Titanium and titanium alloy U-shaped profile forming method
Through the stamping forming method, the problem of defects such as bending and twisting of titanium and titanium alloy profiles during the extrusion forming process is solved, and high-quality and efficient production of products is achieved, which is suitable for the needs of aerospace and other industries.
Patent Information
- Application Number
- CN202411010067.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-08
AI Technical Summary
Titanium and titanium alloy profiles are prone to defects such as bending and twisting during the extrusion forming process, resulting in unstable product quality. The lack of standardized production technology and quality inspection affects the development of aerospace and other industries.
The stamping forming method is adopted, including making square slabs, heat treatment, stamping forming, vacuum annealing, heat calibration and surface treatment. Through the design of U-shaped profile mold and impact upper mold, the heat treatment and vacuum annealing conditions are controlled to ensure the uniformity and uniformity of forming. Accuracy.
It improves the structural uniformity and appearance quality of titanium and titanium alloy U-shaped profiles, eliminates defects such as cracks, shortens the molding cycle, improves mechanical properties and product quality, and is suitable for small and medium-sized batch production of various specifications.
Smart Images

Figure CN118744191A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of profile production, and in particular relates to a method for forming titanium and titanium alloy U-shaped profiles. Background Art
[0002] Titanium and titanium alloy profiles are important aircraft structural materials and are widely used in wings, wall panels, bulkheads, etc. Since titanium has a close-packed hexagonal crystal structure at room temperature, it has high strength and is difficult to deform, so the extrusion process of titanium and titanium alloy profiles must be carried out under high temperature conditions. When extruding titanium and titanium alloy profiles, the metal flow differences at different parts of the profile cross section are large, which eventually causes the profile to have defects such as bending and twisting. The twisting or bending of titanium and titanium alloy profiles after extrusion is a problem that cannot be completely avoided, especially in thin-walled asymmetric cross-section titanium and titanium alloy profiles.
[0003] Traditional titanium and titanium alloy extruded profiles have very broad application prospects in aerospace and other fields, but the extrusion process is extremely difficult due to problems such as sticking or distortion. At present, although some production technologies of titanium and titanium alloy profiles have been mastered, the production specifications of titanium and titanium alloy profiles have not yet been formed. The long-term lack of standardized technical requirements and consistent quality inspections has resulted in uneven product quality of titanium and titanium alloy profiles and a lack of competitiveness in the application market.
[0004] Therefore, it is necessary to propose a titanium and titanium alloy U-shaped profile forming method that can effectively improve the quality of titanium and titanium alloy profile products and promote the development of aerospace, weapons and other industries. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a titanium and titanium alloy U-shaped profile forming method in view of the deficiencies in the above-mentioned prior art. The stamping forming method can improve the uniformity of the formed structure of the titanium and titanium alloy U-shaped profile, and the operation is simple, there is no weld, the dimensional accuracy is high, and the appearance quality of the titanium and titanium alloy profile is improved. At the same time, defects such as cracks are eliminated, the forming accuracy is improved, the product quality of the titanium and titanium alloy profile is improved, the forming cycle is shortened, and the mechanical properties of the profile are improved.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for forming a titanium and titanium alloy U-shaped profile, characterized in that the method comprises the following steps:
[0007] Step 1: Making square slabs: According to the target product U-shaped profile, titanium sheet or titanium alloy sheet is selected and cut to obtain square slabs;
[0008] Step 2: Heat treatment of the square slab: heat treatment of the square slab is performed using a profile heating device;
[0009] Step 3: stamping to produce a U-shaped profile: installing a U-shaped profile mold on a profile stamping device, using the profile stamping device to set a pressing speed and a set pressing force to stamp the heat-treated square slab to obtain a U-shaped profile;
[0010] Wherein, the U-shaped profile mold comprises a U-shaped profile lower mold with a U-shaped groove and a U-shaped profile impact upper mold matching the U-shaped profile lower mold;
[0011] Step 4: Vacuum annealing of profile: vacuum annealing of the U-shaped profile;
[0012] Step 5: Profile thermal correction: Use profile straightening equipment to perform thermal correction on the U-shaped profile after vacuum annealing;
[0013] Step 6: Profile surface treatment: Surface treatment is performed on the U-shaped profile after heat correction to obtain a finished U-shaped profile.
[0014] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: in step 2, before heat treating the square slab, an anti-oxidation coating is coated on the surface of the square slab.
