced, excessive thinning of the L-shaped profile is avoided, and the uniformity of deformation is improved, which is conducive to the smooth forming of the L-shaped profile.
[0052] During specific implementation, in step three, the pressing speed is preferably set to 30 mm / s, and the pressing force is set to the equipment power, preferably 10 MPa.
[0053] In this embodiment, in step 2, before heat treating the square slab 1 , a high temperature resistant and anti-oxidation coating is coated on the surface of the square slab 1 .
[0054] In actual use, before coating the surface of the square slab 1 with the high temperature resistant anti-oxidation coating, firstly clean the oil stains and debris on the surface of the square slab 1, and the thickness of the high temperature resistant anti-oxidation coating is 0.2mm-1.0mm.
[0055] It should be noted that by coating the surface of the square slab 1 with a high temperature resistant and anti-oxidation coating, oxidation during hot stamping is effectively prevented, the problem of scratches or tears on the outer surface of the square slab 1 during stamping is solved, and the quality of the L-shaped profile is improved.
[0056] In this embodiment, in step 2, the profile heating equipment is a heating furnace. When the square slab 1 is heat treated, the heat treatment temperature is 80°C to 120°C lower than the phase change point temperature of the sheet material used for the square slab 1, and at this heat treatment temperature, the square slab 1 is heated in the heating furnace for 2h to 3h.
[0057] like Figure 2 As shown, in this embodiment, the profile stamping equipment 3 includes an upper workbench 3-1 and a lower workbench 3-2 capable of relative movement, the L-shaped profile lower die 10 is installed on the lower workbench 3-2, and the L-shaped profile impact upper die 11 is installed on the upper workbench 3-1.
[0058] like Figure 5 As shown, in this embodiment, the inner mold surface of the L-shaped profile lower mold 10 includes an L-shaped profile lower mold boss end surface 10-1, an L-shaped profile lower mold end surface 10-2, an L-shaped profile lower mold end surface R angle 10-3, an L-shaped profile lower mold groove side surface 10-4 and an L-shaped profile lower mold groove bottom surface 10-5, which are arranged in sequence from top to bottom, and the L-shaped profile lower mold groove bottom surface 10-5 is a concave arc surface;
[0059] like Figure 6 As shown, the bottom of the L-shaped profile impact upper die 11 is provided with an L-shaped profile upper die R angle 11-1 matching the bottom surface 10-5 of the L-shaped profile lower die groove, and the L-shaped profile upper die R angle 11-1 is the same size as the L-shaped profile inner R angle 12.
[0060] In actual use, the number of the L-shaped profile lower die boss end face 10-1, the L-shaped profile lower die end face 10-2, the L-shaped profile lower die end face R angle 10-3 and the L-shaped profile lower die groove side face 10-4 are all two, and the width of the square slab 1 is smaller than the width between the two L-shaped profile lower die boss end faces 10-1.
[0061] During specific implementation, the two L-shaped profile lower die groove side surfaces 10 - 4 are perpendicular to each other, and the two L-shaped profile lower die groove side surfaces 10 - 4 are connected to the L-shaped profile lower die groove bottom surface 10 - 5 to form an L-shaped groove.
[0062] like Figure 3 and Figure 4 As shown, in this embodiment, when the square slab 1 after heat treatment is hot stamped by the profile stamping equipment 3, the square slab 1 is placed on the end face 10-2 of the lower die of the L-shaped profile, and the profile stamping equipment 3 is started, so that the upper workbench 3-1 drives the L-shaped profile to impact the upper die 11 to hot stamp the square slab 1, until the bottom of the square slab 1 is stamped to the bottom face 10-5 of the groove of the lower die of the L-shaped profile, thereby obtaining the L-shaped profile 13.
[0063] In this embodiment, in step 4, the temperature of vacuum annealing is 500° C. to 800° C., and the holding time of vacuum annealing is 1 h to 2 h.
