Preparation method of composite film for packaging plaster wetting agent
By utilizing multi-layer composite technology and adjusting process parameters in the preparation of composite films for pharmaceutical packaging, the problems of composite film strength and structural uniformity are solved, and more stable packaging performance and a more efficient production process are achieved.
Patent Information
- Application Number
- CN202410782826.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing composite films for pharmaceutical packaging have problems such as low strength and uneven structure, which affects the safety and quality control of pharmaceutical preparations.
A gravure printing machine and a dry laminating machine are used for multi-layer lamination. By adjusting the heating angle and printing rate of the heating device, combined with the curing process, a composite film with good barrier, tensile strength and structural uniformity is formed.
It improves the bonding uniformity and structural stability of the composite film, enhances the firmness and durability of the composite film for packaging, and extends the shelf life of the pharmaceutical. It is suitable for mass production and saves energy consumption.
Smart Images

Figure CN118744547A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite films, and in particular to a method for preparing a composite film for packaging a patch wetting agent. Background Art
[0002] In the existing technology, composite films for pharmaceutical packaging are one of the most commonly used composite films. With the improvement of China's health system and the rapid development of the downstream pharmaceutical industry, the market size of the pharmaceutical packaging materials industry continues to grow. The materials and structural compositions of composite films for pharmaceutical packaging are diverse. These factors will affect the safety of pharmaceutical preparations. In addition, the quality control of composite films is also an important aspect, including barrier properties, tensile strength and appearance, which all need to be identified and controlled.
[0003] Chinese patent publication number: CN115302921A discloses a composite film for drug packaging, including an aluminum foil substrate layer, an inner layer and an outer layer are arranged on both sides of the aluminum foil substrate layer, the inner layer includes: a polypropylene layer, a fresh-keeping layer and a drug attachment layer, the aluminum foil substrate layer is laminated with the polypropylene layer, the polypropylene layer is laminated with the fresh-keeping layer, the fresh-keeping layer is laminated with the drug attachment layer, the surface of the drug attachment layer is provided with a plurality of anti-slip protrusions, and the surface of the outer layer is laminated with a pattern printing layer. It can be seen that the composite film for drug packaging has the problems of low composite film strength and uneven structure. Summary of the invention
[0004] To this end, the present invention provides a method for preparing a composite film for packaging a patch wetting agent, so as to overcome the problems in the prior art.
[0005] To achieve the above-mentioned purpose, the present invention provides a method for preparing a composite film for packaging a patch wetting agent, comprising: using a gravure printing machine to print ink carrying information onto a printing layer; using a dry laminating machine to bond and laminate the printing layer and the barrier layer to form a film to be reinforced, bonding and laminating the reinforcement layer to the surface of the barrier layer of the film to be reinforced to form a film to be sealed, bonding and laminating the heat sealing layer to the surface of the reinforcement layer of the film to be sealed to form a primary composite film; aging the primary composite film to output a finished composite film; and performing strength performance tests on a number of the finished composite films. , to collect the tensile strength of the finished composite film; determine whether the strength of the composite film meets the requirements according to the tensile strength of the finished composite film; if it is determined that the strength of the composite film does not meet the requirements, adjust the heating angle of the heating device of the dry composite machine or determine the structural uniformity of the finished composite film in combination with the surface roughness of the finished composite film; if it is determined that the structural uniformity does not meet the requirements, adjust the heating amplitude of the heating device or adjust the printing speed of the gravure printing machine; wherein the heating angle is the angle between the base films on both sides of the heating roller in the heating device.
