Vinyl chloride-vinyl acetate resin modified polyurethane composite polishing pad and preparation method thereof

Through the alternating hard and soft segment structure and impregnation process of the chlorine-vinegar resin modified polyurethane wet resin, the wear resistance and porosity problems of the fine polishing pad in the chemical mechanical polishing process are solved, the removal rate and service life are improved, and the Wafer flatness and surface quality.

CN118744401AActive Publication Date: 2024-10-08HUANGPU INST OF MATERIALS

Patent Information

Application Number
CN202410888520.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-08
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Existing fine polishing pads have problems such as insufficient wear resistance, poor mechanical properties, uneven cells, low porosity, weak liquid carrying capacity and short service life in the chemical mechanical polishing process, resulting in insufficient wafer flatness and surface defects. High degree.

Method used

The polyurethane wet resin modified with chlorine-vinyl chloride resin is used to form a polyurethane structure with alternating hard and soft segments through prepolymerization, chain extension and grafting reactions. The side chain is chlorine-vinyl chloride-vinyl acetate-vinyl alcohol copolymerized chlorine-vinyl alcohol resin, which improves the number of average molecular weight and porosity, and replaces the PET film as a buffer layer through an impregnation process to simplify the preparation process.

Benefits of technology

It significantly improves the wear resistance, removal rate and service life of the polishing pad, improves porosity and liquid carrying capacity, solves the problems of uneven cells and surface defects, and improves the flatness and surface quality of the wafer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744401A_ABST
    Figure CN118744401A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of chemical mechanical planarization treatment, and discloses a vinyl chloride-vinyl acetate resin modified polyurethane composite polishing pad, which is prepared from the following components in parts by weight: 1000 to 2000 parts of color paste, 15 to 45 parts of nonionic surfactant, 15 to 45 parts of anionic surfactant, 500 to 1000 parts of diluting solvent, 300 to 330 parts of gum, 3000 to 4000 parts of vinyl chloride-vinyl acetate resin modified polyurethane wet resin and 170 to 200 parts of impregnating layer. According to the vinyl chloride-vinyl acetate resin modified polyurethane composite polishing pad, vinyl chloride-vinyl acetate resin modified polyurethane is adopted as wet resin, a main chain of the vinyl chloride-vinyl acetate resin modified polyurethane is of a polyurethane structure with alternate hard and soft segments, and a side chain of the vinyl chloride-vinyl acetate resin modified polyurethane composite polishing pad is of a vinyl chloride-vinyl acetate-vinyl alcohol copolymerized vinyl chloride-vinyl acetate resin structure. The chain segment structure of the vinyl chloride-vinyl acetate resin modified polyurethane wet-process resin is more diversified, the upper limit of the number-average molecular weight can be effectively improved, the wear resistance and the mechanical property of the vinyl chloride-vinyl acetate resin modified polyurethane wet-process resin are greatly improved, and the prepared polishing pad has the characteristics of good wear resistance, high porosity, high removal rate and long service life. The invention further discloses a preparation method of the vinyl chloride-vinyl acetate resin modified polyurethane composite polishing pad.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical mechanical planarization treatment, and in particular relates to a chlorovinyl resin modified polyurethane composite polishing pad and a preparation method thereof. Background Art

[0002] Chemical mechanical polishing (CMP) is a key process in the integrated circuit manufacturing process to achieve global uniform planarization of the wafer. CMP uses softer materials for polishing to achieve high-quality surface effects. It is currently the only technology that can take into account both global and local planarization of the surface.

[0003] Polishing pads used in CMP processes are roughly divided into hard rough polishing pads and soft fine polishing pads. In recent years, as the market demand for high-precision advanced process devices has become more urgent, the consumption of fine polishing pads in the CMP process has also increased. Due to the common disadvantages of domestic fine polishing pads, such as insufficient wear resistance, poor mechanical properties, uneven pores, low porosity, weak liquid carrying capacity and short service life, the wafers in the CMP process have problems such as low material removal rate, insufficient wafer flatness, and high surface defects. Therefore, most domestic wafer manufacturers mainly use imported fine polishing pads.

[0004] The prior art discloses a polishing pad, which is a linear structure polyurethane wet-process resin synthesized with diisocyanate and small molecule diol / amine as hard segments and polyester diol and polyether diol as soft segments. The upper limit of the number average molecular weight is low, the chain segment structure is single, and there is no hydrophilic group. Most of them have defects such as insufficient wear resistance and poor mechanical properties. The polishing pad prepared by the polishing pad generally has the disadvantages of uneven pores, low porosity, weak liquid carrying capacity, low polishing removal rate, and short service life. The prior art also discloses another polishing pad, which is a fine polishing pad prepared with a polyethylene terephthalate (PET) film as a buffer layer. The coating slurry needs to be coated on a release film for solidification, water washing, and drying, and then the coating layer is peeled off from the release film. Finally, the coating layer and the PET film are bonded and bonded with hot melt adhesive. The preparation process is relatively complicated, and the compression ratio and rebound rate of the prepared polishing pad are low, and the buffering effect is not good. In the CMP fine polishing process, it is very easy to cause poor wafer flatness and high surface defects. Summary of the invention

[0005] In order to solve the deficiencies of the prior art, the present invention provides a polyurethane composite polishing pad modified by chlorovinyl resin, which adopts a polyurethane wet resin modified by chlorovinyl resin, whose main chain is a polyurethane structure with alternating hard and soft segments, and whose side chain is a polyurethane structure of vinyl chloride-vinyl acetate-vinyl alcohol copolymer. The segment structure of the polyurethane wet resin modified by chlorovinyl resin is more diversified, which can effectively increase the upper limit of the number average molecular weight, greatly improve its wear resistance and mechanical properties, and the polishing pad prepared has the characteristics of good wear resistance, high porosity, high removal rate and long service life. The present invention also provides a preparation method of the polyurethane composite polishing pad modified by chlorovinyl resin.

[0006] The technical effects to be achieved by the present invention are achieved through the following technical aspects:

[0007] In a first aspect, the present invention provides a chlorovinyl resin modified polyurethane composite polishing pad, which is prepared from the following components in parts by weight:

[0008] 1000-2000 parts of color paste, 15-45 parts of nonionic surfactant, 15-45 parts of anionic surfactant, 500-1000 parts of diluent solvent, 300-330 parts of adhesive, 3000-4000 parts of chloroacetic resin modified polyurethane wet resin, and 170-200 parts of impregnation layer.

