Roller remanufacturing method based on seamless gluing
Through seamless gluing technology, the problem of on-site remanufacturing and partial remanufacturing in roller manufacturing is solved, efficient and seamless roller remanufacturing is achieved, the service life and reliability of the roller are improved, and it is suitable for various forms of damage. Roller repair and new roller fabrication.
Patent Information
- Application Number
- CN202411037991.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-08
AI Technical Summary
In the existing roller manufacturing method, the rubber-coated roller cannot be remanufactured on site. The rubber-coated roller has structural defects in gaps and high production costs, and local damage cannot be remanufactured, resulting in low production efficiency and poor reliability.
A roller remanufacturing method based on seamless gluing is adopted, using V2210 rubber treatment agent, V430 multifunctional primer and V7088 polyurethane-based wear-resistant composite material, to form a seamless wear-resistant coating through grinding, brushing and heating and curing. Achieve partial or complete remanufacturing of the rubber layer on the surface of the roller.
It realizes efficient on-site remanufacturing of the roller, eliminates the structural defects of the rubber coating gap, improves the service life and reliability, can carry out partial remanufacturing in a narrow space, supports unlimited recycling remanufacturing, and is suitable for old rollers. Repair and new drum fabrication.
Smart Images

Figure CN118744546A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heavy-load conveying equipment manufacturing, and in particular to a roller remanufacturing method based on seamless glue coating. Background Art
[0002] In large-scale bulk material production, storage and transportation enterprises, heavy-duty rubber conveyor belts are key equipment, and the core component of the conveyor belt operation is the roller. A conveyor belt usually consists of several rollers, such as: drive roller, redirection roller, booster roller, tensioning roller, support roller, etc.
[0003] 1. Commonly used roller manufacturing methods:
[0004] There are two common types of rollers: cast rubber rollers and rubber-coated rollers.
[0005] 1. Characteristics of the manufacturing process of cast rubber roller:
[0006] The metal base of the roller is threaded, clay is bonded on the thread, rubber is poured on the clay to make a roller embryonic body, the embryonic body is placed in a vulcanizing tank to vulcanize the rubber, and the outer circle is turned.
[0007] The advantages of cast rubber rollers are: they are manufactured on professional equipment in professional factories, there are no gaps on the roller surface, and the product quality is good.
[0008] The disadvantages of cast rubber rollers are:
[0009] (1) It cannot be manufactured on site. After the rubber lagging is damaged, the roller can only be disassembled and returned to the factory for remanufacturing;
[0010] (2) If the rubber coating is damaged, it cannot be partially remanufactured. The rubber coating can only be completely removed and manufactured according to the new roller process;
[0011] (3) It takes a long time and is costly to return to the factory for remanufacturing.
[0012] 2. Characteristics of rubber-coated roller manufacturing process:
[0013] The metal substrate of the roller is polished, and the modified chloroprene rubber adhesive is applied on the metal substrate and the semi-vulcanized layer (CN layer) of the rubber sheet respectively. After being left in the air for a while, the rubber sheet is pasted on the metal substrate.
[0014] The advantages of rubber-coated rollers are: they make up for the deficiency that cast rubber rollers cannot be remanufactured on site, and can be remanufactured on site or online without disassembly.
[0015] Disadvantages of rubber-coated rollers:
[0016] (1) The rubber sheet is composed of several pieces. The joints between the sheets are structural defects. These gaps are the weak points of the pulley rubber lagging. They are often damaged by water or foreign objects entering the gaps, causing the rubber lagging to crack and become scrapped (such as Figure 4 shown);
[0017] (2) The time required for large-scale drum lagging is more than 10 hours. If the online lagging is carried out, production must be stopped, which is something that large enterprises try their best to avoid;
[0018] (3) Lagging can only be made as a whole, and local damage cannot be remanufactured;
[0019] (4) The lagging is greatly affected by factors such as temperature, space, and experience, and the quality fluctuates greatly.
[0020] Second, the common forms of roller damage are: surface rubber layer wear and thinning (such as Figure 1 As shown), partial metal exposure (such as Figure 2 As shown), all exposed metal (such as Figure 3 As shown), cracking of the lagging gap (as shown Figure 4 shown).
[0021] Therefore, how to address the shortcomings of "cast rubber rollers" and "rubber-coated rollers" to make the remanufacturing of old rollers more high-quality and efficient and provide a way of thinking for the manufacture of new rollers is a topic that technicians in this field are constantly studying. Summary of the invention
[0022] To this end, the technical problem to be solved by the present invention is to overcome the problem in the prior art of lacking a method for on-site remanufacturing of rollers that have already experienced problems such as surface rubber layer wear and thinning, partial metal exposure, complete metal exposure, and cracking in the rubber coating to improve their performance.