[0006] Further, the step of forming the primary composite membrane comprises:
[0007] The barrier layer is compounded, and the barrier layer and the printing layer are respectively introduced into a first substrate unwinding roller and a second substrate unwinding roller of an unwinding device of a dry-type compounding machine to form the film to be strengthened;
[0008] Applying adhesive: applying adhesive to the surface of the barrier layer by means of a glue coating device;
[0009] Heating and drying, heating the barrier layer with the adhesive by a three-stage heating device to evaporate the liquid component of the adhesive;
[0010] Bonding and laminating, bonding and laminating the barrier layer of the dried adhesive and the printing layer by a laminating device;
[0011] The reinforcement layer is compounded, and the film to be reinforced and the reinforcement layer are respectively introduced into the first substrate unwinding roller and the second substrate unwinding roller of the unwinding device of the dry type compounding machine to form the film to be sealed;
[0012] Repeating the adhesive application process, heating and drying process, and bonding and laminating process on the film to be sealed;
[0013] The heat-sealing layer is compounded, and the mold to be sealed and the heat-sealing layer are respectively introduced into the first substrate unwinding roller and the second substrate unwinding roller of the unwinding device of the dry compounding machine to form the primary composite film;
[0014] The adhesive application process, the heating and drying process, and the bonding and laminating process are repeated on the primary composite film.
[0015] Further, judging whether the strength of the composite film meets the requirements according to the tensile strength of the finished composite film includes:
[0016] Comparing the tensile strength of the finished composite film with a preset second tensile strength;
[0017] If the tensile strength of the finished composite film is less than or equal to the preset second tensile strength, it is determined that the strength of the composite film does not meet the requirements; if the tensile strength of the composite film is greater than the second tensile strength, it is determined that the strength of the composite film meets the requirements.
[0018] Furthermore, the step of adjusting the heating angle includes:
[0019] If the tensile strength of the finished composite film is less than or equal to the preset first tensile strength, reducing the heating angle of the heating device;
[0020] Wherein, the adjusted heating angle of the heating device is inversely proportional to the tensile strength of the finished composite film.
[0021] Further, judging whether the structural uniformity of the finished composite film meets the requirements according to the surface roughness of the finished composite film includes:
[0022] Comparing the surface roughness of the finished composite film with a preset first surface roughness and a preset second surface roughness respectively;
[0023] If the tensile strength of the finished composite film is less than the preset second tensile strength and greater than the first tensile strength, it is preliminarily determined that the structural uniformity of the finished composite film does not meet the requirements, and the surface roughness of the finished composite film is obtained;
[0024] If the surface roughness is greater than a preset first surface roughness and less than or equal to a preset second surface roughness, increasing the printing speed of the gravure printing press;
[0025] If the surface roughness is greater than the preset second surface roughness, reducing the heating amplitude;
[0026] Wherein, the preset first surface roughness is smaller than the preset second surface roughness.
[0027] Furthermore, the primary composite membrane has a aging temperature of 50±5° C. and a aging time of not less than 72 hours.
[0028] Furthermore, the thickness of the heat seal layer ranges from 40 to 80 μm, and the density of the adhesive is 3 to 4 g / m 2 / layer.
[0029] Furthermore, the finished composite film comprises: a PET printing layer, an AL barrier layer, a BOPA or PET reinforcement layer, a PE heat sealing layer, ink and an adhesive.
[0030] Furthermore, the PE material is blown to form a heat sealing layer, and then the heat sealing layer is compounded.
[0031] Compared with the prior art, the beneficial effect of the present invention lies in that the method of the present invention sets a processing step for determining whether the tensile strength of the composite film meets the requirements. When the film is towed and rolled by the equipment and there is tension in the film, the adhesive applied on the film will gather in the concave parts and become thicker, thereby causing the bonding uniformity between the film and other composite layers to become lower. When the tensile strength of the composite film does not meet the requirements, the heating angle of the heating device of the dry composite machine is adjusted, and the thickened area on the film is heated with greater intensity and for a longer time to weaken the thickness, thereby achieving improved bonding uniformity between the film and other composite layers. In the processing step for determining whether the structural uniformity of the composite film meets the requirements, if the ink is not smooth during printing, the base film structure of the composite film will be uneven, resulting in a decrease in structural uniformity. The structural uniformity of the composite film is improved by reducing the heating amplitude or increasing the printing rate.
[0032] Furthermore, the method described in the present invention provides a printing layer, a barrier layer, a reinforcing layer and a heat-sealing layer as the base film of the composite film. The barrier layer material has good moisture-proof, anti-oxidation and heat-insulating properties, and protects the medicine in the composite film for packaging. The reinforcing layer material has excellent tensile properties, impact resistance and puncture resistance, and can increase the heat-sealing strength and tensile strength of the composite film. The heat-sealing layer is in direct contact with the medicine in the composite film for packaging and has stability. The heat-sealing layer forms a seal after cooling and solidifying. This seal prevents the entry of foreign substances such as gas, moisture, and dust, maintains the integrity of the composite film, and further achieves the protection effect on the medicine.