[0009] In some embodiments, the chlorovinyl resin modified polyurethane wet resin is prepared from the following components by weight: 40-60 parts of diisocyanate, 180-540 parts of polyether diol, 5-15 parts of aromatic diamine, 100-200 parts of chlorovinyl resin, 1-5 parts of chain terminator, and 605-2460 parts of solvent;

[0010] The chlorovinyl resin is a vinyl chloride-vinyl acetate-vinyl alcohol copolymer, the hydroxyl value of which is between 50 and 100 mgKOH / g, and the molecular weight is between 30,000 and 50,000.

[0011] In some embodiments, the diisocyanate includes at least one of toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, 4,4'-diphenylmethane diisocyanate, or 2,4'-diphenylmethane diisocyanate.

[0012] In some embodiments, the polyether diol is at least one of polytetramethylene glycol or polypropylene glycol; wherein the specification of the polytetramethylene glycol is PTMG-1000, PTMG-2000 or PTMG-3000, and the specification of the polypropylene glycol is PPG-1000, PPG-2000 or PPG-3000.

[0013] In some embodiments, the aromatic diamine includes at least one of 4,4'-diaminodiphenylmethane, 2,4'-diaminodiphenylmethane, 2,4-diaminotoluene, or 2,6-diaminotoluene;

[0014] The chain terminator is methanol, ethanol or isopropanol.

[0015] In some embodiments, the chlorovinyl chloride resin modified polyurethane wet process resin is prepared by the following method:

[0016] Prepolymerization reaction: dehydrating the polyether diol at 105-110° C. and negative pressure of 0.08-0.10 MPa for 1 hour, adding diisocyanate to carry out prepolymerization reaction at 80-90° C. for 2-3 hours to obtain an isocyanate-terminated prepolymer;

[0017] Chain extension reaction: adding solvent and aromatic diamine to the prepared prepolymer in sequence for chain extension, and maintaining the reaction temperature at 80-90°C for 2-3 hours until the system solution is polymerized to a molecular weight between 60,000 and 80,000;

[0018] Grafting reaction: adding chlorovinyl resin and maintaining 80-90°C for grafting reaction for 3-4 hours to chemically graft the chlorovinyl resin onto the polyurethane chain segment;

[0019] The reaction is terminated, and when the grafting reaction reaches a number average molecular weight Mn between 120,000 and 150,000, a chain terminator is added to terminate the reaction, and the material is discharged to obtain a vinyl chloride resin modified polyurethane wet process resin.

[0020] In some embodiments, the color paste is a carbon black paste or a titanium dioxide paste;

[0021] The nonionic surfactant is sorbitan monostearate or sorbitan monooleate;

[0022] The anionic surfactant is sodium docusate or sodium dodecylbenzene sulfonate;

[0023] The solvent is N,N-dimethylformamide, N-methylpyrrolidone or dimethyl sulfoxide;

[0024] The adhesive backing is a pressure-sensitive acrylic adhesive backing, and its model is 568HM2, 560PSD or 5628C, and its thickness is between 100 and 200 μm.

[0025] In some embodiments, the impregnation layer is prepared from the following components in parts by weight: 2000-3000 parts of chlorovinyl resin modified polyurethane wet resin, 4000-5000 parts of solvent, and 130-140 parts of non-woven fabric.

[0026] In some embodiments, in the impregnation layer, the viscosity of the impregnation slurry at 25° C. is 200 to 500 mPa·S, and the resin impregnation ratio is 30% to 35%;

[0027] The nonwoven fabric includes PET needle-punched nonwoven fabric or PET spunlace nonwoven fabric, and the thickness of the nonwoven fabric is between 0.8 and 1.0 mm, and the gram weight is between 130 and 140 g / m 2 between.

[0028] In some embodiments, the impregnation layer is prepared by the following method:

[0029] Add chlorovinyl resin modified polyurethane wet resin and solvent, disperse at a speed of 800-1000r / min for 1-2h until mixed evenly; then degas for 2-3h under vacuum conditions of negative pressure 0.08-0.10Mpa to obtain impregnation slurry; finally, mix and impregnate the non-woven fabric and the impregnation slurry evenly, put it into DMF aqueous solution for coagulation, wash with water, dry and shape, and obtain the impregnation layer.

[0030] In a second aspect, the present invention embodies a method for preparing a chlorovinyl acetate resin modified polyurethane composite polishing pad, which is used to prepare the above-mentioned chlorovinyl acetate resin modified polyurethane composite polishing pad, comprising the following steps:

[0031] Step 1: Dispersing the coating slurry: adding the chlorovinyl resin modified polyurethane wet resin, color paste, nonionic surfactant, anionic surfactant and diluent into a container, dispersing at a speed of 800-1000 r / min for 2-3 hours until the mixture is uniformly mixed, to obtain the coating slurry;

[0032] Step 2: Degassing the coating slurry, degassing the uniformly dispersed coating slurry under a negative pressure of 0.08 to 0.10 MPa for 3 to 4 hours, and the viscosity of the coating slurry at 25°C is 10000 to 15000 mPa·S;

[0033] Step 3: wet coating and solidification, coating a layer of the coating slurry obtained in step 2 on the impregnation layer, the wet film thickness of the coating slurry is 1.5-2.0 mm, and placing it in a DMF aqueous solution with a temperature of 25-45° C. and a mass concentration of 10%-30% for solidification and foaming to obtain a solidified sample;

[0034] Step 4: Washing and drying to fix the solidified sample, place it in deionized water at 40-60°C to clean the solvent, repeat more than 10 times until the sample solvent concentration is within 1%, and place it at 100-120°C to dry for 4-6 hours to fix the shape;

[0035] Step 5: Grinding and hot pressing: Grind the shaped sample with 150-400 mesh sandpaper to remove the dense layer on the surface of the coating layer to expose the upright bubbles, and then perform hot pressing to press the pattern. The hot pressing temperature is 120-140°C.

[0036] Step 6: adhesive bonding and cutting, the hot pressed sample is adhesive bonded and cut into discs to obtain a vinyl chloride resin modified polyurethane composite polishing pad.