[0023] In order to solve the above technical problems, the present invention selects the company's products V2210 rubber treatment agent, V430 multifunctional primer and V7088 polyurethane-based wear-resistant composite material, the V7088 polyurethane-based wear-resistant composite material includes component A wear-resistant aggregate, component B prepolymer and component C curing agent, the V2210 rubber treatment agent includes component D solvent and component E reinforcing agent, the V430 multifunctional primer is a two-component polyurethane type adhesive, and adopts the roller remanufacturing method based on seamless glue coating of the present invention to perform on-site remanufacturing of local wear or all wear of the rubber layer on the surface of the roller, including:
[0024] S1: Grind the surface of the roller body so that the metal substrate or rubber substrate is exposed to a clean surface;
[0025] S2: Applying the rubber treatment agent on the surface of the polished rubber substrate to perform chlorination treatment on the rubber, or applying the multifunctional primer on the surface of the polished metal substrate to perform interface coupling treatment on the metal, the rubber treatment agent is naturally volatilized for 5-10 minutes, and the multifunctional primer is heated and cured at 60-90° C. and kept warm for 10-20 minutes to obtain a rubber substrate or metal substrate with good surface adhesion;
[0026] S3: preparing the polyurethane-based wear-resistant composite material on site, first adding a specified proportion of component A to component B, and stirring evenly by electric means, then adding a specified proportion of component C to the AB mixture, and stirring evenly by electric means;
[0027] S4: coating the polyurethane-based wear-resistant composite material prepared in S3 on the surface of the rubber substrate modified by the rubber treatment agent in S2 and dried, or coating on the surface of the metal substrate treated by the multifunctional primer in S2 and cured, and the coating thickness of the polyurethane-based wear-resistant composite material is controlled to be 2 mm-20 mm;
[0028] S5: heating the polyurethane-based wear-resistant composite material coating at 60-90° C. and keeping the temperature for 10-20 minutes until the coating is substantially cured.
[0029] In one embodiment of the present invention, when performing S2, the rubber treating agent is first applied to the transition area on both sides of the boundary line between the rubber matrix and the metal matrix on the roller surface, and after the rubber treating agent evaporates naturally, the multifunctional primer is applied and heated for curing.
[0030] In one embodiment of the present invention, the rubber treatment agent applied on the transition area on both sides of the boundary line between the rubber matrix and the metal matrix on the roller surface needs to volatilize naturally for 5-10 minutes, the multifunctional primer needs to be heated at 60-90°C and kept warm for 10-20 minutes to basically cure the multifunctional primer, and then the polyurethane-based wear-resistant composite material coating is applied and heated and kept warm at 60-90°C for 10-20 minutes to basically cure the polyurethane-based wear-resistant composite material coating.
[0031] In one embodiment of the present invention, when the ambient temperature is greater than 5°C and there is no time limit, the polyurethane-based wear-resistant composite material coating can also be cured at room temperature for 1-24 hours. When the ambient temperature is less than 5°C and there is a time limit, the polyurethane-based wear-resistant composite material coating is heated at 60-90°C and kept warm for 10-20 minutes to cure.
[0032] In one embodiment of the present invention, when the ambient temperature is greater than 5°C and there is no time limit, the multifunctional primer can also be cured at room temperature for 1-24 hours. When the ambient temperature is less than 5°C and there is a time limit, the multifunctional primer is heated at 60-90°C and kept warm for 10-20 minutes to cure.
[0033] In one embodiment of the present invention, the polyurethane-based wear-resistant composite material coating is coated by repeated and uniform scraping, and the scraping of the polyurethane-based wear-resistant composite material coating needs to be completed before the polyurethane-based wear-resistant composite material coating loses fluidity.
[0034] In one embodiment of the present invention, the D component is the solvent of the rubber treating agent, and the D component is a mixture of dichloromethane, ketones or lipid solvents. The E component reinforcing agent is the solute of the rubber treating agent, and the E component reinforcing agent is trichloroisocyanuric acid.
[0035] In one embodiment of the present invention, the component A is a wear-resistant aggregate composed of a monomer or a mixture of ceramics and silicon carbide, the component B is a polyurethane prepolymer, and the component C is a matching curing agent.