[0033] Furthermore, the method of the present invention uses a dry laminating machine to perform three-time lamination on each functional layer of the composite membrane, thereby further achieving a stable and durable composite membrane material structure, being suitable for mass production, improving production efficiency, and saving a lot of energy consumption compared to wet lamination.
[0034] Furthermore, the method of the present invention improves the strength of the composite film by reducing the heating angle of the heating device when the tensile strength of the composite film is less than the first tensile strength, further enhancing the firmness of the composite film for packaging during transportation and storage, reducing the risk of product damage, and effectively isolating the external environment, thereby extending the shelf life of the medicine in the composite film.
[0035] Furthermore, the method of the present invention increases the printing rate when the surface roughness is greater than a preset first surface roughness and less than or equal to a preset second surface roughness, and reduces the heating amplitude when the surface roughness is greater than the preset second surface roughness, thereby improving the uniformity of the composite film structure, making the composite film run more smoothly on a high-speed production line, reducing downtime and production failures caused by uneven material structure, and improving production efficiency.
[0036] Furthermore, the method of the present invention sets the aging temperature to 50±5°C and the aging time to not less than 72 hours, thereby improving the curing effect of the adhesive and allowing the adhesive to form a more stable chemical structure, thereby enhancing the adhesion between the functional layers of the composite film, improving the resistance of the composite film to chemical substances, and improving the overall strength of the composite film, further achieving the enhancement of the barrier effect of the composite film and reducing the probability of delamination, blistering and decreased bonding strength of the composite film during long-term use or storage.
[0037] Furthermore, the method of the present invention sets the thickness of the heat seal layer to 40-80 μm and the density of the adhesive to 3-4 g / m 2 / layer, reducing the negative impact of alcohol in the medicine on the heat sealing layer and adhesive. PE material has better tolerance and chemical stability to alcohol, further realizing the heat sealing effect of the composite film and reducing the risk of medicine leakage. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The process flow chart of the method for preparing the composite film for packaging the wetting agent of the patch according to the embodiment of the present invention;
[0039] Figure 2 This is a primary composite film flow chart of the method for preparing a composite film for packaging a patch wetting agent according to an embodiment of the present invention;
[0040] Figure 3 The composite flow chart of the method for preparing the composite film for packaging the wetting agent of the patch according to the embodiment of the present invention;
[0041] Figure 4 The present invention is a logical flow chart of a method for preparing a composite film for packaging a patch wetting agent according to an embodiment of the present invention. DETAILED DESCRIPTION
[0042] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0043] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0044] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0045] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0046] See also Figure 1 , Figure 2 , Figure 3 as well as Figure 4 As shown, they are respectively Figure 1 The process flow chart, primary composite film flow chart, composite flow chart, and logic flow chart of the method for preparing a composite film for packaging a paste wetting agent according to an embodiment of the present invention are shown in FIG. The method for preparing a composite film for packaging a paste wetting agent according to the present invention comprises:
[0047] Step S1, using a gravure printing machine to print ink carrying information onto a printing layer;
[0048] Step S2, using a dry laminating machine to bond and laminate the printing layer and the barrier layer to form a film to be reinforced, bonding and laminating the reinforcement layer to the surface of the barrier layer of the film to be reinforced to form a film to be sealed, and bonding and laminating the heat sealing layer to the surface of the reinforcement layer of the film to be sealed to form a primary composite film;
[0049] Step S3, aging the primary composite membrane to output a finished composite membrane;
[0050] Step S4, performing strength performance tests on a number of the finished composite films, and collecting the tensile strength of the finished composite films;
[0051] Step S5, judging whether the strength of the composite film meets the requirements according to the tensile strength of the finished composite film;
[0052] Step S6, if it is determined that the strength of the composite film does not meet the requirements, the heating angle of the heating device of the dry composite machine is adjusted or the structural uniformity of the finished composite film is determined in combination with the surface roughness of the finished composite film;
[0053] Step S7, if it is determined that the structural uniformity does not meet the requirements, adjusting the heating amplitude of the heating device or adjusting the printing speed;
[0054] Wherein, the heating angle is the angle between the base films on both sides of the heating roller in the heating device.