[0037] In summary, the present invention has at least the following benefits:

[0038] 1. The chlorovinyl acetate resin modified polyurethane composite polishing pad provided by the present invention is prepared by using chlorovinyl acetate resin modified polyurethane wet resin as the main raw material. The wet resin is a polyurethane modified by chlorovinyl acetate resin grafting, and its main chain is a polyurethane structure with alternating hard and soft segments, and the side chain is a chlorovinyl acetate resin structure of vinyl chloride-vinyl acetate-vinyl alcohol copolymerization, so that the overall segment structure is more diversified, the upper limit of the number average molecular weight can be effectively increased, and its wear resistance and mechanical properties are greatly improved. The prepared polishing pad has good wear resistance, high removal rate and long service life, which effectively solves the problems of insufficient wear resistance, poor mechanical properties and short service life of existing fine polishing pads.

[0039] 2. The chloroacetic acid resin modified polyurethane composite polishing pad provided by the present invention adopts chloroacetic acid resin modified polyurethane as wet resin, wherein the chloroacetic acid resin grafted modified polyurethane introduces hydroxyl groups that do not participate in the reaction on the side chains of the wet resin, which helps to promote the exchange of solvent and water in the wet foaming process, forming more uniform droplet-shaped pores and improving their porosity, effectively solving the problems of uneven pores, low porosity, insufficient liquid carrying capacity, poor affinity with polishing liquid and low polishing removal rate commonly existing in existing fine polishing pads.

[0040] 3. The preparation method of the chlorovinyl acetate resin modified polyurethane composite polishing pad provided by the present invention comprises the following steps: preparing an impregnation layer from a synthesized chlorovinyl acetate resin modified polyurethane wet resin and a non-woven fabric through an impregnation process to replace a PET film as a buffer layer of the polishing pad; and then directly scraping the coating slurry onto the impregnation layer for solidification, water washing, and drying and shaping. The impregnation layer and the coating layer do not need to be peeled off or hot-melt glued together, which greatly simplifies the cumbersome preparation process of using the PET film as a buffer layer, and can also effectively improve the compression ratio and rebound rate of the polishing pad, thereby solving the problems of poor wafer flatness and high surface defectivity in the CMP fine polishing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The present invention is a simplified flow chart of the preparation method of the chlorovinyl resin modified polyurethane composite polishing pad.

[0042] Figure 2This is a surface SEM image of the chlorovinyl resin modified polyurethane composite polishing pad prepared in Example 1 of the present invention.

[0043] Figure 3 This is a cross-sectional SEM image of the chlorovinyl resin modified polyurethane composite polishing pad prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0044] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with the accompanying drawings and specific embodiments. Preferred embodiments of the present invention are provided in the embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0046] References in the specification to "one embodiment", "embodiment", "exemplary embodiment", etc. mean the embodiment being described, but not every embodiment may include a particular feature, structure, or characteristic. Specific features, structures, or characteristics are included. Moreover, such phrases do not necessarily refer to the same embodiment. In addition, when specific features, structures, or characteristics are described in conjunction with certain embodiments, whether or not explicitly described, it is within the knowledge of those skilled in the art to consider the effects of applying the features, structures, or characteristics to other embodiments.

[0047] The values ​​expressed as ranges should be interpreted in a flexible manner, including not only the values ​​explicitly listed as the limits of the range, but also all individual values ​​or sub-ranges included in the range, as if each value and sub-range were clearly stated. For example, a (mass) concentration range of "about 0.1% to about 5%" should be interpreted as including not only the explicitly listed values ​​of about 0.1% to about 5% by weight, but also the individual (mass) concentrations (e.g., 1%, 2%, 3% and 4%) and sub-ranges (e.g., 0.1% to 0.5%, 1.1% to 2.2% and 3.3% to 4.4%) within the specified range.

[0048] As described herein, unless stated otherwise, the terms "a" and "an" are used to include one or more than one, and the term "or" is used to refer to a non-exclusive "or". In addition, when a term or terms used herein are not otherwise qualified, they should be understood to be used for descriptive purposes only and not for limiting purposes. In addition, all publications, patents, and patent documents mentioned in the specification are incorporated herein by reference in their entirety, as if individually incorporated by introduction. If there is an inconsistency in usage between this document and those documents incorporated by reference, the usage in the cited references should be considered to supplement this document. For irreconcilable inconsistencies, the usage in this document shall prevail.

[0049] A chlorovinyl acetate resin modified polyurethane composite polishing pad is prepared from the following components in parts by weight: 1000-2000 parts of color paste, 15-45 parts of nonionic surfactant, 15-45 parts of anionic surfactant, 500-1000 parts of diluent, 300-330 parts of back glue, 3000-4000 parts of chlorovinyl acetate resin modified polyurethane wet resin, and 170-200 parts of impregnation layer.

[0050] Among the above components, the color paste is selected from carbon black paste or titanium dioxide paste;

[0051] The nonionic surfactant is selected from sorbitan monostearate (Span-60) or sorbitan monooleate (Span-80);

[0052] The anionic surfactant is selected from docusate sodium (OT-100) or sodium dodecylbenzene sulfonate (SDBS);

[0053] The diluent solvent is N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP) or dimethyl sulfoxide (DMSO);

[0054] The adhesive backing is a pressure-sensitive acrylic adhesive backing, preferably 568HM2, 560PSD or 5628C produced by Sekisui Chemical Co., Ltd. of Japan, with a thickness of 100 to 200 μm.

[0055] The chlorovinyl acetate resin modified polyurethane wet process resin is prepared from the following components in parts by weight: 40-60 parts of diisocyanate, 180-540 parts of polyether diol, 5-15 parts of aromatic diamine, 100-200 parts of chlorovinyl acetate resin, 1-5 parts of chain terminator, and 605-2460 parts of solvent; the chlorovinyl acetate resin modified polyurethane wet process resin has a solid content of 25.0wt%-35.0wt%, a viscosity of 150000-200000mPa·S at 25°C, and a number average molecular weight Mn of 120000-150000.

[0056] Among them, the chlorovinyl resin is a vinyl chloride-vinyl acetate-vinyl alcohol copolymer, with a hydroxyl value between 50 and 100 mgKOH / g and a molecular weight between 30,000 and 50,000;

[0057] The diisocyanate is selected from at least one of toluene-2,4-diisocyanate (2,4-TDI), toluene-2,6-diisocyanate (2,6-TDI), 4,4'-diphenylmethane diisocyanate (4,4-MDI) and 2,4'-diphenylmethane diisocyanate (2,4-MDI).