[0064] In this embodiment, in step 5, before heat-calibrating the L-shaped profile 13, the profile is first heat-treated according to the method in step 2;
[0065] like Figure 7 As shown, when the L-shaped profile 13 is subjected to thermal profiling, one end of the L-shaped profile 13 is clamped by the fixed end clamping assembly 9-4 of the profile straightening device 9, and the other end of the profile is clamped by the movable slide 9-1 and the power propulsion assembly 9-2 of the profile straightening device 9. When the movable slide 9-1 slides, it drives the other end of the L-shaped profile 13 to move for straightening.
[0066] In actual use, after the heat treatment of the L-shaped profile 13 is completed, it is quickly hoisted to the profile straightening device 9 for heat correction.
[0067] During specific implementation, a heating device is further provided between the fixed end clamping assembly 9 - 4 and the movable slide 9 - 1 , and the middle portion of the L-shaped profile 13 is passed through the heating device, thereby enabling thermal calibration.
[0068] It should be noted that when straightening is performed, the movable slide 9-1 and the power propulsion assembly 9-2 clamp the other end of the L-shaped profile 13, and the movable slide 9-1 and the power propulsion assembly 9-2 drive the other end of the L-shaped profile 13 to move, so that the L-shaped profile 13 is stretched, thereby straightening the L-shaped profile 13 in the length direction.
[0069] In specific implementation, before straightening the L-shaped profile 13, when clamping the two ends of the L-shaped profile 13, a supporting block matching it is set at both ends of the L-shaped profile 13 to prevent the two ends of the L-shaped profile 13 from being deformed under the action of the fixed end clamping assembly 9-4 or the power propulsion assembly 9-2.
[0070] In this embodiment, in step six, when the profile is subjected to surface treatment, the surface of the profile is sequentially subjected to shot blasting, degreasing, water washing and drying.
[0071] In specific implementation, the dimensions of the L-shaped profile 13, thickness × cross-sectional length × cross-sectional width, are generally 3 × 50 × 50 mm, 4 × 60 × 60 mm or 5 × 80 × 80 mm; the widths of the square slabs 1 corresponding to the three dimensions are 100 mm, 120 mm and 160 mm respectively.
[0072] When the size of the L-shaped profile is 3×50×50mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 500°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly hoisted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 4 is preferably 500°C, and the insulation time of the vacuum annealing is preferably 2h; in step 5, before the L-shaped profile 13 is heat-corrected, the L-shaped profile 13 is placed in a heating furnace and heated at 500°C for 2h for heat treatment;
[0073] When the size of the L-shaped profile is 4×60×60mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 700°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly hoisted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 4 is preferably 700°C, and the insulation time of the vacuum annealing is preferably 2h; in step 5, before the L-shaped profile 13 is heat-corrected, the L-shaped profile 13 is placed in a heating furnace and heated at 550°C for 2h for heat treatment;
[0074] When the size of the L-shaped profile is 5×80×80mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 800°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly lifted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 4 is preferably 600°C, and the insulation time of the vacuum annealing is preferably 2h; in step 5, before hot-calibrating the L-shaped profile 13, the L-shaped profile 13 is placed in a heating furnace and heated at 800°C for 2h for heat treatment.
[0075] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for forming titanium and titanium alloy L-shaped profiles, characterized in that: The method comprises the following steps: Step 1: Making a square slab: According to the target L-shaped profile, a titanium sheet or a titanium alloy sheet is selected and cut to obtain a square slab (1); Step 2: Heat treatment of square slab: heat treatment of the square slab (1) is performed using a profile heating device; Step 3: Stamping to produce an L-shaped profile: Installing an L-shaped profile mold on a profile stamping device (3), and using the profile stamping device (3) to stamp the heat-treated square slab (1) at a set pressing speed and a set pressing force to obtain an L-shaped profile (13); Wherein, the L-shaped profile mold comprises an L-shaped profile lower mold (10) having an L-shaped groove and an L-shaped profile impact upper mold (11) matching the L-shaped profile lower mold (10); Step 4: vacuum annealing of the profile: vacuum annealing the L-shaped profile (13); Step 5: Thermal alignment of the profile: thermally aligning the L-shaped profile (13) after vacuum annealing using a profile alignment device (9); Step 6, profile surface treatment: Surface treatment is performed on the L-shaped profile (13) after thermal correction to obtain a finished L-shaped profile (13).