[0015] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: in step two, the profile heating equipment is a heating furnace, and when the square slab is heat treated, the heat treatment temperature is lower than the phase change point of the square slab by 80°C to 120°C, and at the heat treatment temperature, the square slab is heated in the heating furnace for 2h to 3h.
[0016] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: the profile stamping equipment includes an upper workbench and a lower workbench capable of relative movement, the U-shaped profile lower die is installed on the lower workbench, and the U-shaped profile impact upper die is installed on the upper workbench.
[0017] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: the inner mold surface of the U-shaped profile lower mold includes the U-shaped profile lower mold boss end face, the U-shaped profile lower mold end face, the U-shaped profile lower mold groove side face and the U-shaped profile lower mold groove bottom face which are arranged in sequence from top to bottom, and the U-shaped profile lower mold end face R angle is arranged between the U-shaped profile lower mold end face and the U-shaped profile lower mold groove side face, and the U-shaped profile lower mold groove R angle is arranged between the U-shaped profile lower mold groove side face and the U-shaped profile lower mold groove bottom face;
[0018] The bottoms on both sides of the U-shaped profile impact upper die are both provided with U-shaped profile upper die R angles matching the R angles of the U-shaped profile lower die grooves, and the U-shaped profile upper die R angle has the same size as the U-shaped profile inner R angle.
[0019] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: when using profile stamping equipment to hot stamp the heat-treated square slab, the square slab is placed on the end face of the lower die of the U-shaped profile, and the profile stamping equipment is started, so that the upper workbench drives the U-shaped profile to impact the upper die to hot stamp the square slab until the bottom of the square slab is stamped to the bottom surface of the groove of the lower die of the U-shaped profile to obtain a U-shaped profile.
[0020] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: in step four, the vacuum annealing temperature is 500°C to 800°C, and the vacuum annealing holding time is 1h to 2h.
[0021] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: in step 5, before the U-shaped profile is heat-treated according to the method in step 2;
[0022] When the U-shaped profile is thermally corrected, one end of the U-shaped profile is clamped and fixed by the fixed end clamping assembly of the profile straightening equipment, and the other end of the U-shaped profile is clamped by the moving slide, power propulsion assembly and moving end transverse clamping mechanism of the profile straightening equipment. When the moving slide slides, the other end of the U-shaped profile is driven to move for straightening.
[0023] The above-mentioned titanium and titanium alloy U-shaped profile forming method is characterized in that: in step six, when the profile is subjected to surface treatment, the surface of the profile is shot peened, degreased, washed with water and dried in sequence.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1. The present invention breaks the traditional method of extrusion molding of titanium and titanium alloy profiles and proposes a new preparation method. The above method can improve the uniformity of the formed structure of the titanium and titanium alloy profiles, is simple to operate, has no welds, has high dimensional accuracy, and improves the appearance quality of the titanium and titanium alloy profiles. At the same time, defects such as cracks are eliminated, the molding accuracy is improved, the product quality of the titanium and titanium alloy profiles is improved, the molding cycle is shortened, and the mechanical properties of the profiles are improved.
[0026] 2. The present invention adopts a stamping forming method to obtain a U-shaped profile with a wall thickness greater than 2 mm, which can be produced continuously, has a simple process, and the preparation method has a high utilization rate of raw materials, can also greatly save energy and reduce processing costs, and improve production efficiency.
[0027] 3. The process of the present invention is simple, easy to operate, has low investment cost, and has a wide range of applications. It is particularly suitable for making small and medium batches of U-shaped profiles of various specifications, and has broad prospects for promotion and application.
[0028] In summary, the stamping forming method used in the present invention can improve the uniformity of the formed structure of the titanium and titanium alloy U-shaped profiles, is simple to operate, has no welds, has high dimensional accuracy, and improves the appearance quality of the titanium and titanium alloy profiles. At the same time, defects such as cracks are eliminated, the forming accuracy is improved, the product quality of the titanium and titanium alloy profiles is improved, the forming cycle is shortened, and the mechanical properties of the profiles are improved.
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a flowchart of the present invention.
[0031] Figure 2 It is a schematic structural diagram of the profile stamping equipment of the present invention.
[0032] Figure 3 It is a structural schematic diagram of the lower die of the U-shaped profile of the present invention.