[0058] The polyether diol is selected from at least one of polytetrahydrofuran diol and polypropylene glycol; wherein the specification of polytetrahydrofuran diol is PTMG-1000, PTMG-2000 or PTMG-3000, and the specification of polypropylene glycol is PPG-1000, PPG-2000 or PPG-3000.

[0059] The aromatic diamine is at least one selected from 4,4'-diaminodiphenylmethane (4,4-MDA), 2,4'-diaminodiphenylmethane (2,4-MDA), 2,4-diaminotoluene (2,4-TDA) or 2,6-diaminotoluene (2,6-TDA);

[0060] The chain terminator is selected from methanol, ethanol or isopropanol.

[0061] The above-mentioned chlorovinyl resin modified polyurethane wet resin is prepared by the following method:

[0062] (1) prepolymerization reaction, dehydrating the polyether diol at 105-110° C. and negative pressure of 0.08-0.10 MPa for 1 hour, adding diisocyanate and prepolymerizing at 80-90° C. for 2-3 hours to obtain an isocyanate-terminated prepolymer;

[0063] (2) chain extension reaction, adding solvent and aromatic diamine to the obtained prepolymer in sequence for chain extension, and maintaining the reaction at 80-90° C. for 2-3 hours until the system solution is polymerized to a molecular weight between 60,000 and 80,000;

[0064] (3) Grafting reaction: adding chlorovinyl acetate resin and maintaining the temperature at 80-90° C. for 3-4 hours to chemically graft the chlorovinyl acetate resin onto the polyurethane chain segment;

[0065] (4) Termination reaction: when the grafting reaction reaches a number average molecular weight Mn between 120,000 and 150,000, a chain terminator is added to terminate the reaction, and the material is discharged to obtain a vinyl chloride resin modified polyurethane wet process resin.

[0066] The impregnation layer is prepared from the following components by weight: 2000-3000 parts of chlorovinyl resin modified polyurethane wet resin, 4000-5000 parts of solvent, and 130-140 parts of non-woven fabric.

[0067] In the impregnation layer, the viscosity of the impregnation slurry at 25°C is 200-500mPa·S, and the resin impregnation ratio is 30%-35%; the non-woven fabric is selected from PET needle-punched non-woven fabric or PET spunlace non-woven fabric, and the thickness of the non-woven fabric is between 0.8 and 1.0 mm, and the gram weight is between 130 and 140 g / m 2 between.

[0068] The impregnation layer is prepared by the following method:

[0069] Add chlorovinyl resin modified polyurethane wet resin and solvent, disperse at a speed of 800-1000r / min for 1-2h until mixed evenly; then degas for 2-3h under vacuum conditions of negative pressure 0.08-0.10Mpa to obtain impregnation slurry; finally, mix and impregnate the non-woven fabric and the impregnation slurry evenly, put it into DMF aqueous solution for coagulation, wash with water, dry and shape, and obtain the impregnation layer.

[0070] The above-mentioned chlorovinyl resin modified polyurethane composite polishing pad is prepared by the following preparation method, which comprises the following steps:

[0071] Step 1: Dispersing the coating slurry: adding the chlorovinyl resin modified polyurethane wet resin, color paste, nonionic surfactant, anionic surfactant and diluent into a container, dispersing at a speed of 800-1000 r / min for 2-3 hours until the mixture is uniformly mixed, to obtain the coating slurry;

[0072] Step 2: Degassing the coating slurry, degassing the uniformly dispersed coating slurry under a negative pressure of 0.08 to 0.10 MPa for 3 to 4 hours, and the viscosity of the coating slurry at 25°C is 10000 to 15000 mPa·S;

[0073] Step 3: wet coating and solidification, coating a layer of the coating slurry obtained in step 2 on the impregnation layer, the wet film thickness of the coating slurry is 1.5-2.0 mm, and placing it in a DMF aqueous solution with a temperature of 25-45° C. and a mass concentration of 10%-30% for solidification and foaming to obtain a solidified sample;

[0074] Step 4: Washing and drying to fix the solidified sample, place it in deionized water at 40-60°C to clean the solvent, repeat more than 10 times until the sample solvent concentration is within 1%, and place it at 100-120°C to dry for 4-6 hours to fix the shape;

[0075] Step 5: Grinding and hot pressing: Grind the shaped sample with 150-400 mesh sandpaper to remove the dense layer on the surface of the coating layer to expose the upright bubbles, and then perform hot pressing to press the pattern. The hot pressing temperature is 120-140°C.

[0076] Step 6: adhesive bonding and cutting, the hot pressed sample is adhesive bonded and cut into discs to obtain a vinyl chloride resin modified polyurethane composite polishing pad.

[0077] Example 1

[0078] The present embodiment provides a chlorovinyl resin modified polyurethane composite polishing pad, which is prepared from the following raw materials and parts by weight: 1500 parts of color paste, 30 parts of nonionic surfactant, 30 parts of anionic surfactant, 750 parts of diluent solvent, 315 parts of backing glue, 3500 parts of chlorovinyl resin modified polyurethane wet resin, and 185 parts of impregnation layer; the chlorovinyl resin modified polyurethane composite polishing pad has a thickness of 1.5 mm, a 100% modulus of 14 MPa, a hardness of 52 Shore A, a compression ratio of 23%, a rebound rate of 92%, a pore size of 35 μm, and a porosity of 60%.

[0079] Preferably, the color paste is a carbon black paste with a solid content of 20wt% and a median particle size of 120nm, the nonionic surfactant is sorbitan monooleate (Span-80), the anionic surfactant is docusate sodium (OT-100), the diluent is N,N-dimethylformamide (DMF), and the backing adhesive is 560PSD of Sekisui Chemical Co., Ltd. of Japan with a thickness of 150μm.

[0080] In this embodiment, the vinyl chloride resin modified polyurethane wet resin is synthesized from the following raw materials and parts by weight: 50 parts of diisocyanate, 360 parts of polyether diol, 10 parts of aromatic diamine, 150 parts of vinyl chloride resin, 2 parts of chain terminator, and 1300 parts of diluent; the vinyl chloride resin modified polyurethane wet resin has a solid content of 30.6wt%, a viscosity of 180000mPa·S at 25°C, and a number average molecular weight Mn of 135000.