[0055] Specifically, the thickness of the film to be reinforced is smaller than the thickness of the film to be sealed, smaller than the thickness of the primary composite film, and smaller than the thickness of the finished composite film.
[0056] Specifically, the standard tensile strength of the finished composite film is 60N / 15mm.
[0057] Specifically, the equipment used to collect the tensile strength of the finished composite film is the AG-1S10KN universal material testing machine and the HST-H heat sealing tester.
[0058] Specifically, the gravure printing machine controls its printing speed to not exceed 350 m / min, and the drying temperature range is set to 40-80°C.
[0059] In implementation, the method of the present invention sets a processing step for determining whether the tensile strength of the composite film meets the requirements. When the film is towed and rolled by the equipment and there is tension in the film, the adhesive applied on the film will gather in the concave parts and become thicker, thereby causing the bonding uniformity between the film and other composite layers to become lower. When the tensile strength of the composite film does not meet the requirements, the heating angle of the heating device of the dry laminator is adjusted, and the thickened area on the film is heated with greater intensity and for a longer time to weaken the thickness, thereby achieving improved bonding uniformity between the film and other composite layers. In the processing step for determining whether the structural uniformity of the composite film meets the requirements, if the ink is not smooth during printing, the base film structure of the composite film will be uneven, resulting in a decrease in structural uniformity. The structural uniformity of the composite film is improved by reducing the heating amplitude or increasing the printing rate.
[0060] Specifically, the structure of the film to be reinforced includes a printing layer and a barrier layer, the structure of the film to be composited includes a printing layer, a barrier layer and a reinforcement layer, and the structure of the primary composite film includes a printing layer, a barrier layer, a reinforcement layer and a heat-sealing layer.
[0061] Specifically, the steps of forming the primary composite membrane include:
[0062] The barrier layer is compounded, and the barrier layer and the printing layer are respectively introduced into a first substrate unwinding roller and a second substrate unwinding roller of an unwinding device of a dry-type compounding machine to form the film to be strengthened;
[0063] Applying adhesive: applying adhesive to the surface of the barrier layer by means of a glue coating device;
[0064] Heating and drying, heating the barrier layer with the adhesive by a three-stage heating device to evaporate the liquid component of the adhesive;
[0065] Bonding and laminating, bonding and laminating the barrier layer of the dried adhesive and the printing layer by a laminating device;
[0066] The reinforcement layer is compounded, and the film to be reinforced and the reinforcement layer are respectively introduced into the first substrate unwinding roller and the second substrate unwinding roller of the unwinding device of the dry type compounding machine to form the film to be sealed;
[0067] Repeating the adhesive application process, heating and drying process, and bonding and laminating process on the film to be sealed;
[0068] The heat-sealing layer is compounded, and the mold to be sealed and the heat-sealing layer are respectively introduced into the first substrate unwinding roller and the second substrate unwinding roller of the unwinding device of the dry compounding machine to form the primary composite film;
[0069] The adhesive application process, the heating and drying process, and the bonding and laminating process are repeated on the primary composite film.
[0070] Specifically, the glue coating device is a glue coating machine inside the dry laminating machine; the heating device is a drying tunnel inside the dry laminating machine, and its heating method is electric heating; the compounding device is a compounding pressure roller inside the dry laminating machine, and the compounding method is extrusion compounding; the unwinding device is an unwinding roller, and the composite film structure is introduced by rotating the unwinding roller.
