Special plastic concrete for circulating fluidized bed boiler and preparation method thereof
By using binders such as vinyl siloxane, stearyl acrylate and styrene in the refractory layer of the circulating fluidized bed boiler, and using the pre-emulsification semi-continuous emulsion method to form a core-shell structure polyacrylate Resin solves the problem of insufficient performance of the refractory layer under high temperature and pressure, and significantly improves its heat insulation, pressure resistance and high temperature resistance properties.
Patent Information
- Application Number
- CN202410732806.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-07
AI Technical Summary
The refractory layer of existing circulating fluidized bed boilers is prone to wear, erosion, cracks and other problems under high temperatures and pressures, resulting in insufficient thermal insulation, compressive strength and high temperature resistance, affecting the safety and service life of the system.
Vinyl siloxane and stearyl acrylate functional monomers are used as binders, combined with styrene to improve the high-temperature resistance of the binder, and polymerized through pre-emulsification semi-continuous emulsion method to form a core-shell structure. Acrylic thermoplastic resin is used as a binder to enhance the compressive strength and thermal conductivity of the binder.
Significantly improve the maximum operating temperature, compressive strength, thermal conductivity and heating permanent linear change performance of plastic concrete for circulating fluidized bed boilers, extend the service life of the refractory layer and enhance its heat insulation, pressure resistance and high temperature resistance properties.
Smart Images

Figure BDA0004880734680000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and particularly relates to a special plastic concrete for a circulating fluidized bed boiler and a preparation method thereof. Background Art
[0002] The circulating fluidized bed boiler in a power plant is a medium-sized or large boiler that provides steam in a power plant. It needs to withstand high temperatures above 150°C. The inner wall and top of the boiler are paved with refractory bricks, and plastic concrete is coated on the surface. After drying and curing, it forms a refractory layer. During use, the airflow pressure and other factors can easily cause the surface of the refractory layer to wear, erosion and damage. Therefore, how to improve its thermal insulation, compressive strength, and fire resistance determines the safety, stability and service life of the entire system.
[0003] Generally, by adding expansion agents, the volume shrinkage caused by the binder during the use of the boiler is offset, cracks are prevented during use, and the high-temperature performance and room-temperature compressive strength of the product are improved. By adding engineering fibers to form a multi-directional support system, the directional stress of the mud is dispersed, the occurrence and development of primary cracks in the mud are prevented, and the number of primary microcracks is eliminated or reduced. At the same time, by utilizing the strength of the engineering fiber itself, the fiber is evenly dispersed in the mud and forms an anchoring effect, which can absorb a certain amount of destructive energy during the use of the boiler and reduce the possibility of cracks in the furnace lining. However, the uneven dispersion of components such as engineering fibers and expansion agents in plastic concrete and the insufficient bonding force of the binder can easily lead to insufficient compressive strength, thermal insulation and high temperature resistance. Summary of the invention
[0004] In order to overcome the problems existing in the prior art, the purpose of the present invention is to provide a special plastic concrete for circulating fluidized bed boilers and a preparation method thereof. The use of vinyl siloxane and octadecyl acrylate functional monomers in the binder can improve the bonding strength, and the use of styrene can improve the high temperature resistance of the binder, thereby improving the compressive strength, heat insulation, high temperature resistance and durability. In addition, by using a pre-emulsified semi-continuous emulsion polymerization method, the polyester fiber is first coated with a portion of the monomer solution to form a core layer, and then the monomer solution is added dropwise to prepare a shell layer, and a polyacrylate thermoplastic resin with a core-shell structure is obtained as a binder, which can improve its maximum use temperature, compressive strength, thermal conductivity, and heating permanent linear change performance, thereby improving the heat insulation, compressive strength and high temperature resistance.
[0005] The objective of the present invention is achieved through the following technical scheme: a special plastic concrete for circulating fluidized bed boiler, the raw materials of which contain 20-30 parts of perlite, 30-35 parts of fly ash, 5-12 parts of silicon powder, 3-5 parts of expansion agent, 5-12 parts of coupling agent, 24-30 parts of binder, 1-3 parts of engineering fiber, 1.5-2 parts of water reducer and 1-5 parts of curing agent.