[0081] Preferably, the diisocyanate is 4,4'-diphenylmethane diisocyanate (4,4-MDI), the polyether diol is polytetramethylene glycol (preferably PTMG-2000), the aromatic diamine is 4,4'-diaminodiphenylmethane (4,4-MDA), the chloroacetic acid resin is a vinyl chloride-vinyl acetate-vinyl alcohol copolymer, its hydroxyl value is 75 mgKOH / g, and its molecular weight is 40000, and the chain terminator is methanol.

[0082] In this embodiment, the synthesis method of chlorovinyl resin modified polyurethane wet resin comprises the following steps:

[0083] Step 1: prepolymerization reaction, dehydrating the polyether diol at 105-110° C. and negative pressure of 0.08-0.10 MPa for 1 hour, adding diisocyanate to carry out prepolymerization reaction at 80-90° C. for 2-3 hours to obtain an isocyanate-terminated prepolymer;

[0084] Step 2: Chain extension reaction, adding a diluent solvent and an aromatic diamine to the prepolymer in sequence for chain extension, and maintaining the reaction at 80-90° C. for 2-3 hours until the system solution is polymerized to a molecular weight between 60,000 and 80,000;

[0085] Step 3: Grafting reaction: adding chlorovinyl resin to the above system and maintaining the temperature at 80-90°C for 3-4 hours to chemically graft the chlorovinyl resin onto the polyurethane chain segment;

[0086] Step 4: Termination of the reaction. When the grafting reaction of the above system reaches a number average molecular weight Mn between 120,000 and 150,000, a chain terminator is added to terminate the reaction and obtain a vinyl chloride resin modified polyurethane wet process resin.

[0087] In this embodiment, the impregnation layer is prepared from the following raw materials and weight parts: 2500 parts of vinyl chloride resin modified polyurethane wet resin, 4500 parts of diluent, and 135 parts of non-woven fabric; the viscosity of the impregnation slurry at 25°C is 350mPa·S, and the resin impregnation ratio is 33%.

[0088] Preferably, the non-woven fabric is a PET needle-punched non-woven fabric with a thickness of 0.9 mm and a gram weight of 135 g / m 2 .

[0089] In this embodiment, the method for preparing the impregnation layer includes the following steps:

[0090] The chlorovinyl resin modified polyurethane wet resin and the diluent solvent are dispersed at a speed of 800-1000 r / min for 1-2 hours until they are evenly mixed; then degassing is performed at a negative pressure of 0.08-0.10 MPa for 2-3 hours; finally, the non-woven fabric and the impregnation slurry are mixed and impregnated evenly, placed in a DMF aqueous solution for coagulation, washed with water, and dried to form an impregnation layer.

[0091] The above-mentioned chlorovinyl resin modified polyurethane composite polishing pad is prepared by the following preparation method. Figure 1 The preparation method specifically comprises the following steps, and the raw materials prepared in each step are calculated by weight according to the present embodiment:

[0092] Step 1: Disperse the coating slurry, disperse the chlorovinyl resin modified polyurethane wet resin, color paste, surfactant, and diluent at a speed of 800-1000r / min for 2-3h until the mixture is uniform;

[0093] Step 2: Degassing the coating slurry, degassing the uniformly dispersed coating slurry for 3 to 4 hours under a negative pressure of 0.08 to 0.10 MPa vacuum condition, and the viscosity of the coating slurry at 25° C. is 10,000 to 15,000 mPa·S;

[0094] Step 3: wet coating and solidification, a coating slurry with a wet film thickness of 1.5 to 2.0 mm is coated on the above impregnation layer, and placed in a DMF aqueous solution with a temperature of 25 to 45° C. and a concentration of 10% to 30% for solidification and foaming;

[0095] Step 4: Washing and drying to fix the solidified sample, place the solidified sample in deionized water at 40-60°C to clean the solvent, repeat more than 10 times until the sample solvent concentration is less than 1%, and place it at 100-120°C to dry for 4-6 hours to fix the sample;

[0096] Step 5: grinding and hot pressing, grinding the above-shaped sample with 150-400 mesh sandpaper to remove the dense layer on the surface of the coating layer to expose the upright bubbles, and then hot pressing to press the pattern, the hot pressing temperature is 120-140°C;

[0097] Step 6: adhesive bonding and cutting, the hot-pressed sample is adhesive-bonded and cut into discs to obtain a vinyl chloride resin modified polyurethane composite polishing pad.

[0098] The surface SEM image and cross-sectional SEM image of the chlorovinyl resin modified polyurethane composite polishing pad prepared in this embodiment are respectively Figure 1 and Figure 2 .

[0099] Example 2

[0100] The present embodiment provides a chlorovinyl resin modified polyurethane composite polishing pad, which is prepared from the following raw materials and parts by weight: 1000 parts of color paste, 15 parts of nonionic surfactant, 15 parts of anionic surfactant, 500 parts of diluent solvent, 300 parts of backing glue, 3000 parts of chlorovinyl resin modified polyurethane wet resin, and 170 parts of impregnation layer; the chlorovinyl resin modified polyurethane composite polishing pad has a thickness of 1.4 mm, a 100% modulus of 10 MPa, a hardness of 45 Shore A, a compression ratio of 30%, a rebound rate of 90%, a pore size of 30 μm, and a porosity of 40%.

[0101] Preferably, the color paste is titanium dioxide paste, the solid content is 10wt%, the median particle size is 100nm, the non-ionic surfactant is sorbitan monostearate (Span-60), the anionic surfactant is sodium dodecylbenzene sulfonate (SDBS), the diluent is N-methylpyrrolidone (NMP), and the backing glue is 568HM2 of Sekisui Chemical Co., Ltd., Japan, with a thickness of 100μm.

[0102] In this embodiment, the vinyl chloride resin modified polyurethane wet process resin is synthesized from the following raw materials and weight parts: 40 parts of diisocyanate, 180 parts of polyether diol, 5 parts of aromatic diamine, 100 parts of vinyl chloride resin, 1 part of chain terminator, and 605 parts of diluent; its solid content is 35.0wt%, the viscosity at 25°C is 150000mPa·S, and the number average molecular weight Mn is 120000.

[0103] Preferably, the diisocyanate is toluene-2,4-diisocyanate (2,4-TDI), the polyether diol is polypropylene glycol (preferably PPG-1000), the aromatic diamine is 2,4'-diaminodiphenylmethane (2,4-MDA), the chloroacetic acid resin is a vinyl chloride-vinyl acetate-vinyl alcohol copolymer, the hydroxyl value is 50 mgKOH / g, the molecular weight is 50000, and the chain terminator is ethanol.