[0036] The roller remanufacturing method based on seamless glue coating described in the present invention has the following advantages compared with the existing roller manufacturing process:
[0037] 1. The present invention utilizes a multifunctional primer to form an anchoring connection with a metal substrate and can form a molecular bond connection with a polyurethane-based wear-resistant composite material; at the same time, the rubber layer on the surface of the old drum modified by a rubber treatment agent can form a molecular bond connection with the polyurethane-based wear-resistant composite material;
[0038] 2. The present invention can be used to specifically remanufacture rollers with different forms of damage, such as rollers with worn and thinned rubber layers on the roller surface, rollers with partially exposed metal, rollers with fully exposed metal, rollers with cracked rubber coating gaps, etc.
[0039] 3. The present invention adopts advanced composite material wear-resistant technology. The thinner coating can obtain a longer service life than other technical solutions with thicker rubber, thus improving quality and efficiency;
[0040] 4. The wear-resistant layer of the rubber-coated roller remanufactured by the present invention is a seamless coating, which completely eliminates the structural defect of the rubber-coated roller having gaps, and the reliability is better after remanufacturing;
[0041] 5. The present invention can be used to partially remanufacture the roller according to the specific damage characteristics of the roller lagging;
[0042] 6. The present invention can remanufacture the roller on site in batches according to the specific workload of the roller lagging and the production permission time;
[0043] 7. The present invention can operate in a narrow space, can operate without loosening the belt, and can retain useful residual glue as much as possible, breaking through the limitations of traditional technologies in many aspects.
[0044] 8. The present invention can realize unlimited recycling and remanufacturing;
[0045] 9. The present invention can be used not only for repairing old rollers, but also for manufacturing new rollers. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein
[0047] Figure 1 It is a schematic diagram of the wear and thinning of the rubber layer on the roller surface;
[0048] Figure 2 It is a schematic diagram of the partially exposed metal on the drum surface;
[0049] Figure 3 This is a schematic diagram showing that all metal is exposed on the drum surface;
[0050] Figure 4 Schematic diagram of debonding the gap on the drum surface:
[0051] Figure 5 It is a schematic diagram of seamlessly coating a roller with worn rubber layer with the roller remanufacturing method based on seamless coating of the present invention before, during and after coating;
[0052] Figure 6 It is a schematic diagram of seamlessly coating a roller with partially exposed metal before, during and after coating using the roller remanufacturing method based on seamless coating of the present invention;
[0053] Figure 7 It is a schematic diagram of the rollers with all exposed metals being seamlessly coated with glue before, during and after the coating of glue using the roller remanufacturing method based on seamless coating of glue of the present invention;
[0054] Figure 8 Schematic diagrams of the layer structures of the coatings for only the metal substrate, only the rubber substrate, and for both the metal substrate and the rubber substrate.
[0055] Explanation of the reference numerals in the drawings in the specification: 1. Metal substrate; 2. Rubber substrate; 3. Rubber treating agent; 4. Multifunctional primer; 5. Polyurethane-based wear-resistant composite material. DETAILED DESCRIPTION
[0056] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0057] Example 1
[0058] Reference Figures 1 to 8As shown, in order to solve the above technical problems, the present invention selects the company's products V2210 rubber treatment agent 3, V430 multifunctional primer 4 and V7088 polyurethane-based wear-resistant composite material 5, V7088 polyurethane-based wear-resistant composite material 5 includes component A wear-resistant aggregate, component B prepolymer and component C curing agent, V2210 rubber treatment agent 3 includes component D solvent and component E reinforcing agent, V430 multifunctional primer 4 is a two-component polyurethane type adhesive, and adopts a roller remanufacturing method based on seamless glue coating of the present invention to remanufacture the local wear or all wear of the rubber layer on the surface of the roller on site, including:
[0059] S1: grinding the surface of the roller body so that the metal substrate 1 or the rubber substrate 2 is exposed to a clean surface;
[0060] S2: Applying rubber treatment agent 3 on the surface of the polished rubber substrate 2 to perform chlorination treatment on the rubber, or applying multifunctional primer 4 on the surface of the polished metal substrate 1 to perform interface coupling treatment on the metal, the rubber treatment agent 3 is naturally volatilized for 5-10 minutes, and the multifunctional primer 4 is heated and cured at 60-90° C. and kept warm for 10-20 minutes to obtain a rubber substrate 2 or a metal substrate 1 with good surface adhesion;
[0061] S3: preparing the polyurethane-based wear-resistant composite material 5 on site, first adding the component A in a specified proportion to the component B, and stirring them evenly by electric stirring, then adding the component C in a specified proportion to the AB mixture, and stirring them evenly by electric stirring;
[0062] S4: coating the polyurethane-based wear-resistant composite material 5 prepared in S3 on the surface of the rubber substrate 2 modified and dried by the rubber treatment agent 3 in S2 or on the surface of the metal substrate 1 treated and cured by the multifunctional primer 4 in S2, and the coating thickness of the polyurethane-based wear-resistant composite material 5 is controlled to be 2mm-20mm;
[0063] S5: heating the polyurethane-based wear-resistant composite material 5 coating at 60-90° C. and keeping the temperature for 10-20 minutes until the coating is substantially cured.