[0006] Preferably, the particle size of the perlite is ≤3 mm; and the particle size of the expander is ≤80 μm.
[0007] Preferably, the expansion agent is silica powder; the water reducing agent is industrial grade sodium tripolyphosphate; and the curing agent is industrial grade sodium fluorosilicate powder.
[0008] Preferably, the coupling agent is a silane coupling agent.
[0009] Preferably, the engineering fiber is polyester fiber with a fiber length of 5 mm to 20 mm and a fiber diameter of 15 μm to 40 μm.
[0010] Preferably, the binder is a polyacrylate thermoplastic resin with a core-shell structure, which is formed by in-situ polymerization in the presence of polyester fibers using methyl methacrylate, styrene, dodecyl acrylate and vinyl siloxane as raw materials.
[0011] Preferably, the preparation method of the binder comprises:
[0012] Step 1, 5-10 parts of KH570 modified polyester fiber, 100 parts of deionized water, and 2-5 parts of initiator azobisisobutyronitrile are mixed to prepare solution A;
[0013] Step 2: 25-60 parts of methyl methacrylate, 5-18 parts of styrene, 5-10 parts of octadecyl acrylate, 5-10 parts of vinyl siloxane, 5-10 parts of emulsifier, and 100 parts of deionized water are mixed, and solution B is prepared by ultrasonic stirring;
[0014] Step three, add solution A and 1 / 5 of solution B into the reactor, stir evenly, and heat to 50-80°C, react for 0.5-1h to form a core emulsion, continue to add the remaining solution B, the addition time is 4-6h, after the addition is completed, add 0.5-1 part of the redox initiator, continue to react for 1-2h, cool to room temperature, and obtain a polyacrylate thermoplastic resin with a core-shell structure.
[0015] Preferably, the vinyl siloxane, emulsifier, and redox initiator may be common compounds in this field.
[0016] Preferably, the mass ratio of solution A to solution B is 1:10-50.
[0017] Preferably, the polyester fiber used in the KH570 modified polyester fiber has a length of 3 mm to 5 mm and a fiber diameter of 10 μm to 15 μm.
[0018] A method for preparing plastic concrete for circulating fluidized bed boilers comprises the following reaction steps:
[0019] Step 1, weigh the raw materials according to the ratio;
[0020] Step 2: Mix perlite, fly ash, silica powder, expansion agent and coupling agent at 10-35°C for 3-10 minutes to obtain mixture A for later use; mix binder, engineering fiber, water reducer and curing agent and stir for 3-10 minutes to obtain mixture B for later use; then mix mixture A with mixture B and stir evenly to obtain plastic concrete for circulating fluidized bed boiler.
[0021] The beneficial effects of the present invention are:
[0022] 1. The special plastic concrete for circulating fluidized bed boilers of the present invention adopts vinyl siloxane and octadecyl acrylate functional monomers in the binder to improve the bonding strength, and adopts styrene to improve the high temperature resistance of the binder, thereby improving the compressive strength, high temperature resistance and durability of the special plastic concrete for circulating fluidized bed boilers.
[0023] 2. The binder of the present invention prepares a polyacrylate thermoplastic resin with a core-shell structure as a binder by in-situ adding polyester fibers, which can make the polyester fibers better dispersed in the plastic concrete composition, so that the binder, engineering fiber, perlite, fly ash, silica powder, expansion agent and other components in the composition are evenly dispersed and fully play their roles, thereby improving the maximum use temperature, compressive strength, thermal conductivity, heating permanent linear change performance, and then improving the thermal insulation, compressive strength and high temperature resistance of the plastic concrete specially used for circulating fluidized bed boilers.
[0024] 3. The binder of the present invention adopts a pre-emulsified semi-continuous emulsion polymerization method. First, the polyester fiber is coated with a part of the monomer solution to form a core layer, and then the monomer solution is added dropwise to prepare the shell layer. The polyester fiber can be well locked in the core layer, and a layer of polyacrylate polymer is in situ polymerized and coated on the surface of the core layer, so that the polyester fiber is fully and evenly dispersed in the polyacrylate binder, and an island structure is formed in the special plastic concrete composition for circulating fluidized bed boilers, thereby further improving the compressive strength and high temperature resistance of the special plastic concrete for circulating fluidized bed boilers. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The present invention is further explained below in conjunction with specific implementation modes.