[0104] In this embodiment, the impregnation layer is prepared from the following raw materials and weight parts: 2000 parts of chlorovinyl resin modified polyurethane wet resin, 5000 parts of diluent, and 130 parts of non-woven fabric; the viscosity of the impregnation slurry at 25° C. is 200 mPa·S, and the resin impregnation ratio is 30%.

[0105] Preferably, the nonwoven fabric is a PET spunlace nonwoven fabric with a thickness of 0.8 mm and a gram weight of 130 g / m 2 .

[0106] For the preparation method of the vinyl chloride resin modified polyurethane wet resin, the preparation method of the impregnation layer, and the preparation method of the vinyl chloride resin modified polyurethane composite polishing pad of this embodiment, please refer to Example 1; during the preparation process, the raw materials required for each step are calculated according to the weight parts of this embodiment.

[0107] Example 3

[0108] The present embodiment provides a chlorovinyl resin modified polyurethane composite polishing pad, which is prepared from the following raw materials and weight portions: 2000 parts of color paste, 45 parts of nonionic surfactant, 45 parts of anionic surfactant, 1000 parts of diluent solvent, 330 parts of backing glue, 4000 parts of chlorovinyl resin modified polyurethane wet resin, and 200 parts of impregnation layer; its thickness is 1.6 mm, 100% modulus is 12 MPa, hardness is 50 Shore A, compression ratio is 28%, rebound rate is 97%, pore diameter is 40 μm, and porosity is 46%.

[0109] Preferably, the color paste is a carbon black paste with a solid content of 30wt% and a median particle size of 200nm, the nonionic surfactant is sorbitan monostearate (Span-60), the anionic surfactant is docusate sodium (OT-100), the diluting solvent is dimethyl sulfoxide (DMSO), and the backing adhesive is 5628C of Sekisui Chemical Co., Ltd. of Japan with a thickness of 200μm.

[0110] In this embodiment, the vinyl chloride resin modified polyurethane wet process resin is synthesized from the following raw materials and weight parts: 60 parts of diisocyanate, 540 parts of polyether diol, 15 parts of aromatic diamine, 200 parts of vinyl chloride resin, 5 parts of chain terminator, and 2460 parts of diluent; its solid content is 25.0wt%, the viscosity at 25°C is 200000mPa·S, and the number average molecular weight Mn is 144000.

[0111] Preferably, the diisocyanate is toluene-2,6-diisocyanate (2,6-TDI), the polyether diol is polypropylene glycol (preferably PPG-3000), the aromatic diamine is 2,6-diaminotoluene (2,6-TDA), the chloroacetic acid resin is a vinyl chloride-vinyl acetate-vinyl alcohol copolymer, the hydroxyl value is 100 mgKOH / g, the molecular weight is 30000, and the chain terminator is isopropanol.

[0112] In this embodiment, the impregnation layer is prepared from the following raw materials and weight parts: 3000 parts of chlorovinyl resin modified polyurethane wet resin, 4000 parts of diluent, and 140 parts of non-woven fabric; the viscosity of the impregnation slurry at 25° C. is 500 mPa·S, and the resin impregnation ratio is 35%.

[0113] Preferably, the nonwoven fabric is a PET spunlace nonwoven fabric with a thickness of 1.0 mm and a gram weight of 140 g / m 2 .

[0114] For the preparation method of the vinyl chloride resin modified polyurethane wet resin, the preparation method of the impregnation layer, and the preparation method of the vinyl chloride resin modified polyurethane composite polishing pad of this embodiment, please refer to Example 1; during the preparation process, the raw materials required for each step are calculated according to the weight parts of this embodiment.

[0115] Example 4

[0116] The present embodiment provides a chlorovinyl resin modified polyurethane composite polishing pad, which is prepared from the following raw materials and weight portions: 1600 parts of color paste, 33 parts of nonionic surfactant, 33 parts of anionic surfactant, 800 parts of diluent solvent, 310 parts of backing glue, 3600 parts of chlorovinyl resin modified polyurethane wet resin, and 180 parts of impregnation layer; its thickness is 1.5 mm, 100% modulus is 15 MPa, hardness is 55 Shore A, compression ratio is 20%, rebound rate is 100%, pore size is 36 μm, and porosity is 55%.

[0117] Preferably, the color paste is titanium dioxide paste, has a solid content of 30wt%, and a median particle size of 200nm, the non-ionic surfactant is sorbitan monooleate (Span-80), the anionic surfactant is sodium dodecylbenzene sulfonate (SDBS), the diluent is N,N-dimethylformamide (DMF), and the backing glue is 560PSD of Sekisui Chemical Co., Ltd., Japan, with a thickness of 180μm.

[0118] In this embodiment, the vinyl chloride resin modified polyurethane wet resin is synthesized from the following raw materials and parts by weight: 55 parts of diisocyanate, 330 parts of polyether diol, 12 parts of aromatic diamine, 160 parts of vinyl chloride resin, 3 parts of chain terminator, and 1240 parts of diluent; its solid content is 31.1wt%, the viscosity at 25°C is 175000mPa·S, and the number average molecular weight Mn is 150000.

[0119] Preferably, the diisocyanate is 2,4'-diphenylmethane diisocyanate (2,4-MDI), the polyether diol is polytetramethylene glycol (preferably PTMG-1000), the aromatic diamine is 2,4-diaminotoluene (2,4-TDA), the chloroacetic acid resin is a vinyl chloride-vinyl acetate-vinyl alcohol copolymer, the hydroxyl value is 70 mgKOH / g, the molecular weight is 45000, and the chain terminator is methanol.

[0120] In this embodiment, the impregnation layer is prepared from the following raw materials and weight parts: 2600 parts of vinyl chloride resin modified polyurethane wet resin, 4400 parts of diluent, and 133 parts of non-woven fabric; the viscosity of the impregnation slurry at 25°C is 300mPa·S, and the resin impregnation ratio is 32%.

[0121] Preferably, the non-woven fabric is a PET needle-punched non-woven fabric with a thickness of 0.9 mm and a gram weight of 133 g / m 2 .

[0122] For the preparation method of the vinyl chloride resin modified polyurethane wet resin, the preparation method of the impregnation layer, and the preparation method of the vinyl chloride resin modified polyurethane composite polishing pad of this embodiment, please refer to Example 1; during the preparation process, the raw materials required for each step are calculated according to the weight parts of this embodiment.