[0071] In practice, the method of the present invention provides a printing layer, a barrier layer, a reinforcing layer and a heat-sealing layer as the base film of the composite film. The barrier layer material has good moisture-proof, anti-oxidation and heat-insulating properties, and protects the medicine in the composite film for packaging. The reinforcing layer material has excellent tensile properties, impact resistance and puncture resistance, and can increase the heat-sealing strength and tensile strength of the composite film. The heat-sealing layer is in direct contact with the medicine in the composite film for packaging and has stability. The heat-sealing layer forms a seal after cooling and solidifying. This seal prevents the entry of foreign substances such as gas, moisture, and dust, maintains the integrity of the composite film, and further achieves the protection effect on the medicine.
[0072] In practice, the method of the present invention uses a dry laminating machine to perform three laminations on the functional layers of the composite membrane, thereby further achieving a stable and durable composite membrane material structure, being suitable for mass production, improving production efficiency, and saving a lot of energy consumption compared to wet lamination.
[0073] Specifically, whether the strength of the composite film meets the requirements is determined based on the tensile strength of the finished composite film, including:
[0074] Comparing the tensile strength of the finished composite film with a preset second tensile strength;
[0075] If the tensile strength of the finished composite film is less than or equal to the preset second tensile strength, it is determined that the strength of the composite film does not meet the requirements; if the tensile strength of the composite film is greater than the second tensile strength, it is determined that the strength of the composite film meets the requirements.
[0076] Specifically, the step of adjusting the heating angle includes:
[0077] Comparing the tensile strength of the finished composite film with the preset first tensile strength and the preset second tensile strength respectively;
[0078] If the tensile strength of the finished composite film is less than or equal to the preset first tensile strength, reducing the heating angle of the heating device;
[0079] Wherein, the adjusted heating angle of the heating device is inversely proportional to the tensile strength of the finished composite film.
[0080] Specifically, the heating angle is adjusted by adjusting the height difference between the heating rollers.
[0081] In practice, the preset first tensile strength is generally [38N / 15mm, 48N / 15mm], and the preset second tensile strength is generally [50N / 15mm, 75N / 15mm].
[0082] Optionally, a preferred embodiment of the preset first tensile strength is 44 N / 15 mm, and a preferred embodiment of the preset second tensile strength is 60 N / 15 mm.
[0083] During implementation, when the tensile strength of the finished composite film is 5N / 15mm lower than the preset first tensile strength, the heating angle of the heating device is reduced by 0.1 times compared with the current heating angle. When the difference between the tensile strength of the finished composite film and the preset first tensile strength exceeds 5N / 15mm, the heating angle of the heating device is reduced by 4° for every 1N / 15mm difference. For example, when the tensile strength of the finished composite film is 36N / 15mm, the heating angle of the heating device is reduced to 180°×(1-0.1)-4°×3=150°.
[0084] In implementation, the method of the present invention improves the strength of the composite film by reducing the heating angle of the heating device when the tensile strength of the composite film is less than the first tensile strength, further enhancing the firmness of the composite film for packaging during transportation and storage, reducing the risk of product damage, and effectively isolating the external environment, thereby extending the shelf life of the medicine in the composite film.
[0085] Specifically, judging whether the structural uniformity of the finished composite film meets the requirements according to the surface roughness of the finished composite film includes:
[0086] Comparing the surface roughness of the finished composite film with a preset first surface roughness and a preset second surface roughness respectively;
[0087] If the tensile strength of the finished composite film is less than the preset second tensile strength and greater than the first tensile strength, it is preliminarily determined that the structural uniformity of the finished composite film does not meet the requirements, and the surface roughness of the finished composite film is obtained;
[0088] If the surface roughness is greater than a preset first surface roughness and less than or equal to a preset second surface roughness, increasing the printing speed of the gravure printing press;
[0089] If the surface roughness is greater than the preset second surface roughness, reducing the heating amplitude;
[0090] Wherein, the preset first surface roughness is smaller than the preset second surface roughness.
[0091] Specifically, three groups of ovens are arranged in the heating device of the dry compound machine in sequence, and the heating ranges thereof are 50-65°C, 65-85°C, and 75-90°C respectively.
[0092] In implementation, the preset first surface roughness is generally [0.05um, 0.075um], and the preset second surface roughness is generally [0.08um, 0.1um].
[0093] Optionally, a preferred embodiment of the preset first surface roughness is 0.06 um, and a preferred embodiment of the preset second surface roughness is 0.09 um.