[0027] Preparation Example 1
[0028] A polyacrylate thermoplastic resin binder is formed by in-situ polymerization in the presence of polyester fibers using methyl methacrylate, styrene, dodecyl acrylate, and vinyl siloxane as raw materials. Specifically, the reaction steps are as follows:
[0029] Step 1: 45 parts of KH570 modified polyester fiber, 100 parts of deionized water, and 2 parts of initiator azobisisobutyronitrile are mixed to prepare solution A;
[0030] Step 2: 30 parts of methyl methacrylate, 8 parts of styrene, 5 parts of octadecyl acrylate, 5 parts of KH570, 8 parts of emulsifier SDS, and 100 parts of deionized water are mixed, and solution B is prepared by ultrasonic stirring;
[0031] Step 3, add solution A and 1 / 5 of solution B to the reactor, ultrasonically homogenize, stir and heat to 65°C, react for 0.5h, form a core emulsion, continue to drip the remaining solution B, the dripping time is 5h, and after the dripping is completed, add 0.8 parts of redox initiator potassium sulfate / sodium sulfite, continue to react for 1.5h, cool to room temperature, and obtain a polyacrylate thermoplastic resin with a core-shell structure. The mass ratio of solution A to solution B is 1:10. The polyester fiber used in the KH570 modified polyester fiber has a length of 3mm and a fiber diameter of 10μm.
[0032] Preparation Example 2
[0033] A polyacrylate thermoplastic resin binder is formed by in-situ polymerization of methyl methacrylate as a raw material in the presence of polyester fibers. Specifically, the reaction steps are as follows:
[0034] Step 1: 45 parts of KH570 modified polyester fiber, 100 parts of deionized water, and 2 parts of initiator azobisisobutyronitrile are mixed to prepare solution A;
[0035] Step 2: 48 parts of methyl methacrylate, 8 parts of emulsifier SDS, and 100 parts of deionized water are mixed, and solution B is prepared by ultrasonic stirring;
[0036] Step 3, add solution A and 1 / 5 of solution B to the reactor, ultrasonically homogenize, stir and heat to 65°C, react for 0.5h, form a core emulsion, continue to drip the remaining solution B, the dripping time is 5h, and after the dripping is completed, add 0.8 parts of redox initiator potassium sulfate / sodium sulfite, continue to react for 1.5h, cool to room temperature, and obtain a polyacrylate thermoplastic resin with a core-shell structure. The mass ratio of solution A to solution B is 1:10. The polyester fiber used in the KH570 modified polyester fiber has a length of 3mm and a fiber diameter of 10μm.
[0037] Preparation Example 3
[0038] A polyacrylate thermoplastic resin binder is formed by in-situ polymerization in the presence of polyester fibers using methyl methacrylate, styrene, dodecyl acrylate, and vinyl siloxane as raw materials. Specifically, the reaction steps are as follows:
[0039] Step 1: 45 parts of KH570 modified polyester fiber, 100 parts of deionized water, and 2 parts of initiator azobisisobutyronitrile are mixed to prepare solution A;
[0040] Step 2: 30 parts of methyl methacrylate, 8 parts of styrene, 5 parts of octadecyl acrylate, 5 parts of KH570, 8 parts of emulsifier SDS, and 100 parts of deionized water are mixed, and solution B is prepared by ultrasonic stirring;
[0041] Step 3, add solution A and solution B to the reactor, stir evenly with ultrasonic stirring, stir and heat to 65°C, react for 5 hours, then add 0.8 parts of redox initiator potassium sulfate / sodium sulfite, continue to react for 1.5 hours, cool to room temperature, and obtain polyacrylate thermoplastic resin. The mass ratio of solution A to solution B is 1:10. The polyester fiber used in the KH570 modified polyester fiber has a length of 3 mm and a fiber diameter of 10 μm.