[0123] Comparative Example 1

[0124] The difference of Comparative Example 1 and Example 1 is only: when synthesizing wet process resin, the synthetic raw material is replaced by polytetrahydrofuran diol (PTMG-2000) with parts by weight such as chlorovinyl resin, and all the other are all consistent with Example 1.

[0125] Comparative Example 2

[0126] The difference between Comparative Example 2 and Example 1 is that in the raw material for preparing the polishing pad, an equal weight portion of the impregnation layer is replaced with a PET (polyethylene terephthalate) film with a thickness of 0.188 mm, and the rest is consistent with Example 1.

[0127] Test example

[0128] The physical parameters and polishing performance of the chlorovinyl resin modified polyurethane composite polishing pads prepared in Examples 1 to 4 and the polishing pads prepared in Comparative Examples 1 to 2 were tested.

[0129] The test method of number average molecular weight Mn refers to the national standard "GB / T 27843-2011", and the gel permeation chromatograph (GPC) model is Agilent 1260Infinity II.

[0130] The resin impregnation ratio is determined by the following formula: RIR = (M1-M0) / M1×100%, where M0 is the mass of the nonwoven fabric and M1 is the mass of the impregnation layer.

[0131] The test method of 100% modulus refers to the national standard "GB / T 1040.3-2006", and the electronic universal material testing machine model is ZwickRoll 5kN Allround table top.

[0132] The hardness test method refers to the national standard "GB / T 2411-2008", and the Shore A hardness tester model is Teclock GS-709G.

[0133] The test methods for compression ratio and rebound rate refer to GB / T 30709-2014, and the dynamic mechanical analyzer (DMA) model is TA DMA850.

[0134] The test method for wear resistance refers to GB / T 5478-2008, and the abrasion testing machine model is Taber 1700.

[0135] The test methods for pore size and porosity refer to the national standard "GB / T 21650.1-2008", and the pore size analyzer model is MicroActive AutoPore V 9600.

[0136] The liquid carrying rate is determined by the following formula: LCR = (M1-M0) / M0×100%, wherein M0 is the mass of the polishing pad before being loaded with liquid, and M1 is the mass of the polishing pad after being loaded with liquid.

[0137] The test methods for polishing removal rate, life time, surface roughness and surface defects are as follows:

[0138] Remove the release paper from the 30-inch polishing pad sample and stick it on the CMP machine. The polishing liquid model is Anji-D3000, the flow rate is 300cc / min, the wafer model is 12-inch Teos Wafer, the CMP machine model is Universal-300B, the pressure is 1.3psi, the grinding head speed is 70rpm, the grinding disc speed is 75rpm, and the dressing disc is Blue Brush;

[0139] Polishing removal rate (Removal Rate) is the average value calculated by recording the removal rate during the polishing process using a four-probe film thickness meter (KLA Filmetrics R50);

[0140] Surface roughness (Roughness) was measured by a 3D surface profiler (CHOTEST Superview W1);

[0141] The number of surface defects is the total number of defects on the wafer surface with a size greater than 100 nm detected by the defect analysis system (AMAT SEMVision G7);

[0142] The service life (Life Time) is measured by recording the maximum length of time that the polishing pad is continuously subjected to chemical mechanical polishing (CMP) testing until the polishing removal rate drops significantly.

[0143] The test results of the physical parameters and polishing performance of the chlorovinyl resin modified polyurethane composite polishing pads prepared in Examples 1 to 4 and the polishing pads prepared in Comparative Examples 1 to 2 are shown in Table 1.

[0144] Table 1 Physical parameters and polishing performance test results of polishing pads prepared in Examples and Comparative Examples 1 to 2

[0145]

[0146]

[0147] The test results of the physical parameters and polishing performance of the polishing pads in the above embodiments and comparative examples show that:

[0148] Compared with the chloroacetic acid resin modified polyurethane composite polishing pads prepared in Comparative Examples 1, 1 to 4, the polyurethane is modified by grafting the chloroacetic acid resin side chains, so that the segment structure of the wet resin is more diversified, the upper limit of the number average molecular weight can be effectively increased, and its wear resistance (reduced wear) and mechanical properties (increased 100% modulus and hardness) are greatly improved. The prepared polishing pad has a high removal rate and a long service life.

[0149] In the vinyl chloride resin modified polyurethane composite polishing pad prepared in Examples 1 to 4, the vinyl chloride resin modified polyurethane wet resin segment has abundant hydroxyl groups that do not participate in the reaction, which helps to promote the formation of more uniform droplet-shaped bubbles and improve its porosity and liquid carrying rate in the wet foaming process, thereby effectively improving its liquid carrying capacity and polishing removal rate.

[0150] Compared with Comparative Example 2, in the chlorovinyl resin modified polyurethane composite polishing pad prepared in Examples 1 to 4, the synthetic wet resin and non-woven fabric are prepared into an impregnation layer through an impregnation process to replace the PET film as the polishing pad buffer layer, which can effectively improve the compression ratio and rebound rate of the polishing pad, and can improve the flatness of the wafer (reduce the roughness) and reduce the surface defects (reduce the number of defects) in the CMP fine polishing process.

[0151] The above contents are merely examples and illustrations of the structure of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and these obvious replacement forms all belong to the protection scope of the present invention.

Claims

1. A chlorovinyl resin modified polyurethane composite polishing pad, It is characterized in that It is prepared from the following components by weight: 1000-2000 parts of color paste, 15-45 parts of nonionic surfactant, 15-45 parts of anionic surfactant, 500-1000 parts of diluent solvent, 300-330 parts of adhesive, 3000-4000 parts of chloroacetic resin modified polyurethane wet resin, and 170-200 parts of impregnation layer.

2. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 1, It is characterized in that The chlorovinyl resin modified polyurethane wet resin is prepared from the following components by weight: 40-60 parts of diisocyanate, 180-540 parts of polyether diol, 5-15 parts of aromatic diamine, 100-200 parts of chlorovinyl resin, 1-5 parts of chain terminator, and 605-2460 parts of solvent; The chlorovinyl resin is a vinyl chloride-vinyl acetate-vinyl alcohol copolymer, the hydroxyl value of which is between 50 and 100 mgKOH / g, and the molecular weight is between 30,000 and 50,000.

3. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 2, It is characterized in that The diisocyanate includes at least one of toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, 4,4'-diphenylmethane diisocyanate or 2,4'-diphenylmethane diisocyanate.

4. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 2, It is characterized in that The polyether diol is at least one of polytetrahydrofuran diol and polypropylene glycol; wherein the specification of the polytetrahydrofuran diol is PTMG-1000, PTMG-2000 or PTMG-3000, and the specification of the polypropylene glycol is PPG-1000, PPG-2000 or PPG-3000.

5. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 2, It is characterized in that The aromatic diamine includes at least one of 4,4'-diaminodiphenylmethane, 2,4'-diaminodiphenylmethane, 2,4-diaminotoluene or 2,6-diaminotoluene; The chain terminator is methanol, ethanol or isopropanol.

6. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 2, It is characterized in that The chlorovinyl acetate resin modified polyurethane wet process resin is prepared by the following method: Prepolymerization reaction: dehydrating the polyether diol at 105-110° C. and negative pressure of 0.08-0.10 MPa for 1 hour, adding diisocyanate to carry out prepolymerization reaction at 80-90° C. for 2-3 hours to obtain an isocyanate-terminated prepolymer; Chain extension reaction: adding solvent and aromatic diamine to the prepared prepolymer in sequence for chain extension, and maintaining the reaction temperature at 80-90°C for 2-3 hours until the system solution is polymerized to a molecular weight between 60,000 and 80,000; Grafting reaction: adding chlorovinyl resin and maintaining 80-90°C for grafting reaction for 3-4 hours to chemically graft the chlorovinyl resin onto the polyurethane chain segment; The reaction is terminated, and when the grafting reaction reaches a number average molecular weight Mn between 120,000 and 150,000, a chain terminator is added to terminate the reaction, and the material is discharged to obtain a vinyl chloride resin modified polyurethane wet process resin.

7. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 1, It is characterized in that The color paste is carbon black paste or titanium dioxide paste; The nonionic surfactant is sorbitan monostearate or sorbitan monooleate; The anionic surfactant is sodium docusate or sodium dodecylbenzene sulfonate; The diluting solvent is N,N-dimethylformamide, N-methylpyrrolidone or dimethyl sulfoxide; The adhesive backing is a pressure-sensitive acrylic adhesive backing, and its model is 568HM2, 560PSD or 5628C, and its thickness is between 100 and 200 μm.

8. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 1, It is characterized in that The impregnation layer is prepared from the following components by weight: 2000-3000 parts of chlorovinyl resin modified polyurethane wet resin, 4000-5000 parts of solvent, and 130-140 parts of non-woven fabric.

9. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 8, It is characterized in that In the impregnation layer, the viscosity of the impregnation slurry at 25° C. is 200 to 500 mPa·S, and the resin impregnation ratio is 30% to 35%; The nonwoven fabric includes PET needle-punched nonwoven fabric or PET spunlace nonwoven fabric, and the thickness of the nonwoven fabric is between 0.8 and 1.0 mm, and the gram weight is between 130 and 140 g / m 2 between.

10. The chlorovinyl acetate resin modified polyurethane composite polishing pad according to claim 8, It is characterized in that The impregnation layer is prepared by the following method: Add chlorovinyl resin modified polyurethane wet resin and solvent, disperse at a speed of 800-1000r / min for 1-2h until mixed evenly; then degas for 2-3h under vacuum conditions of negative pressure 0.08-0.10Mpa to obtain impregnation slurry; finally, mix and impregnate the non-woven fabric and the impregnation slurry evenly, put it into DMF aqueous solution for coagulation, wash with water, dry and shape, and obtain the impregnation layer.

11. A method for preparing a chlorovinyl acetate resin modified polyurethane composite polishing pad, which is used to prepare the chlorovinyl acetate resin modified polyurethane composite polishing pad according to any one of claims 1 to 10. It is characterized in that The following steps are involved: Step 1: Dispersing the coating slurry: adding the chlorovinyl resin modified polyurethane wet resin, color paste, nonionic surfactant, anionic surfactant and diluent into a container, dispersing at a speed of 800-1000 r / min for 2-3 hours until the mixture is uniformly mixed, to obtain the coating slurry; Step 2: Degassing the coating slurry, degassing the uniformly dispersed coating slurry under a negative pressure of 0.08 to 0.10 MPa for 3 to 4 hours, and the viscosity of the coating slurry at 25°C is 10000 to 15000 mPa·S; Step 3: wet coating and solidification, coating a layer of the coating slurry obtained in step 2 on the impregnation layer, the wet film thickness of the coating slurry is 1.5-2.0 mm, and placing it in a DMF aqueous solution with a temperature of 25-45° C. and a mass concentration of 10%-30% for solidification and foaming to obtain a solidified sample; Step 4: Washing and drying to fix the solidified sample, place it in deionized water at 40-60°C to clean the solvent, repeat more than 10 times until the sample solvent concentration is within 1%, and place it at 100-120°C to dry for 4-6 hours to fix the shape; Step 5: Grinding and hot pressing: Grind the shaped sample with 150-400 mesh sandpaper to remove the dense layer on the surface of the coating layer to expose the upright bubbles, and then perform hot pressing to press the pattern. The hot pressing temperature is 120-140°C. Step 6: adhesive bonding and cutting, the hot pressed sample is adhesive bonded and cut into discs to obtain a vinyl chloride resin modified polyurethane composite polishing pad.

Citation Information

Patent Citations

  • Waterborne polyurethane resin emulsion and preparation method thereof, two-component waterborne silver powder coating composition and preparation method thereof

    CN102875736A

  • Manufacturing method of polyurethane polishing pad

    CN104385120A

  • Binder for printing ink, laminate ink composition for soft packaging, and printed article

    CN105705595A

  • High-abrasion-resistance polyurethane elastomer foaming material and preparation method thereof

    CN106633795A

  • Non-woven grinding product and application thereof

    CN109352539A

Cited By

  • Rough polishing pad for SiC wafer and preparation method of rough polishing pad

    CN119458143A

  • Polishing pad and preparation method thereof

    CN121156908A

  • A polishing pad and a method of making the same

    CN121156908B

  • Polishing pad for fine polishing process of silicon wafer as well as preparation method and application of polishing pad

    CN121670547A

  • Polishing pad for silicon wafer final polishing process and method of making and use thereof

    CN121670547B