[0064] When performing S2, the rubber treatment agent 3 is first applied to the transition area on both sides of the boundary line between the rubber substrate 2 and the metal substrate 1 on the roller surface. After the rubber treatment agent 3 evaporates naturally, the multifunctional primer 4 is applied and heated for curing.
[0065] The rubber treatment agent 3 applied on the transition area on both sides of the boundary line between the rubber matrix 2 and the metal matrix 1 on the roller surface needs to volatilize naturally for 5-10 minutes, and the multifunctional primer 4 needs to be heated at 60-90°C and kept warm for 10-20 minutes to basically cure the multifunctional primer 4, and then the polyurethane-based wear-resistant composite material 5 coating is applied and heated and kept warm at 60-90°C for 10-20 minutes to basically cure the polyurethane-based wear-resistant composite material 5 coating.
[0066] When the ambient temperature is greater than 5°C and there is no time limit, the polyurethane-based wear-resistant composite material 5 coating can also be cured at room temperature for 1-24 hours. When the ambient temperature is less than 5°C and there is a time limit, the polyurethane-based wear-resistant composite material 5 coating is heated at 60-90°C and kept warm for 10-20 minutes to cure.
[0067] When the ambient temperature is greater than 5°C and there is no time limit, the multifunctional primer 4 can also be cured at room temperature for 1-24 hours. When the ambient temperature is less than 5°C and there is a time limit, the multifunctional primer 4 is heated at 60-90°C and kept warm for 10-20 minutes to cure.
[0068] The coating method of the polyurethane-based wear-resistant composite material 5 coating is repeated and uniform scraping, and the scraping of the polyurethane-based wear-resistant composite material 5 coating needs to be completed before the polyurethane-based wear-resistant composite material 5 coating loses fluidity.
[0069] The D component is the solvent of the rubber treatment agent 3, and the D component is a mixture of dichloromethane, ketones or lipid solvents. The E component reinforcing agent is the solute of the rubber treatment agent 3, and the E component reinforcing agent is trichloroisocyanuric acid.
[0070] Component A is a wear-resistant aggregate composed of a monomer or a mixture of ceramics and silicon carbide, component B is a polyurethane prepolymer, and component C is a matching curing agent.
[0071] This roller remanufacturing method based on seamless glue coating has the following advantages compared with the existing technical solutions:
[0072] 1. The present invention utilizes a multifunctional primer 4 to form an anchoring connection with a metal substrate 1 and can form a molecular bond connection with a polyurethane-based wear-resistant composite material 5; at the same time, the rubber layer on the surface of the old drum modified by the rubber treatment agent 3 can form a molecular bond connection with the polyurethane-based wear-resistant composite material 5;
[0073] 2. The present invention can be used to specifically remanufacture rollers with different forms of damage, such as rollers with worn and thinned rubber layers on the roller surface, rollers with partially exposed metal, rollers with fully exposed metal, rollers with cracked rubber coating gaps, etc.
[0074] 3. The present invention adopts advanced composite material wear-resistant technology. The thinner coating can obtain a longer service life than other technical solutions with thicker rubber, thus improving quality and efficiency;
[0075] 4. The wear-resistant layer of the rubber-coated roller remanufactured by the present invention is a seamless coating, which completely eliminates the structural defect of the rubber-coated roller having gaps, and the reliability is better after remanufacturing;
[0076] 5. The present invention can be used to partially remanufacture the roller according to the specific damage characteristics of the roller lagging;
[0077] 6. The present invention can remanufacture the roller on site in batches according to the specific workload of the roller lagging and the production permission time;
[0078] 7. The present invention can be operated in a narrow space, can operate without loosening the belt, and can retain useful residual glue as much as possible, breaking through the limitations of traditional technology in many aspects;
[0079] 8. The present invention can realize unlimited recycling and remanufacturing;
[0080] 9. The present invention can be used not only for repairing old rollers, but also for manufacturing new rollers.