[0042] Preparation Example 4
[0043] A polyacrylate thermoplastic resin binder is formed by in-situ polymerization of methyl methacrylate, styrene, dodecyl acrylate and vinyl siloxane as raw materials. Specifically, the following reaction steps are included:
[0044] Step 1, 30 parts of methyl methacrylate, 8 parts of styrene, 5 parts of octadecyl acrylate, 5 parts of KH570, 8 parts of emulsifier SDS, and 100 parts of deionized water are mixed, and solution B is prepared by ultrasonic stirring;
[0045] Step 3, add solution B to the reactor, stir and heat to 65°C, react for 5 hours, then add 0.8 parts of redox initiator potassium persulfate / sodium sulfite, continue to react for 1.5 hours, cool to room temperature, and obtain polyacrylate thermoplastic resin.
[0046] Example 1
[0047] A special plastic concrete for a circulating fluidized bed boiler comprises 20 parts of perlite, 35 parts of fly ash, 5 parts of silicon micropowder, 3 parts of expansion agent, 28 parts of binder, 1 part of engineering fiber, 1.5 parts of water reducing agent, 1 part of curing agent and 5 parts of coupling agent.
[0048] The particle size of the perlite is 2 mm; the particle size of the expander is 35 μm. The expander is silica powder; the water reducer is industrial grade sodium tripolyphosphate; and the curing agent is industrial grade sodium fluorosilicate powder. The engineering fiber is polyester fiber with a fiber length of 5 mm and a fiber diameter of 30 μm. The binder is the polyacrylate thermoplastic resin with a core-shell structure prepared in Preparation Example 1.
[0049] The preparation method comprises the following reaction steps:
[0050] Step 1, weigh the raw materials according to the ratio;
[0051] Step 2: At 25°C, mix perlite, fly ash, silica powder, expansion agent and coupling agent and stir for 5 minutes to obtain mixture A for use; mix binder, engineering fiber, water reducer and curing agent and stir for 5 minutes to obtain mixture B for use; then mix mixture A with mixture B and stir evenly to obtain plastic concrete for circulating fluidized bed boilers.
[0052] Comparative Example 1
[0053] A special plastic concrete for a circulating fluidized bed boiler comprises 20 parts of perlite, 35 parts of fly ash, 5 parts of silicon micropowder, 3 parts of expansion agent, 28 parts of binder, 1 part of engineering fiber, 1.5 parts of water reducing agent, 1 part of curing agent and 5 parts of coupling agent.
[0054] The particle size of the perlite is 2 mm; the particle size of the expander is 35 μm. The expander is silica powder; the water reducer is industrial grade sodium tripolyphosphate; and the curing agent is industrial grade sodium fluorosilicate powder. The engineering fiber is polyester fiber with a fiber length of 5 mm and a fiber diameter of 30 μm. The binder is the polyacrylate thermoplastic resin with a core-shell structure prepared in Preparation Example 2.
[0055] The preparation method comprises the following reaction steps:
[0056] Step 1, weigh the raw materials according to the ratio;
[0057] Step 2: At 25°C, mix perlite, fly ash, silica powder, expansion agent and coupling agent and stir for 5 minutes to obtain mixture A for use; mix binder, engineering fiber, water reducer and curing agent and stir for 5 minutes to obtain mixture B for use; then mix mixture A with mixture B and stir evenly to obtain plastic concrete for circulating fluidized bed boilers.
[0058] Example 2
[0059] A special plastic concrete for a circulating fluidized bed boiler comprises 20 parts of perlite, 35 parts of fly ash, 5 parts of silicon micropowder, 3 parts of expansion agent, 28 parts of binder, 1 part of engineering fiber, 1.5 parts of water reducing agent, 1 part of curing agent and 5 parts of coupling agent.
[0060] The particle size of the perlite is 2 mm; the particle size of the expander is 35 μm. The expander is silica powder; the water reducer is industrial grade sodium tripolyphosphate; and the curing agent is industrial grade sodium fluorosilicate powder. The engineering fiber is polyester fiber with a fiber length of 5 mm and a fiber diameter of 30 μm. The binder is the polyacrylate thermoplastic resin prepared in Preparation Example 3.
[0061] The preparation method comprises the following reaction steps:
[0062] Step 1, weigh the raw materials according to the ratio;
[0063] Step 2: At 25°C, mix perlite, fly ash, silica powder, expansion agent and coupling agent and stir for 5 minutes to obtain mixture A for use; mix binder, engineering fiber, water reducer and curing agent and stir for 5 minutes to obtain mixture B for use; then mix mixture A with mixture B and stir evenly to obtain plastic concrete for circulating fluidized bed boilers.