[0033] Figure 4 It is a schematic diagram of the positional relationship between the square slab, the U-shaped profile lower die and the U-shaped profile impact upper die during hot stamping of the present invention.
[0034] Figure 5 It is a schematic diagram of the positional relationship between the U-shaped profile after hot stamping, the U-shaped profile lower die and the U-shaped profile impact upper die of the present invention.
[0035] Figure 6 It is a structural schematic diagram of the U-shaped profile of the present invention.
[0036] Figure 7 It is a structural schematic diagram of the profile straightening device of the present invention.
[0037] Description of reference numerals:
[0038] 1—square slab; 2—U-shaped profile; 3—profile stamping equipment; 3-1—upper workbench; 3-2—lower workbench; 4—U-shaped profile lower die; 4-1—U-shaped profile lower die boss end face; 4-2—U-shaped profile lower die end face; 4-3—U-shaped profile lower die end face R angle; 4-4—U-shaped profile lower die groove side face; 4-5—U-shaped profile lower die groove R angle; 4-6—U-shaped profile lower die groove bottom face; 5—U-shaped profile impact upper die; 5-1—U-shaped profile upper die R angle; 6—U-shaped profile section; 7—U-shaped profile inner R angle; 8—U-shaped profile outer R angle; 9—profile straightening equipment; 9-1—movable slide; 9-2—power propulsion assembly; 9-3—movable end lateral clamping mechanism; 9-4—fixed end clamping assembly. DETAILED DESCRIPTION
[0039] like Figures 1 to 7A titanium and titanium alloy U-shaped profile forming method is shown, the method comprising the following steps:
[0040] Step 1: Making a square slab: According to the target product U-shaped profile, a titanium sheet or a titanium alloy sheet is selected and cut to obtain a square slab 1;
[0041] Step 2: Heat treatment of square slab: heat treatment of the square slab 1 is performed using a profile heating device;
[0042] Step 3: stamping to produce a U-shaped profile: installing a U-shaped profile mold on a profile stamping device 3, and using the profile stamping device 3 to set a pressing speed and a set pressing force to stamp the heat-treated square slab 1 to obtain a U-shaped profile 2;
[0043] The U-shaped profile mold includes a U-shaped profile lower mold 4 having a U-shaped groove and a U-shaped profile impact upper mold 5 matching the U-shaped profile lower mold 4;
[0044] Step 4: Vacuum annealing of profile: vacuum annealing the U-shaped profile 2;
[0045] Step 5: Profile thermal correction: Use profile straightening equipment 9 to perform thermal correction on the U-shaped profile 2 after vacuum annealing;
[0046] Step 6: Profile surface treatment: Surface treatment is performed on the U-shaped profile 2 after heat correction to obtain a finished U-shaped profile 2.
[0047] In actual use, when cutting the sheet material, a water jet cutting method is adopted to obtain a square sheet blank 1 .
[0048] It should be noted that by using the profile stamping equipment 3 to hot stamp the square plate blank 1 after heat treatment to obtain the U-shaped profile 2, the uniformity of the formed structure of the titanium and titanium alloy profiles can be effectively improved. The operation is simple, there is no weld, the dimensional accuracy is high, and the appearance quality of the titanium and titanium alloy profiles is improved. At the same time, defects such as cracks are eliminated, the forming accuracy is improved, the product quality of the titanium and titanium alloy profiles is improved, the forming cycle is shortened, and the mechanical properties of the profile are improved.
[0049] In addition, the stamping method can be used for continuous production with a simple process. The preparation method has a high utilization rate of raw materials and can also significantly save energy, reduce processing costs, and improve production efficiency.
[0050] It should be noted that the stamping forming method has effectively improved the quality and yield rate of U-shaped profiles, and greatly reduced the production cost of the entire equipment during the manufacturing process of the entire product, significantly improving the economic benefits; it is easy to obtain U-shaped profiles with a wall thickness greater than 2 mm, and the mechanical properties and chemical composition of the U-shaped profiles can meet the relevant standard requirements, effectively solving the problems of high weight requirements, thin wall thickness and great forming difficulty in the aerospace, weapons and other industries.
[0051] In particular, during hot stamping, by controlling the hot stamping temperature and pressure and applying high-temperature resistant and anti-oxidation coatings, the pressure is effectively reduced, excessive thinning of the U-shaped profile is avoided, and the uniformity of deformation is improved, which is conducive to the smooth forming of the U-shaped profile.
