ZTO spraying powder and preparation method thereof

By controlling process parameters and intermediate material properties, ZTO spray powder with good deposition rate and spherical morphology is prepared, which solves the problems of limited target size and powder agglomeration in traditional methods, and achieves efficient preparation and production of large-size targets. Increase in deposition rate.

CN118745112APending Publication Date: 2024-10-08PILOT THIN FILM MATERIALS (ZIBO) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410751417.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult to prepare ZTO spray powder with good deposition rate and spherical morphology with the existing technology, especially in the production of large-size targets. The target size prepared by traditional methods is limited, and high-temperature sintering can easily lead to powder agglomeration, affecting the preparation efficiency. .

Method used

By controlling process parameters such as the temperature and time of secondary sintering, and optimizing the particle size and viscosity of intermediate materials such as powder and slurry, the steps of primary sintering and crushing, spray granulation, re-sintering and crushing are used to prepare ZTO spray powder with good deposition rate and spherical morphology.

Benefits of technology

It achieves an increase in deposition rate and the formation of a spherical morphology of the powder, meets the production needs of large-size targets, avoids powder agglomeration, and improves the preparation efficiency of spray powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745112A_ABST
    Figure CN118745112A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of target material preparation, and discloses a ZTO spraying powder preparation method, which comprises: mixing zinc oxide and tin oxide powder, homogenizing to obtain powder I, carrying out primary sintering and crushing on the powder I to obtain powder II, mixing the powder II with water, grinding to obtain slurry, and finally carrying out spray granulation, secondary sintering, crushing and screening on the slurry to obtain the ZTO spraying powder. The secondary sintering temperature is 1000-1400 DEG C, the secondary sintering time is 6-8 h, the ZTO spraying powder with the good spherical morphology and the good deposition rate is prepared through the design, and in addition, the invention further discloses the ZTO spraying powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of spray powder preparation, and in particular to a ZTO spray powder and a preparation method thereof. Background Art

[0002] The target material is the raw material for magnetron sputtering coating. By bombarding the cathode target material with positively charged particles, the target atoms gain energy and escape, which is then deposited on the surface of the substrate to form a thin film. The thin films sputtered by the target material are widely used in decoration, molds, energy-saving glass, integrated circuits, semiconductors, magnetic recording, flat-panel displays, solar cells and other fields. With the increase in consumer market demand and the upgrading of industrial technology, the target material has not only increased significantly in quantity and variety, but also put forward higher requirements for the high utilization rate and large size of the target material. According to the shape, the target material is roughly divided into plate-shaped target material and tubular target material. Since the magnetic field applied by magnetron sputtering is a circular magnetic field, erosion will occur during sputtering, resulting in a utilization rate of less than 30% for plate-shaped targets, while the utilization rate of tubular targets can reach 80%. In addition, the larger the size of the target material, the larger the sputtering area and the higher the coating efficiency. Therefore, large size and tubularization are important directions for the development of target material production;

[0003] As a surface technology, plasma spraying is not limited by size and space. It can produce coatings with a certain thickness on the surface of large workpieces. It has been gradually applied to target production. ZTO film is a zinc tin oxide film, which is mainly composed of zinc oxide and tin oxide, and its main component is Zn2SnO4. ZTO film has similar photoelectric properties to ITO film, and has the characteristics of low price, good chemical stability, and non-toxicity. It is used to replace ITO film. The traditional preparation methods of oxide targets for ZTO films are hot isostatic pressing and sintering, but the size of the targets they prepare is limited and cannot be used for the preparation of large-size targets. However, plasma spraying can avoid this problem and prepare large-size targets to meet production needs. The spray powder of plasma spraying targets needs to be prepared separately, and the spray powder needs to meet the requirements of good fluidity, narrow particle size distribution, and good sphericity.