[0064] Comparative Example 2
[0065] A special plastic concrete for a circulating fluidized bed boiler comprises 20 parts of perlite, 35 parts of fly ash, 5 parts of silicon micropowder, 3 parts of expansion agent, 28 parts of binder, 4 parts of engineering fiber, 1.5 parts of water reducing agent, 1 part of curing agent and 5 parts of coupling agent.
[0066] The particle size of the perlite is 2 mm; the particle size of the expander is 35 μm. The expander is silica powder; the water reducer is industrial grade sodium tripolyphosphate; and the curing agent is industrial grade sodium fluorosilicate powder. The engineering fiber is polyester fiber with a fiber length of 5 mm and a fiber diameter of 30 μm. The binder is the polyacrylate thermoplastic resin prepared in Preparation Example 4.
[0067] The preparation method comprises the following reaction steps:
[0068] Step 1, weigh the raw materials according to the ratio;
[0069] Step 2: At 25°C, mix perlite, fly ash, silica powder, expansion agent and coupling agent and stir for 5 minutes to obtain mixture A for use; mix binder, engineering fiber, water reducer and curing agent and stir for 5 minutes to obtain mixture B for use; then mix mixture A with mixture B and stir evenly to obtain plastic concrete for circulating fluidized bed boilers.
[0070] Performance Testing
[0071] For the plastic concrete for circulating fluidized bed boilers obtained in Example 1-2 and Comparative Example 1-2, samples were prepared according to the provisions of DL / T777-2012, and the maximum operating temperature, compressive strength, thermal conductivity, and heating permanent linear change performance were tested, and compared with the technical indicators of amorphous insulating refractory material Type II as shown in the following table.
[0072] Table 1 Plastic concrete for circulating fluidized bed boiler
[0073]
[0074] From the comparison between Example 1 and Comparative Example 1, it can be seen that the maximum operating temperature, compressive strength, thermal conductivity and heating permanent linear change performance of the plastic concrete specially used for circulating fluidized bed boilers in Example 1 are significantly improved. This may be due to the use of octadecyl acrylate and vinylsiloxane functional monomers in the preparation of the binder, which can improve the bonding strength, and the use of styrene can increase the high temperature resistance, thereby improving the compressive strength, high temperature resistance and durability.
[0075] From the comparison of Examples 1 and 2 and Comparative Example 2, it can be seen that the in-situ addition of polyester fibers in the preparation of the binder for the special plastic concrete for circulating fluidized bed boilers of the present invention can improve the maximum use temperature, compressive strength, thermal conductivity, and heating permanent linear change performance of the plastic concrete, thereby improving its thermal insulation, compressive strength and high temperature resistance. This may be because the in-situ added polyester fibers can be better dispersed in the plastic concrete composition, so that the binder, engineering fiber, perlite, fly ash, silica powder, expansion agent and other components in the composition are evenly dispersed and fully play their role, thereby improving its thermal insulation, compressive strength and high temperature resistance.
[0076] Comparison between Examples 1 and 2 shows that the maximum use temperature, compressive strength, thermal conductivity, and heating permanent linear change performance of the plastic concrete for circulating fluidized bed boilers are improved as the degree of coating of the polyester fiber by the polyacrylate binder increases. This may be because Example 1 adopts pre-emulsified semi-continuous emulsion polymerization, firstly coats the polyester fiber with 1 / 5 of the monomer solution to form a core layer, and then drips the monomer solution to prepare the shell layer, which can well lock the polyester fiber in the core layer, and in-situ polymerize and coat a layer of polyacrylate polymer on the surface of the core layer, so that the polyester fiber is fully and evenly dispersed in the polyacrylate binder and is heated in the circulating fluidized bed. An island structure is formed in the boiler-specific plastic concrete composition, which further improves the compressive strength, high temperature resistance, thermal insulation and durability. In Example 2, the polyester fiber and the monomer solution are directly mixed and polymerized, and the possibility of forming a shell layer on the surface of the polyester fiber is reduced. It is more likely to form an interpenetrating network structure with acrylate through the coupling agent on its surface. Compared with Example 1, the dispersion of other components such as perlite, fly ash, silica powder, expansion agent, and engineering fiber is poor, so the maximum use temperature, compressive strength, thermal conductivity, and heating permanent line change performance are cracked as the degree of coating of the polyacrylate binder on the polyester fiber decreases.