[0081] In this embodiment, the V2210 rubber treatment agent 3 is composed of a solvent and a strengthening agent. As mentioned above, the solvent is a mixed solvent containing ketone lipid components modified by dichloromethane, which is a non-flammable solvent that meets the control of flammable materials in mines. The strengthening agent is trichloroisocyanuric acid, which changes the polarity of the rubber interface and converts the rubber with poor adhesion into rubber with good adhesion. The use specification is to volatilize naturally for 5-10 minutes after brushing, and then brush the subsequent materials. After the treatment agent evaporates, the rubber interface has no physical thickness;
[0082] V430 multifunctional primer 4 is a kind of polyurethane adhesive that cures at room temperature. After curing, it forms a physical transition layer. It is applied on metal to form an anchor bond with the metal. It is applied on the rubber treatment agent 3 to achieve molecular bond with the rubber. The polyurethane-based wear-resistant composite material 5 is applied on it to form a molecular bond with it, and finally achieves high-strength bonding between the coating and the metal substrate 1 or the rubber substrate 2. Moreover, V430 multifunctional primer 4 can be well bonded with metal, rubber, and polyurethane-based wear-resistant coating at room temperature. Its standard curing process is: room temperature curing for 1-24 hours. When rapid curing is required (such as the on-site remanufacturing mentioned above or the ambient temperature is below 5°C), it is heated at 60-90°C and kept warm for 10-20 minutes. The specific curing method can be selected according to the on-site ambient temperature and the permitted time.
[0083] V7088 polyurethane-based wear-resistant composite material 5 is composed of three components. The matrix phase is component B polyurethane prepolymer and component C curing agent. The reinforcing phase is component A wear-resistant aggregate. The reinforcing phase material can be a monomer or mixture of ceramic, silicon carbide and wear-resistant fiber. The specific reinforcing phase type and parameters can be flexibly selected according to the application conditions. The standard preparation method of V7088 is: first add component A wear-resistant aggregate to component B prepolymer, stir evenly by electric stirring, then add component C curing agent, stir evenly by electric stirring, and the stirring time is generally 25-35s. The curing method and time of V7088 are selected according to the ambient temperature and the permitted time. When there is no limit on the operating time, it can be cured at room temperature for 1-24 hours. When it is required to operate as soon as possible (such as the on-site remanufacturing mentioned above or the ambient temperature is below 5°C), it can be heated at 60-90°C and kept warm for 10-20 minutes before operation;
[0084] In addition, in practical applications, the coating thickness of polyurethane-based wear-resistant composite materials 5 can be selected in a wide range. It is generally believed that the thicker the coating, the longer the service life. Sometimes a thick coating is selected for good appearance, but the thicker the coating, the longer the construction time, which increases the material cost. The optimized thickness is: the coating thickness on rubber is generally 2-5mm, and the coating thickness on metal is generally 6-10mm. The upper limit thickness can be selected as appropriate.
[0085] In this embodiment, the part to be coated with glue can be the area where the rubber layer on the surface of the roller is partially worn but the metal is not exposed, such as Figure 1 As shown, at this time, the damaged surface can be polished with a wire wheel to expose a fresh rubber interface; the area to be coated with glue can also be an area where the rubber layer is severely worn and the metal is exposed, such as Figure 2 , Figure 3 and Figure 4 As shown, at this time, the metal needs to be polished with a flexible emery wheel until the surface oxide layer of the metal substrate 1 is removed to reveal the metallic luster. It should be noted that a wire wheel should be used as little as possible to polish the metal to prevent the grinding debris of the wire wheel from adhering to the surface of the metal substrate 1 and affecting the final gluing effect. At the same time, when performing step S2, the rubber treatment agent 3 should be brushed on the entire area of the rubber and the local area on the metal side of the boundary between the rubber substrate 2 and the metal substrate 1, and then the multifunctional primer 4 should be brushed on the entire rest of the metal and the local area of the rubber at the boundary. Only with this process can the polyurethane-based wear-resistant composite material 5 coating be achieved on both sides of the boundary, with good bonding quality to the substrate (as shown in the following test example).