[0004] Chinese patent application 202310235344.X discloses a method for preparing a rare earth-modified spray powder and the spray powder thereof. The method for preparing a rare earth-modified spray powder of the scheme comprises the following steps:

[0005] A base powder of a first shape having a first predetermined size and a rare earth powder of a second shape having a second predetermined size are cold welded by mechanical ball milling and pressed into the rare earth powder by extrusion, wherein the base powder includes metal and its alloy, ceramic or organic polymer;

[0006] The rare earth powder includes single substances and compounds of cerium, lanthanum, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium, and the first predetermined size is greater than the second predetermined size;

[0007] The matrix powder into which the rare earth powder is pressed after mechanical ball milling is subjected to solid solution heat treatment to form a composite powder, thereby obtaining a rare earth modified spray powder;

[0008] Although the base powder of the above scheme includes zinc, tin metal powder or alloy powder, further observation shows that the process route of this scheme is obviously different from that of this scheme. This scheme is more concerned with how to modify the base powder with rare earth powder. Its process route is to press the rare earth powder into the base powder through ball milling, and then form a mixed powder through solid solution treatment to finally obtain the spray powder.

[0009] Chinese patent application 202310951467.3 discloses a process for preparing a zinc tin oxide target, which is characterized by comprising the following steps:

[0010] (1) Mixing raw materials: Add the dispersant to deionized water and mix well, then add zinc oxide powder and tin oxide powder and stir at a stirring frequency of 15-35 Hz and a stirring time of 0.5-1.5 h to obtain a mixed slurry;

[0011] (2) Slurry sand grinding: The mixed slurry is sand ground at a sand mill speed of 600-1600 rpm, a sand grinding time of 8-12 h, and a sand grinding number of 6 times to obtain a sand ground slurry;

[0012] (3) Powder granulation: Add zinc powder, tin powder and defoamer into the sand mill slurry and stir.

[0013] The amount is 5%-15% of the weight of the sand-grinding slurry, wherein the weight ratio of zinc powder to tin powder is 1:1, the stirring time is 2-6 hours, and then spray granulation is performed to obtain a mixed powder;

[0014] (4) Powder sintering: Spread the mixed powder in a crucible and then sinter at a temperature of 300-400° C. for 15-60 min. After sintering, sieve the powder through a 100-270 mesh sieve to obtain a composite zinc oxide tin powder containing metallic zinc and tin.

[0015] (5) Plasma spraying: The composite zinc oxide tin powder containing metallic zinc and tin is subjected to atmospheric plasma spraying, wherein the Ar flow rate is 2200-2800 L / h, the H2 flow rate is 420-500 L / h, the spraying voltage is 50-70 V, the current is 400-450 A, the carrier gas flow rate is 180-200 L / h, and the powder feeding amount is 100-120 g / min, to obtain a zinc oxide tin target;

[0016] This solution provides a zinc oxide tin target material preparation process, which adopts a method of grinding first and then granulating. First, the zinc oxide powder and the tin oxide powder are ground, and then zinc powder and tin powder are added for granulation and sintering to form a conductive zinc oxide tin powder, and finally a zinc oxide tin target material with good conductive properties is prepared by a plasma spraying process;

[0017] However, by observing the steps of this scheme, it can be seen that, on the one hand, it is necessary to add a dispersant during the raw material mixing process in this scheme to ensure the dispersion effect between zinc oxide and tin oxide. On the other hand, by observing step 4 of the embodiment of this scheme, it can be seen that "the mixed powder is spread in a crucible and then sintered at a sintering temperature of 350°C and a sintering time of 40 minutes. After sintering, the mixed powder is sieved through a 140-mesh sieve." This scheme directly sieves the mixed powder after sintering, but according to common sense, high-temperature sintering is prone to cause powder agglomeration, so it often needs to be crushed before sieving. At the same time, by observing the sintering time and sintering temperature of step 4, it can be inferred that this scheme may not completely burn off the moisture in the mixed powder in step 4, so that the agglomeration phenomenon of the mixed powder is not obvious, thereby omitting the crushing step.

[0018] The problem to be solved by this scheme is: how to provide a method for preparing ZTO spray powder with good deposition rate and spherical morphology. Summary of the invention

[0019] The purpose of the present application is to provide a method for preparing a ZTO spray powder with a good deposition rate and a spherical morphology by controlling the process parameters in the experimental process, such as the temperature and time of the secondary sintering, and controlling the particle size and viscosity of the intermediate materials in the preparation process, such as the powder and slurry.

[0020] To achieve the above object, the present application discloses a method for preparing a ZTO spray powder, comprising the following steps:

[0021] Step 1: Mix and homogenize zinc oxide and tin oxide powder to obtain powder 1;

[0022] Step 2: sintering and crushing the powder 1 obtained in step 1 to obtain powder 2;

[0023] Step 3: Mix and grind the powder obtained in step 2 with water to obtain a slurry;

[0024] Step 4: spray granulation, secondary sintering, crushing and sieving the slurry obtained in step 3 to obtain ZTO spray powder;

[0025] In step 4, the temperature of the secondary sintering is 1000-1400° C., and the time of the secondary sintering is 6-8 hours.