[0094] In practice, for every 0.01um difference between the surface roughness of the finished composite film and the preset second surface roughness, the heating amplitude is reduced from 15°C by 3°C. For example, when the surface roughness of the finished composite film is 0.11um, the heating amplitude is reduced to 9°C.
[0095] In practice, the faster the printing speed, the lower the thickness of the ink attached to the printing layer per unit area. For every 0.01um difference between the surface roughness of the finished composite film and the preset first surface roughness, the speed of the gravure printing machine is increased by 15m / min.
[0096] In implementation, the method of the present invention increases the printing rate when the surface roughness is greater than a preset first surface roughness and less than or equal to a preset second surface roughness, and reduces the heating amplitude when the surface roughness is greater than the preset second surface roughness, thereby improving the uniformity of the composite film structure, making the composite film run more smoothly on a high-speed production line, reducing downtime and production failures caused by uneven material structure, and improving production efficiency.
[0097] Specifically, the primary composite membrane has an aging temperature of 50±5° C. and an aging time of not less than 72 hours.
[0098] In practice, the method of the present invention sets the aging temperature to 50±5°C and the aging time to not less than 72 hours, thereby improving the curing effect of the adhesive and allowing the adhesive to form a more stable chemical structure, thereby enhancing the adhesion between the functional layers of the composite film, improving the resistance of the composite film to chemical substances, and improving the overall strength of the composite film, further achieving the enhancement of the barrier effect of the composite film and reducing the probability of delamination, bubbling and decreased bonding strength of the composite film during long-term use or storage.
[0099] Specifically, the thickness of the heat seal layer ranges from 40 to 80 μm, and the density of the adhesive is 3 to 4 g / m 2 / layer.
[0100] Preferably, the preferred embodiment of the heat seal layer is 60um.
[0101] Specifically, the components of the finished composite film include: a PET printing layer, an AL barrier layer, a BOPA or PET reinforcement layer, a PE heat sealing layer, ink and an adhesive.
[0102] Specifically, the adhesive includes solvent-based polyurethane adhesive, RP-05 adhesive, and solvent-free adhesive.
[0103] In practice, the thickness of the PET printing layer is set to 12-20um, the thickness of the AL barrier layer is set to 7-9um, and the thickness of the BOPA reinforcement layer is set to 15um. If PET is used as the reinforcement layer, the thickness is set to 12-20um, the thickness of the PE heat sealing layer is set to 40-80um, the ink density is 0-3g / ㎡, and the density of the adhesive is set to 3-4g / m 2 / layer.
[0104] Specifically, the PE material is blown to form a heat sealing layer, and then the heat sealing layer is compounded.
[0105] In practice, the method of the present invention sets the thickness of the heat seal layer to 40-80 μm and the density of the adhesive to 3-4 g / m 2 / layer, reducing the negative impact of alcohol in the medicine on the heat sealing layer and adhesive. PE material has better tolerance and chemical stability to alcohol, further realizing the heat sealing effect of the composite film and reducing the risk of medicine leakage.
[0106] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
Claims
1. A method for preparing a composite film for packaging a patch wetting agent, characterized in that: The following steps are involved: Printing ink carrying information onto a substrate using a gravure printing press; Using a dry laminating machine to bond and laminate the printing layer and the barrier layer to form a film to be reinforced, bonding and laminating the reinforcement layer to the surface of the barrier layer of the film to be reinforced to form a film to be sealed, and bonding and laminating the heat sealing layer to the surface of the reinforcement layer of the film to be sealed to form a primary composite film; Curing the primary composite film to output a finished composite film; Conducting strength performance tests on a number of the finished composite films to collect the tensile strength of the finished composite films; Determining whether the strength of the composite film meets the requirements according to the tensile strength of the finished composite film; If it is determined that the strength of the composite film does not meet the requirements, the heating angle of the heating device of the dry composite machine is adjusted or the structural uniformity of the finished composite film is determined in combination with the surface roughness of the finished composite film; If it is determined that the structural uniformity does not meet the requirements, adjusting the heating amplitude of the heating device or adjusting the printing speed of the gravure printing press; Wherein, the heating angle is the angle between the base films on both sides of the heating roller in the heating device.