[0086] In this embodiment, a rubber treating agent 3 is applied on the rubber surface. The rubber treating agent 3 is a common material in the industry. Its function is to chlorinate the surface of the rubber substrate 2 after grinding, so that the rubber substrate 2 has adhesiveness. The rubber treating agent 3 evaporates quickly to meet the specific requirements of online maintenance. Moreover, the function of the rubber treating agent 3 is to change the molecular structure of the rubber surface so that the rubber and the polyurethane-based wear-resistant composite material 5 form a molecular bond connection. In this embodiment and a large amount of practical data, it is shown that the rubber treating agent 3 needs to react with the rubber for 5 minutes after the application to achieve the best chlorination effect. The multifunctional primer 4 performs interface coupling on the surface of the metal substrate 1 after the oxide layer is removed. The multifunctional primer 4 is a common material in the industry. The principle is that the cured multifunctional primer 4 can form a molecular bond with the polyurethane-based wear-resistant composite material 5 while forming an anchoring connection with the metal interface. In this embodiment and in actual application, in order to accelerate the curing speed of the multifunctional primer 4, it is necessary to use an electric blanket or a hot hair dryer to heat it. The embodiment and a large amount of practical data show that the multifunctional primer 4 is best heated at 85°C for 15 minutes. Accelerating the curing speed can fully meet the requirements of online maintenance, but when there is no limit on the startup time during normal temperature maintenance or after maintenance, natural curing for 1-24 hours can be adopted.
[0087] In this embodiment, the polyurethane-based wear-resistant composite material 5 is composed of three components, namely, a matrix phase cast polyurethane prepolymer, a matrix phase curing agent, and a monomer or mixture of an inorganic aggregate in the reinforcing phase. Products with different characteristics can be selected for different working conditions; the reinforcing phase is independently packaged during daily storage and transportation, and is unpacked and prepared when in use, which can maximize the performance stability of the product; the prepared polyurethane-based wear-resistant composite material 5 should be quickly applied to the surface of the roller to be repaired, and constructed in a low-temperature environment or in working conditions where rapid curing is desired to ensure the final actual effect of light, brightness and hardness. The coating of the polyurethane-based wear-resistant composite material 5 is heated at 60-90°C for 10-20 minutes to optimize the curing process; if there is no limit on the start-up time during maintenance at room temperature or after maintenance, the coating can be naturally cured for 1-24 hours.
[0088] More, the Mohs hardness of the wear-resistant aggregate of component A is generally 6-9, which is greater than the hardness of various friction pair materials of the conveying system. It is suitable for the technical requirements of the roller coating material under heavy-load wear, and can play a good role in improving the wear resistance of the roller; in this embodiment and a large amount of practical data, it is shown that when the best hardness is selected as ceramic aggregate and the ceramic is spherical particles, the comprehensive mechanical properties of the entire polyurethane-based wear-resistant composite material 5 coating are the best. The mass ratio of the prepolymer of component B and the curing agent of component C is usually 100:11, and the mass ratio of the BC mixed liquid to component A is 1:1. In actual application, the mass ratio of component B and component C is usually 100:11-100, and the mass ratio of the BC mixed liquid to component A is 1:0.8-1.2. Polyurethane-based wear-resistant composite material 5 products with different characteristics can be selected according to specific working conditions.
[0089] Example 2 - Related Tests
[0090] Test 2.1: Adhesion test of V2210 rubber treatment agent
[0091] Test method: Grind the rubber layer on the surface of the roller, one group without rubber treatment agent 3, and one group with rubber treatment agent 3. Coat the V7088 matrix on the rubber layer without V2210 treatment and the rubber layer treated with V2210. The coating thickness is 3-6mm and the width is 4-6cm. Curing at room temperature for 24 hours, perform 135° peeling and tearing, and observe the fracture characteristics. If the fracture characteristics are interface separation, it is unqualified; if the fracture characteristics are rubber extension greater than 10mm, it is qualified.
[0092] Test data:
[0093]
[0094] Test 2.2: Adhesion test of V430 multifunctional primer to metal
[0095] Test method: Grinding roller is metal, one group is not coated with V430 multifunctional primer 4, and the other group is coated with V430 and cured at room temperature for 24 hours. V7088 matrix phase is coated on metal without V430 treatment and metal treated with V430, with coating thickness of 3-6mm and width of 4-6cm. It is cured at room temperature for 24 hours, and 135° peeling and tearing are performed to observe the fracture characteristics. If the fracture characteristics are interface separation, it is unqualified; if the fracture is matrix phase extension greater than 10mm, it is qualified.
[0096] Test data:
[0097]
[0098]
[0099] Test 2.3: Adhesion test between V430 multifunctional primer and rubber
[0100] Test method: Grind the surface of the drum with a rubber layer, directly apply V430 on one group of rubber and cure it at room temperature for 24 hours, first apply V2210 rubber treatment agent 3 on one group, then apply V430 multifunctional primer 4 and cure it at room temperature for 24 hours, set a comparative example in which one group is first applied V2210 rubber treatment agent 3, then apply V410 metal primer, V410 metal primer is also a product of our company, and like V430 multifunctional primer 4, it has the same adhesion when used on metal substrate 1, then apply V7088 substrate on the three groups of specimens, the coating thickness is 3-6mm, width is 4-6cm, cure it at room temperature for 24 hours, do 135° peeling and tearing, observe the fracture characteristics, the fracture characteristics are interface separation, which is unqualified; the fracture is qualified if the rubber extension is greater than 10mm.