[0026] Further, the temperature of the secondary sintering includes but is not limited to 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C;

[0027] The secondary sintering time includes but is not limited to 6h, 6.5h, 7h, 7.5h, and 8h;

[0028] Further preferably, the temperature of the secondary sintering in step 4 is 1200-1300° C.;

[0029] Furthermore, in step 1, the molar ratio of zinc oxide to tin oxide is 40-60:40-60.

[0030] Furthermore, in step 1, the molar ratio of zinc oxide to tin oxide is 48-52:48-52;

[0031] Further preferably, in step 1, the molar ratio of zinc oxide to tin oxide includes but is not limited to 48:52, 49:51, 50:50, 51:49, 52:48;

[0032] Furthermore, the step 2 is specifically as follows:

[0033] The powder 1 obtained in step 1 is placed in a sintering furnace for a first sintering, the first sintering temperature is 1100-1400° C., the sintering time is 2-4 hours, and then crushed and pulverized to obtain a powder 2 with a particle size D90<5 μm.

[0034] Furthermore, the step 3 is specifically as follows:

[0035] The powder 2 obtained in step 2 is mixed with pure water according to a solid content of 50-70%, and ground for 3-8 hours at a grinding speed of 800-900 rpm to obtain a slurry, wherein the particle size D90 of the slurry is less than 3 μm and the viscosity is greater than 1000 mPa·s.

[0036] Furthermore, in the spray granulation process in step 4, the inlet temperature is set to 230-250° C., the outlet temperature is 110-120° C., and the atomizing disk rotation speed is 7000-10000 rpm.

[0037] In addition, the present application also discloses a ZTO spray powder, which is prepared by the above-mentioned ZTO spray powder preparation method.

[0038] Preferably, the ZTO spray powder has a spherical morphology, and D10 is not less than 30 μm, D50 is 60 to 80 μm, and D90 is 110 to 120 μm.

[0039] The beneficial effects of the present application are as follows: the present application provides a method for preparing ZTO spray powder with good deposition rate and spherical morphology, and at the same time, the present application controls the process parameters in the experimental process, such as the temperature and time of the secondary sintering, and controls the particle size and viscosity of the intermediate materials in the preparation process, such as the powder and slurry, so that the deposition rate of the ZTO spray powder is further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the SEM image of the ZTO powder prepared in Example 1;

[0041] Figure 2 This is the SEM image of the ZTO powder prepared in Example 2;

[0042] Figure 3 This is the SEM image of the ZTO powder prepared in Comparative Example 2. DETAILED DESCRIPTION

[0043] The present application will be described clearly and completely below in conjunction with the examples of the present application. In the description of the present application, it should be noted that if the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0044] Example 1

[0045] Step 1: Weigh two raw material powders of zinc oxide (ZnO) and tin oxide (SnO2) at a molar ratio of 52:48, place in a homogenizer and homogenize for 2 hours to mix the two raw materials to obtain powder 1;

[0046] Step 2: placing the powder 1 obtained in step 1 in a sintering furnace for pre-sintering at a sintering temperature of 1200° C. for 3 h, and crushing and pulverizing after sintering to obtain a powder 2 with a particle size D90 of 3.5 μm;

[0047] Step 3: The powder obtained in step 2 was mixed with pure water at a solid content of 60%, and ground for 5 hours at a grinding speed of 800 rpm to obtain a slurry with a particle size D90 of 2 μm and a viscosity of 1480 mPa·s;

[0048] Step 4: spray granulation of the slurry obtained in step 3, wherein the inlet temperature during the spray granulation is set to 250°C, the outlet temperature is 120°C, and the atomizing disk speed is 7000 rpm;

[0049] Then, secondary sintering is performed at a temperature of 1300° C. and a time of 6 h. The material obtained after the secondary sintering is crushed and passed through a 325-mesh sieve to obtain ZTO spray powder.