2. The method for preparing the composite film for packaging the patch wetting agent according to claim 1, wherein: The steps of forming the primary composite membrane include: The barrier layer is compounded, and the barrier layer and the printing layer are respectively introduced into a first substrate unwinding roller and a second substrate unwinding roller of an unwinding device of a dry-type compounding machine to form the film to be strengthened; Applying adhesive: applying adhesive to the surface of the barrier layer by means of a glue coating device; Heating and drying, heating the barrier layer with the adhesive by a three-stage heating device to evaporate the liquid component of the adhesive; Bonding and laminating, bonding and laminating the barrier layer of the dried adhesive and the printing layer by a laminating device; The reinforcement layer is compounded, and the film to be reinforced and the reinforcement layer are respectively introduced into the first substrate unwinding roller and the second substrate unwinding roller of the unwinding device of the dry type compounding machine to form the film to be sealed; Repeating the adhesive application process, heating and drying process, and bonding and laminating process on the film to be sealed; The heat-sealing layer is compounded, and the mold to be sealed and the heat-sealing layer are respectively introduced into the first substrate unwinding roller and the second substrate unwinding roller of the unwinding device of the dry compounding machine to form the primary composite film; The adhesive application process, the heating and drying process, and the bonding and laminating process are repeated on the primary composite film.
3. The method for preparing the composite film for packaging a patch wetting agent according to claim 1, wherein: The tensile strength of the finished composite film is used to determine whether the strength of the composite film meets the requirements, including: Comparing the tensile strength of the finished composite film with a preset second tensile strength; If the tensile strength of the finished composite film is less than or equal to the preset second tensile strength, it is determined that the strength of the composite film does not meet the requirements; if the tensile strength of the composite film is greater than the second tensile strength, it is determined that the strength of the composite film meets the requirements.
4. The method for preparing the composite film for packaging the patch wetting agent according to claim 3, characterized in that, The step of adjusting the heating angle comprises: Comparing the tensile strength of the finished composite film with a preset first tensile strength; If the tensile strength of the finished composite film is less than or equal to the preset first tensile strength, reducing the heating angle of the heating device; Wherein, the adjusted heating angle of the heating device is inversely proportional to the tensile strength of the finished composite film.
5. The method for preparing the composite film for packaging a patch wetting agent according to claim 1, characterized in that: Judging whether the structural uniformity of the finished composite film meets the requirements according to the surface roughness of the finished composite film includes: Comparing the surface roughness of the finished composite film with a preset first surface roughness and a preset second surface roughness respectively; If the tensile strength of the finished composite film is less than the preset second tensile strength and greater than the first tensile strength, it is preliminarily determined that the structural uniformity of the finished composite film does not meet the requirements, and the surface roughness of the finished composite film is obtained; If the surface roughness is greater than a preset first surface roughness and less than or equal to a preset second surface roughness, increasing the printing speed of the gravure printing press; If the surface roughness is greater than the preset second surface roughness, reducing the heating amplitude; Wherein, the preset first surface roughness is smaller than the preset second surface roughness.
6. The method for preparing the composite film for packaging a patch wetting agent according to claim 5, characterized in that: The surface roughness is inversely proportional to the printing rate and inversely proportional to the heating amplitude.
7. The method for preparing the composite film for packaging a patch wetting agent according to claim 1, characterized in that: The aging temperature of the primary composite membrane is 50±5° C., and the aging time is not less than 72 hours.
8. The method for preparing the composite film for packaging a patch wetting agent according to claim 1, characterized in that: The thickness of the heat seal layer is in the range of 40-80um, and the density of the adhesive is 3-4g / m 2 / layer.
9. The method for preparing the composite film for packaging a patch wetting agent according to claim 1, characterized in that: The finished composite film comprises: a PET printing layer, an AL barrier layer, a BOPA or PET reinforcement layer, a PE heat sealing layer, ink and an adhesive.
10. The method for preparing the composite film for packaging a patch wetting agent according to claim 1, characterized in that: The PE material is blown to form a heat sealing layer and then the heat sealing layer is compounded.