[0101] Test data:
[0102]
[0103] Example 3 - On-site remanufacturing of a drum
[0104] Case 3.1-Severely worn rubber substrate is remanufactured by online glue coating without disassembly (e.g. Figure 5 (shown)
[0105] Working conditions: The redirection drum of a coal washing plant with a capacity of tens of millions of tons has a diameter of 800 and a length of 2 meters. The transport capacity is 90,000 tons / day. The rubber coating of the drum requires a 15-hour shutdown, which is difficult to dispatch.
[0106] Repair plan: The method of the present invention is used for repair in two times. The first time, the machine is stopped for 3 hours, and the machine is operated at the natural opening position of the belt. First, about 40% of the total amount of one side is repaired, and a 3mm wear-resistant protective layer is scraped and applied. The machine is started 30 minutes after the repair. The second time, the machine is stopped for 5 hours, and then the other side is repaired, about 60% of the total amount, and a 3mm wear-resistant protective layer is scraped and applied. The machine is started 30 minutes after the repair. The belt is not loosened during the whole process, and the original rubber lagging is not removed.
[0107] Process flow:
[0108] The rubber substrate was polished with a steel wire wheel, V2210 rubber treatment agent was applied, and then V7088 polyurethane-based wear-resistant composite material was coated. The coating was heated to 85°C, kept warm for 15 minutes, cooled for 10 minutes, and started. The two times took 8 hours, saving 50% of the time compared to the original plan of rubber encapsulation.
[0109] Effect of use: No production interruption, repair in batches, less auxiliary labor, inspection after 90 days of use, little surface wear and tear, and good effect of use.
[0110] Case 3.2 - Partially exposed metal on the drum without disassembly of the machine for partial remanufacturing (e.g. Figure 6 (shown)
[0111] Working conditions: The tail drum of a 30 million ton open-pit mine has a diameter of 1 meter and a length of 2.2 meters. The metal is partially exposed and there are many peripheral additional devices. The workload of replacing the drum is large, the production stoppage time is long, and the space is narrow and it is difficult to coat the drum with glue. The seamless glue coating drum method of the present invention is used for partial remanufacturing.
[0112] Reconstruction plan: Use 5 hours of daily maintenance time to retain the usable rubber on both sides of the metal. At the same time, use rubber treatment agent and multi-functional primer. The metal coating thickness is 20mm and is flush with the rubber on both sides. The ambient temperature is 0℃, and the whole process is heated and cured. Start the machine 30 minutes after repair.
[0113] Process flow:
[0114] The rubber border area was polished with a steel wire wheel, the metal area was polished with an emery wheel, and the rubber area was brushed with V2210 rubber treatment agent, with a brushing range of 10 cm on both sides of the rubber and metal boundary line, and then V430 multifunctional primer was brushed on the metal, and the rubber was brushed to 5 cm from the boundary line, and the hot hair dryer heated V430 to 85℃, kept warm for 15 minutes to make it basically solidified, and V7088 polyurethane-based wear-resistant composite material 5 was prepared according to the specifications, and a thin coating was scraped, and multiple layers were scraped multiple times. The thickness of the coating was flush with the rubber on both sides, and the thickness was about 20mm. The coating was heated to 85℃, kept warm for 15 minutes, cooled for 10 minutes, and started to run. It took 5 hours, which was 35% of the original planned time to replace the roller.
[0115] Effect of use: After 12 months of use, the surface wear is very small and the effect of use is good.
[0116] Case 3.3 - On-site manufacturing of seamless rubber coating rollers (such as Figure 7 (shown)
[0117] Working conditions: A pressure belt roller for iron ore powder transfer at a certain wharf, with a roller diameter of 1.2 meters, a length of 1.4 meters, a belt speed of 4.5 meters per second, a transport capacity of 1,200 tons per hour, and operation 24 hours a day.
[0118] Process flow:
[0119] The metal substrate was polished with an emery wheel, and V430 multifunctional primer was applied and cured at room temperature for 1 hour. V7088 polyurethane-based wear-resistant composite material was prepared according to specifications, with a coating thickness of 6 mm. The coating was cured at room temperature for 24 hours before installation and use.
[0120] Effect of use: After 180 days of use, the surface wear marks were checked and the wear was significantly smaller than that of traditional rubber lagging, and the effect of use was good.