[0052] During specific implementation, in step three, the pressing speed is preferably set to 30 mm / s, and the pressing force is set to the equipment power, preferably 10 MPa.
[0053] In this embodiment, in step 2, before heat treating the square slab 1 , a high temperature resistant and anti-oxidation coating is coated on the surface of the square slab 1 .
[0054] In actual use, before coating the surface of the square slab 1 with the high temperature resistant anti-oxidation coating, firstly clean the oil stains and debris on the surface of the square slab 1, and the thickness of the high temperature resistant anti-oxidation coating is 0.2mm-1.0mm.
[0055] It should be noted that by coating the surface of the square slab 1 with a high temperature resistant and anti-oxidation coating, oxidation during hot stamping is effectively prevented, the problem of scratches or tears on the outer surface of the square slab 1 during stamping is solved, and the quality of the U-shaped profile is improved.
[0056] In this embodiment, in step 2, the profile heating equipment is a heating furnace. When the square slab 1 is heat treated, the heat treatment temperature is 80°C to 120°C lower than the phase change point temperature of the sheet material used for the square slab 1, and at this heat treatment temperature, the square slab 1 is heated in the heating furnace for 2h to 3h.
[0057] In this embodiment, the profile stamping equipment 3 includes an upper workbench 3-1 and a lower workbench 3-2 capable of relative movement, the U-shaped profile lower die 4 is installed on the lower workbench 3-2, and the U-shaped profile impact upper die 5 is installed on the upper workbench 3-1.
[0058] like Figure 3 , Figure 4 and Figure 6As shown, in this embodiment, the inner mold surface of the U-shaped profile lower mold 4 includes a U-shaped profile lower mold boss end face 4-1, a U-shaped profile lower mold end face 4-2, a U-shaped profile lower mold groove side face 4-4 and a U-shaped profile lower mold groove bottom face 4-6 which are arranged in sequence from top to bottom, a U-shaped profile lower mold end face R angle 4-3 is arranged between the U-shaped profile lower mold end face 4-2 and the U-shaped profile lower mold groove side face 4-4, and a U-shaped profile lower mold groove R angle 4-5 is arranged between the U-shaped profile lower mold groove side face 4-4 and the U-shaped profile lower mold groove bottom face 4-6;
[0059] The bottom of both sides of the U-shaped profile impact upper die 5 are provided with a U-shaped profile upper die R angle 5-1 matching the U-shaped profile lower die groove R angle 4-5, and the U-shaped profile upper die R angle 5-1 is the same size as the U-shaped profile inner R angle 7; the U-shaped profile lower die groove R angle 4-5 is the same size as the U-shaped profile outer R angle 8.
[0060] In actual use, the number of the U-shaped profile lower die boss end face 4-1, the U-shaped profile lower die end face 4-2, the U-shaped profile lower die end face R angle 4-3, the U-shaped profile lower die groove side face 4-4 and the U-shaped profile lower die groove R angle 4-5 are all two.
[0061] In specific implementation, the U-shaped profile lower die boss end face 4-1 is perpendicular to the U-shaped profile lower die end face 4-2, the U-shaped profile lower die groove side face 4-4 is parallel to the U-shaped profile lower die boss end face 4-1, and the U-shaped profile lower die groove bottom face 4-6 is parallel to the U-shaped profile lower die end face 4-2.
[0062] like Figure 2 , Figure 4 and Figure 5 As shown, in this embodiment, when the square slab 1 after heat treatment is hot stamped by the profile stamping equipment 3, the square slab 1 is placed on the end face 4-2 of the lower die of the U-shaped profile, and the profile stamping equipment 3 is started, so that the upper workbench 3-1 drives the U-shaped profile to impact the upper die 5 to hot stamp the square slab 1, until the bottom of the square slab 1 is stamped to the bottom face 4-6 of the groove of the lower die of the U-shaped profile, thereby obtaining the U-shaped profile 2.
[0063] In this embodiment, in step 4, the temperature of vacuum annealing is 500° C. to 800° C., and the holding time of vacuum annealing is 1 h to 2 h.