[0050] Example 2

[0051] Step 1: Weigh two raw material powders of zinc oxide (ZnO) and tin oxide (SnO2) at a molar ratio of 48:52, place in a homogenizer and homogenize for 2 hours to mix the two raw materials to obtain powder 1;

[0052] Step 2: placing the powder 1 obtained in step 1 in a sintering furnace for a sintering process, wherein the sintering temperature is 1100° C., the sintering time is 2 h, and after sintering, the powder is crushed and pulverized to obtain a powder 2 having a particle size D90 of 4.3 μm;

[0053] Step 3: The powder obtained in step 2 was mixed with pure water at a solid content of 70%, and ground for 8 hours at a grinding speed of 900 rpm to obtain a slurry with a particle size D90 of 1.8 μm and a viscosity of 1390 mPa·s;

[0054] Step 4: spray granulation of the slurry obtained in step 3, wherein the inlet temperature during the spray granulation is set to 230°C, the outlet temperature is set to 110°C, and the atomizing disk speed is set to 10000 rpm;

[0055] Then, secondary sintering is performed at a temperature of 1200° C. and a time of 8 h. The material obtained after the secondary sintering is crushed and passed through a 325-mesh sieve to obtain ZTO spray powder.

[0056] Example 3

[0057] Step 1: Weigh two raw material powders of zinc oxide (ZnO) and tin oxide (SnO2) at a molar ratio of 50:50, place in a homogenizer and homogenize for 2 hours to mix the two raw materials to obtain powder 1;

[0058] Step 2: placing the powder 1 obtained in step 1 in a sintering furnace for a sintering process, wherein the sintering temperature is 1300° C., the sintering time is 4 h, and after sintering, the powder is crushed and pulverized to obtain a powder 2 having a particle size D90 of 3.9 μm;

[0059] Step 3: The powder obtained in step 2 was mixed with pure water at a solid content of 50%, and ground for 3 hours at a grinding speed of 850 rpm to obtain a slurry with a particle size D90 of 2.4 μm and a viscosity of 1610 mPa·s;

[0060] Step 4: spray granulation of the slurry obtained in step 3, wherein the inlet temperature during the spray granulation process is set to 240°C, the outlet temperature is 115°C, and the atomizing disk speed is 8500rpm;

[0061] Then, secondary sintering is carried out, the temperature of the secondary sintering is 1250°C, and the time of the secondary sintering is 7 hours. The material obtained after the secondary sintering is crushed and passed through a 325-mesh sieve to obtain ZTO spray powder.

[0062] Example 4

[0063] It is basically the same as Example 3, except that the secondary sintering temperature is 1000°C.

[0064] Example 5

[0065] It is basically the same as Example 3, except that the temperature of the secondary sintering is 1400°C.

[0066] Example 6

[0067] It is basically the same as Example 3, except that, in step 1, the molar ratio of zinc oxide (ZnO) to tin oxide (SnO2) is 40:60.

[0068] Example 7

[0069] It is basically the same as Example 3, except that, in step 1, the molar ratio of zinc oxide (ZnO) to tin oxide (SnO2) is 60:40.

[0070] Comparative Example 1

[0071] Step 1: Weigh two raw material powders of zinc oxide (ZnO) and tin oxide (SnO2) at a molar ratio of 50:50, place in a homogenizer and homogenize for 2 hours to mix the two raw materials to obtain powder 1;

[0072] Step 2: The powder obtained in step 1 is mixed with pure water at a solid content of 50%, and ground for 3 hours at a grinding speed of 850 rpm to obtain a slurry with a particle size D90 of 2.4 μm and a viscosity of 1610 mPa·s;

[0073] Step 3: The slurry prepared in step 2 is subjected to spray granulation. During the spray granulation process, the inlet temperature is set to 240°C, the outlet temperature is 115°C, and the atomizing disk speed is 8500rpm;

[0074] Then, secondary sintering is carried out, the temperature of the secondary sintering is 1250°C, and the time of the secondary sintering is 7 hours. The material obtained after the secondary sintering is crushed and passed through a 325-mesh sieve to obtain ZTO spray powder.

[0075] Comparative Example 2

[0076] It is basically the same as Example 3, except that in step 4, the temperature of the secondary sintering is 350° C., and the time of the secondary sintering is 6 hours.

[0077] Comparative Example 3

[0078] It is basically the same as Example 3, except that in step 4, the temperature of the secondary sintering is 1250° C., and the time of the secondary sintering is 40 minutes.