[0121] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A roller remanufacturing method based on seamless rubber coating, which uses a rubber treatment agent, a multifunctional primer and a polyurethane-based wear-resistant composite material to remanufacture the local wear or the whole wear of the roller surface rubber layer on site, wherein the polyurethane-based wear-resistant composite material comprises a component A wear-resistant aggregate, a component B prepolymer and a component C curing agent, the rubber treatment agent comprises a component D solvent and a component E reinforcing agent, and the multifunctional primer is a two-component polyurethane type adhesive, characterized in that: include: S1: Grind the surface of the roller body so that the metal substrate or rubber substrate is exposed to a clean surface; S2: Applying the rubber treatment agent on the surface of the polished rubber substrate to perform chlorination treatment on the rubber, or applying the multifunctional primer on the surface of the polished metal substrate to perform interface coupling treatment on the metal, the rubber treatment agent is naturally volatilized for 5-10 minutes, and the multifunctional primer is heated and cured at 60-90° C. and kept warm for 10-20 minutes to obtain a rubber substrate or metal substrate with good surface adhesion; S3: preparing the polyurethane-based wear-resistant composite material on site, first adding a specified proportion of component A to component B, and stirring evenly by electric means, then adding a specified proportion of component C to the AB mixture, and stirring evenly by electric means; S4: coating the polyurethane-based wear-resistant composite material prepared in S3 on the surface of the rubber substrate modified by the rubber treatment agent in S2 and dried, or coating on the surface of the metal substrate treated by the multifunctional primer in S2 and cured, and the coating thickness of the polyurethane-based wear-resistant composite material is controlled to be 2-20 mm; S5: heating the polyurethane-based wear-resistant composite material coating at 60-90° C. and keeping the temperature for 10-20 minutes until the coating is substantially cured.
2. The roller remanufacturing method based on seamless glue coating according to claim 1 is characterized in that: When performing S2, the rubber treatment agent is first applied to the transition area on both sides of the boundary line between the rubber substrate and the metal substrate on the roller surface, and after the rubber treatment agent is naturally volatilized, the multifunctional primer is applied and heated for curing.
3. The roller remanufacturing method based on seamless glue coating according to claim 2 is characterized in that: The rubber treatment agent applied on the transition area on both sides of the boundary line between the rubber matrix and the metal matrix on the roller surface needs to volatilize naturally for 5-10 minutes, and the multifunctional primer needs to be heated at 60-90°C and kept warm for 10-20 minutes to basically cure the multifunctional primer, and then the polyurethane-based wear-resistant composite material coating is applied and heated and kept warm at 60-90°C for 10-20 minutes to basically cure the polyurethane-based wear-resistant composite material coating.
4. The roller remanufacturing method based on seamless glue coating according to claim 3 is characterized in that: When the ambient temperature is greater than 5°C and there is no time limit, the polyurethane-based wear-resistant composite material coating can also be cured at room temperature for 1-24 hours. When the ambient temperature is less than 5°C and there is a time limit, the polyurethane-based wear-resistant composite material coating is heated at 60-90°C and kept warm for 10-20 minutes for curing.
5. The roller remanufacturing method based on seamless glue coating according to claim 3 is characterized in that: When the ambient temperature is greater than 5°C and there is no time limit, the multifunctional primer can also be cured at room temperature for 1-24 hours. When the ambient temperature is less than 5°C and there is a time limit, the multifunctional primer is heated at 60-90°C and kept warm for 10-20 minutes to cure.
6. The roller remanufacturing method based on seamless glue coating according to claim 3 is characterized in that: The coating method of the polyurethane-based wear-resistant composite material coating is repeated and uniform scraping, and the scraping of the polyurethane-based wear-resistant composite material coating needs to be completed before the polyurethane-based wear-resistant composite material coating loses fluidity.
7. The roller remanufacturing method based on seamless glue coating according to claim 1 is characterized in that: The D component is the solvent of the rubber treatment agent, and the D component is a mixture of dichloromethane, ketones or lipid solvents. The E component reinforcing agent is the solute of the rubber treatment agent, and the E component reinforcing agent is trichloroisocyanuric acid.
8. The roller remanufacturing method based on seamless glue coating according to claim 1 is characterized in that: The component A is a wear-resistant aggregate composed of a monomer or a mixture of ceramics and silicon carbide, the component B is a polyurethane prepolymer, and the component C is a matching curing agent.
Citation Information
Patent Citations
Coating kit and method for repair and / or reconstitution of rubber and / or metal worn areas
WO2024052724A1