[0064] In this embodiment, in step 5, before heat-correcting the U-shaped profile 2, the profile is first heat-treated according to the method in step 2;
[0065] like Figure 7As shown, when the U-shaped profile 2 is subjected to thermal profiling, one end of the U-shaped profile 2 is clamped and fixed by the fixed end clamping assembly 9-4 of the profile straightening equipment 9, and at the same time, the other end of the U-shaped profile 2 is clamped by the movable slide 9-1, the power propulsion assembly 9-2 and the movable end transverse clamping mechanism 9-3 of the profile straightening equipment 9. When the movable slide 9-1 slides, it drives the other end of the U-shaped profile 2 to move for straightening.
[0066] In actual use, after the U-shaped profile 2 is heat-treated, it is quickly hoisted to the profile straightening device 9 for heat correction.
[0067] During specific implementation, a heating device is further provided between the fixed end clamping assembly 9 - 4 and the movable slide 9 - 1 , and the middle portion of the U-shaped profile 2 is passed through the heating device, thereby enabling thermal calibration.
[0068] It should be noted that when straightening is performed, the power propulsion assembly 9-2 is pressed downward so that it cooperates with the movable slide 9-1 to vertically clamp the U-shaped profile 2, and the mobile end transverse clamping mechanism 9-3 clamps the U-shaped profile 2 laterally, so that the movable slide 9-1, the power propulsion assembly 9-2 and the mobile end transverse clamping mechanism 9-3 can slide synchronously, driving the other end of the U-shaped profile 2 to move, so that the U-shaped profile 2 is stretched, thereby straightening the U-shaped profile 2 in the length direction.
[0069] In specific implementation, before straightening the U-shaped profile 2, when clamping the two ends of the U-shaped profile 2, a support block matching its shape is inserted at both ends of the U-shaped profile 2 to prevent the two ends of the U-shaped profile 2 from deforming during clamping.
[0070] In this embodiment, in step six, when the profile is subjected to surface treatment, the surface of the profile is sequentially subjected to shot blasting, degreasing, water washing and drying.
[0071] In specific implementation, the dimensions of the U-shaped profile thickness × cross-sectional length × cross-sectional width are generally 3×60×60mm, 4×80×80mm or 5×100×100mm; the widths of the square slabs 1 corresponding to the three dimensions are 120mm, 160mm and 200mm respectively.
[0072] When the size of the U-shaped profile is 3×60×60mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 500°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly lifted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 4 is preferably 500°C, and the insulation time of the vacuum annealing is preferably 2h; in step 5, before the U-shaped profile 2 is heat-corrected, the U-shaped profile 2 is placed in a heating furnace and heated at 500°C for 2h for heat treatment;
[0073] When the size of the U-shaped profile is 4×80×80mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 700°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly hoisted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 4 is preferably 700°C, and the insulation time of the vacuum annealing is preferably 2h; in step 5, before the U-shaped profile 2 is heat-corrected, the U-shaped profile 2 is placed in a heating furnace and heated at 550°C for 2h for heat treatment;
[0074] When the size of the U-shaped profile is 5×100×100mm, in step 2, the temperature of the heat treatment of the square slab 1 is preferably 800°C, and the heating time is preferably 3h. After the heat treatment of the square slab 1 is completed, the square slab 1 is quickly lifted to the profile stamping equipment 3 for hot stamping; the temperature of the vacuum annealing in step 4 is preferably 600°C, and the insulation time of the vacuum annealing is preferably 2h; in step 5, before the U-shaped profile 2 is hot-calibrated, the U-shaped profile 2 is placed in a heating furnace and heated at 800°C for 2h for heat treatment.
[0075] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for forming titanium and titanium alloy U-shaped profiles, characterized in that: The method comprises the following steps: Step 1: Making a square slab: According to the target product U-shaped profile, a titanium sheet or a titanium alloy sheet is selected and cut to obtain a square slab (1); Step 2: Heat treatment of square slab: heat treatment of the square slab (1) is performed using a profile heating device; Step 3: stamping a U-shaped profile: installing a U-shaped profile mold on a profile stamping device (3), and using the profile stamping device (3) to stamp the heat-treated square slab (1) at a set pressing speed and a set pressing force to obtain a U-shaped profile (2); The U-shaped profile mold comprises a U-shaped profile lower mold (4) having a U-shaped groove and a U-shaped profile impact upper mold (5) matching the U-shaped profile lower mold (4); Step 4: Vacuum annealing of the profile: vacuum annealing the U-shaped profile (2); Step 5: Profile thermal correction: Use profile straightening equipment (9) to perform thermal correction on the U-shaped profile (2) after vacuum annealing; Step 6: Profile surface treatment: Surface treatment is performed on the U-shaped profile (2) after heat correction to obtain a finished U-shaped profile (2).