2. A method for forming titanium and titanium alloy L-shaped profiles according to claim 1, characterized in that: In step 2, before heat treating the square slab (1), an anti-oxidation coating is applied to the surface of the square slab (1).
3. A method for forming titanium and titanium alloy L-shaped profiles according to claim 1, characterized in that: In step 2, the profile heating equipment is a heating furnace. When the square slab (1) is heat-treated, the heat treatment temperature is 80°C to 120°C lower than the phase transition point of the square slab (1), and at this heat treatment temperature, the square slab (1) is heated in the heating furnace for 2h to 3h.
4. A method for forming titanium and titanium alloy L-shaped profiles according to claim 1, characterized in that: The profile stamping equipment (3) comprises an upper workbench (3-1) and a lower workbench (3-2) capable of relative movement, the L-shaped profile lower die (10) being mounted on the lower workbench (3-2), and the L-shaped profile impact upper die (11) being mounted on the upper workbench (3-1).
5. A method for forming titanium and titanium alloy L-shaped profiles according to claim 4, characterized in that: The inner die surface of the L-shaped profile lower die (10) comprises an L-shaped profile lower die boss end surface (10-1), an L-shaped profile lower die end surface (10-2), an L-shaped profile lower die end surface R angle (10-3), an L-shaped profile lower die groove side surface (10-4) and an L-shaped profile lower die groove bottom surface (10-5) which are sequentially arranged from top to bottom, and the L-shaped profile lower die groove bottom surface (10-5) is a concave arc surface; The bottom of the L-shaped profile impact upper die (11) is provided with an L-shaped profile upper die R angle (11-1) that matches the bottom surface (10-5) of the L-shaped profile lower die groove, and the L-shaped profile upper die R angle (11-1) has the same size as the L-shaped profile inner R angle (12).
6. A method for forming titanium and titanium alloy L-shaped profiles according to claim 5, characterized in that: When hot stamping a square slab (1) after heat treatment is performed using a profile stamping device (3), the square slab (1) is placed on the end surface (10-2) of the lower die of the L-shaped profile, and the profile stamping device (3) is started, so that the upper workbench (3-1) drives the L-shaped profile to impact the upper die (11) to perform hot stamping on the square slab (1) until the bottom of the square slab (1) is stamped to the bottom surface (10-5) of the groove of the lower die of the L-shaped profile, thereby obtaining an L-shaped profile (13).
7. A method for forming titanium and titanium alloy L-shaped profiles according to claim 1, characterized in that: In step 4, the temperature of vacuum annealing is 500° C. to 800° C., and the holding time of vacuum annealing is 1 hour to 2 hours.
8. The method for forming a titanium and titanium alloy L-shaped profile according to claim 1, characterized in that: In step 5, before heat-calibrating the L-shaped profile (13), the profile is first heat-treated according to the method in step 2; When the L-shaped profile (13) is subjected to thermal correction, one end of the L-shaped profile (13) is clamped by the fixed end clamping assembly (9-4) of the profile straightening device (9), and the other end of the profile is clamped by the movable slide (9-1) and the power propulsion assembly (9-2) of the profile straightening device (9), and the other end of the L-shaped profile (13) is driven to move for correction.
9. A method for forming titanium and titanium alloy L-shaped profiles according to claim 1, characterized in that: In step six, when the profile is subjected to surface treatment, the surface of the profile is sequentially subjected to shot blasting, degreasing, water washing and drying.
Citation Information
Patent Citations
Technology for preparing pressure resisting titanium alloy half ball for bathyscaph manned ball
CN104923603A
Manufacturing method for zirconium alloy element box
CN106623487A
Titanium alloy U-shaped thin-wall profile and preparation method thereof
CN112496072A
Big V font panel beating stamping die
CN208050739U
Section bar clamping and straightening device
CN216606736U
Cited By
Straightening structure and straightening method for titanium and titanium alloy profiles with special-shaped sections
CN121669754A
Preparation method of high-performance titanium alloy angle profile
CN122787305A