[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A plastic concrete specially used for circulating fluidized bed boiler, characterized in that: The raw materials include: 20-30 parts of perlite, 30-35 parts of fly ash, 5-12 parts of silicon powder, 3-5 parts of expansion agent, 5-12 parts of coupling agent, 24-30 parts of binder, 1-3 parts of engineering fiber, 1.5-2 parts of water reducer and 1-5 parts of curing agent; the binder is a polyacrylate thermoplastic resin with a core-shell structure, which is formed by in-situ polymerization in the presence of modified polyester fiber with methyl methacrylate, styrene, dodecyl acrylate and vinyl siloxane as raw materials.
2. The special plastic concrete for circulating fluidized bed boiler according to claim 1 is characterized in that: The modified polyester fiber is KH570 modified polyester fiber.
3. The special plastic concrete for circulating fluidized bed boiler according to claim 1 is characterized in that: The preparation method of the binder comprises: Step 1, 5-10 parts of KH570 modified polyester fiber, 100 parts of deionized water, and 2-5 parts of initiator azobisisobutyronitrile are mixed to prepare solution A; Step 2: 25-60 parts of methyl methacrylate, 5-18 parts of styrene, 5-10 parts of octadecyl acrylate, 5-10 parts of vinyl siloxane, 5-10 parts of emulsifier, and 100 parts of deionized water are mixed, and solution B is prepared by ultrasonic stirring; Step three, add solution A and 1 / 5 of solution B into the reactor, stir evenly, and heat to 50-80°C, react for 0.5-1h to form a core emulsion, continue to add the remaining solution B, the addition time is 4-6h, after the addition is completed, add 0.5-1 part of the redox initiator, continue to react for 1-2h, cool to room temperature, and obtain a polyacrylate thermoplastic resin with a core-shell structure.
4. The special plastic concrete for circulating fluidized bed boiler according to claim 3 is characterized in that: The mass ratio of solution A to solution B is 1:10-50.
5. The special plastic concrete for circulating fluidized bed boiler according to claim 3 is characterized in that: The KH570 modified polyester fiber has a length of 3 mm to 5 mm and a fiber diameter of 10 μm to 15 μm.
6. The special plastic concrete for circulating fluidized bed boiler according to claim 1, characterized in that: The expansion agent is silica powder.
7. The special plastic concrete for circulating fluidized bed boiler according to claim 1, characterized in that: The engineering fiber is polyester fiber, the fiber length is 5mm-20mm, and the fiber diameter is 15μm-40μm.
8. The special plastic concrete for circulating fluidized bed boiler according to claim 1, characterized in that: The particle size of the perlite is ≤3 mm.
9. The special plastic concrete for circulating fluidized bed boiler according to claim 1, characterized in that: The particle size of the expansion agent is ≤80 μm.
10. The method for preparing plastic concrete for circulating fluidized bed boiler according to any one of claims 1 to 9, characterized in that: The steps include: Step 1, weigh the raw materials according to the ratio; Step 2: Mix perlite, fly ash, silica powder, expansion agent and coupling agent at 10-35°C for 3-10 minutes to obtain mixture A for later use; mix binder, engineering fiber, water reducer and curing agent and stir for 3-10 minutes to obtain mixture B for later use; then mix mixture A with mixture B and stir evenly to obtain plastic concrete for circulating fluidized bed boiler.
Citation Information
Patent Citations
Poly-light heat-insulating plastic concrete for gasification furnace and power station boiler and production process thereof
CN112194453A
Adhesive sheet
CN115052949A
Aliphatic polyester resin composition and molded article made thereof
JP2011026621A
Polymer Cement Mortar Composition for repair and reinforcement of concrete structure section using graphene and repair and reinforcement method of concrete structure using same
KR102158508B1
Copolymer latex
US5286783A