[0079] Comparative Example 4

[0080] It is basically the same as Example 3, except that in step 3, the particle size D90 of the slurry is 3.4 μm and the viscosity is 620 mPa·s.

[0081] Performance Testing:

[0082] The spray powders prepared in the embodiments and comparative examples were analyzed for microscopic morphology using a scanning electron microscope, and the particle sizes were counted using a laser particle size analyzer;

[0083] The deposition weight is used to calculate the deposition rate of the spray powder. The calculation formula is:

[0084]

[0085] The test results are shown in Tables 1 and 2:

[0086] Table 1

[0087]

[0088]

[0089] Table 2

[0090]

[0091] Result analysis:

[0092] By comparing Examples 1 to 3 and Examples 6 to 7, the range of 40% to 60% of zinc oxide applicable to the present invention can be prepared to meet the particle size of spraying, and the spraying deposition rate can reach 48%. It can be seen from Examples 3 to 5 that the powder can obtain a particle size of about 30 to 120 microns at 1000 to 1400°C, which can make the spraying deposition rate about 45%. By comparing Example 1 with Example 3, it is shown that not adding pre-sintering will not affect the final granulation particle size, but will make the final product component uniformity poor. By comparing Example 3 with Comparative Examples 2 to 3, low-temperature sintering or shortening the sintering time will cause the particle size of the powder to decrease a little, but the spraying deposition rate decreases significantly. This is because the sintering temperature is low or the time is short, the bonding strength of the powder is not good, the powder cracks during the spraying process, and is not deposited on the back tube. By comparing Example 3 with Comparative Example 4, the low-viscosity slurry will cause the particle size of the powder to decrease significantly, which cannot meet the requirements of the spraying process for the powder, resulting in a decrease in the deposition rate.

[0093] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a ZTO spray powder, characterized in that: The following steps are involved: Step 1: Mix and homogenize zinc oxide and tin oxide powder to obtain powder 1; Step 2: sintering and crushing the powder 1 obtained in step 1 to obtain powder 2; Step 3: Mixing and grinding the powder obtained in step 2 with water to obtain a slurry; Step 4: spray granulation, secondary sintering, crushing and sieving the slurry obtained in step 3 to obtain ZTO spray powder; In step 4, the temperature of the secondary sintering is 1000-1400° C., and the time of the secondary sintering is 6-8 hours.

2. The method for preparing the ZTO spray powder according to claim 1, characterized in that: The temperature of the secondary sintering in step 4 is 1200-1300°C.

3. The method for preparing the ZTO spray powder according to claim 1, characterized in that: In the step 1, the molar ratio of zinc oxide to tin oxide is 40-60:40-60.

4. The method for preparing the ZTO spray powder according to claim 1, characterized in that: In the step 1, the molar ratio of zinc oxide to tin oxide is 48-52:48-52.

5. The method for preparing the ZTO spray powder according to claim 1, characterized in that: The step 2 is specifically as follows: The powder 1 obtained in step 1 is placed in a sintering furnace for a first sintering, the first sintering temperature is 1100-1400° C., the sintering time is 2-4 hours, and then crushed and pulverized to obtain a powder 2 with a particle size D90<5 μm.

6. The method for preparing the ZTO spray powder according to claim 1, characterized in that: The step 3 is specifically as follows: The powder 2 obtained in step 2 is mixed with pure water according to a solid content of 50-70%, and ground for 3-8 hours at a grinding speed of 800-900 rpm to obtain a slurry, wherein the particle size D90 of the slurry is less than 3 μm and the viscosity is greater than 1000 mPa·s.

7. The method for preparing the ZTO spray powder according to claim 1, characterized in that: In the spray granulation process in step 4, the inlet temperature is set to 230-250° C., the outlet temperature is 110-120° C., and the atomizing disk rotation speed is 7000-10000 rpm.

8. A ZTO spray powder, characterized in that: The invention is prepared by the preparation method of the ZTO spray powder described in any one of claims 1 to 7.

9. The ZTO spray powder according to claim 8, characterized in that: The ZTO spray powder has a spherical morphology, and D10 is not less than 30 μm, D50 is 60-80 μm, and D90 is 110-120 μm.

Citation Information

Patent Citations

  • Rare earth modified spraying powder preparation method and spraying powder thereof

    CN116237527A

  • Preparation process of zinc tin oxide target material

    CN117089812A

  • TZO ceramic powder as well as preparation method and application thereof

    CN118026671A