2. A method for forming titanium and titanium alloy U-shaped profiles according to claim 1, characterized in that: In step 2, before heat treating the square slab (1), an anti-oxidation coating is applied to the surface of the square slab (1).
3. A method for forming titanium and titanium alloy U-shaped profiles according to claim 1, characterized in that: In step 2, the profile heating equipment is a heating furnace. When the square slab (1) is heat-treated, the heat treatment temperature is 80°C to 120°C lower than the phase transition point of the square slab (1), and at this heat treatment temperature, the square slab (1) is heated in the heating furnace for 2h to 3h.
4. A method for forming titanium and titanium alloy U-shaped profiles according to claim 1, characterized in that: The profile stamping equipment (3) comprises an upper workbench (3-1) and a lower workbench (3-2) capable of relative movement, the U-shaped profile lower die (4) is mounted on the lower workbench (3-2), and the U-shaped profile impact upper die (5) is mounted on the upper workbench (3-1).
5. A method for forming titanium and titanium alloy U-shaped profiles according to claim 4, characterized in that: The inner die surface of the U-shaped profile lower die (4) comprises a U-shaped profile lower die boss end surface (4-1), a U-shaped profile lower die end surface (4-2), a U-shaped profile lower die groove side surface (4-4) and a U-shaped profile lower die groove bottom surface (4-6) arranged in sequence from top to bottom; a U-shaped profile lower die end surface R angle (4-3) is provided between the U-shaped profile lower die end surface (4-2) and the U-shaped profile lower die groove side surface (4-4); and a U-shaped profile lower die groove R angle (4-5) is provided between the U-shaped profile lower die groove side surface (4-4) and the U-shaped profile lower die groove bottom surface (4-6); The bottoms on both sides of the U-shaped profile impact upper die (5) are both provided with U-shaped profile upper die R angles (5-1) that match the U-shaped profile lower die groove R angles (4-5), and the U-shaped profile upper die R angles (5-1) are the same size as the U-shaped profile inner R angles (7).
6. A method for forming titanium and titanium alloy U-shaped profiles according to claim 5, characterized in that: When hot stamping a square slab (1) after heat treatment is performed using a profile stamping device (3), the square slab (1) is placed on the end surface (4-2) of the lower die of the U-shaped profile, and the profile stamping device (3) is started, so that the upper workbench (3-1) drives the U-shaped profile to impact the upper die (5) to perform hot stamping on the square slab (1) until the bottom of the square slab (1) is stamped to the bottom surface (4-6) of the groove of the lower die of the U-shaped profile, thereby obtaining a U-shaped profile (2).
7. A method for forming titanium and titanium alloy U-shaped profiles according to claim 1, characterized in that: In step 4, the temperature of vacuum annealing is 500° C. to 800° C., and the holding time of vacuum annealing is 1 hour to 2 hours.
8. A method for forming titanium and titanium alloy U-shaped profiles according to claim 1, characterized in that: In step 5, before heat-calibrating the U-shaped profile (2), the profile is first heat-treated according to the method in step 2; When the U-shaped profile (2) is thermally corrected, one end of the U-shaped profile (2) is clamped and fixed by the fixed end clamping assembly (9-4) of the profile straightening device (9), and the other end of the U-shaped profile (2) is clamped by the movable slide (9-1), the power propulsion assembly (9-2) and the movable end transverse clamping mechanism (9-3) of the profile straightening device (9). When the movable slide (9-1) slides, the other end of the U-shaped profile (2) is driven to move and be straightened.
9. A method for forming titanium and titanium alloy U-shaped profiles according to claim 1, characterized in that: In step six, when the profile is subjected to surface treatment, the surface of the profile is sequentially subjected to shot blasting, degreasing, water washing and drying.
Citation Information
Patent Citations
Technology for preparing pressure resisting titanium alloy half ball for bathyscaph manned ball
CN104923603A
Titanium alloy sheet metal part cold-die hot-stamping forming tool and machining method
CN106513508A
Rapid heating cold-mold hot plate forming method for titanium alloy thin-walled component
CN110252899A
Forming method for titanium alloy thin-walled component and sizing device
CN112157157A
Titanium alloy U-shaped thin-wall profile and preparation method thereof
CN112496072A