No.5-site binaphthyl diisocyanate, synthesis method thereof and application of No.5-site binaphthyl diisocyanate in preparation of binaphthyl polyurethane material
By using the synthesis method of No. 5 binaphthyl diisocyanate in polyurethane materials, the problem of insufficient impact resistance and mechanical properties of existing materials in extreme environments is solved, and an urethane armor with high mechanical strength and shock-absorbing and energy-absorbing properties is prepared. Acid ester material, suitable for high damping and high vibration scenarios.
Patent Information
- Application Number
- CN202410737424.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Existing polyurethane materials lack sufficient impact resistance, hardness and mechanical properties in extreme environments (high damping, high vibration scenarios), and applicable isocyanate monomers are scarce.
Binaphthyl diisocyanate at position 5 is used as an important organic synthesis intermediate and is prepared through acylation reaction, Ullmann coupling reaction and carbonylation reaction to generate carbamic acid with high covalent bond stability and rigid molecular structure. Ester material, used to make polyurethane elastomers with high elasticity and hardness.
The generated urethane material has excellent thermal stability, tensile resistance and high mechanical strength, and is suitable for new energy vehicle batteries, bridges, military industry and other fields. It especially shows excellent attenuation in high damping and high vibration scenarios. Shock energy absorption performance.
Smart Images

Figure BDA0004882203400000021 
Figure BDA0004882203400000031 
Figure BDA0004882203400000032
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of carbamate materials, and specifically relates to a 5-binaphthyl diisocyanate and a synthesis method thereof, and application thereof in the preparation of a binaphthyl polycarbamate material. Background Art
[0002] Polyurethane, PU for short, is a type of polymer material that contains a large number of repeated urethane groups (-NHCOO-) in the molecular chain. Polyurethane elastomer is a relatively special type of elastomer. From the perspective of molecular structure, polyurethane elastomer is a block polymer, generally composed of a soft segment of a flexible long chain of oligomer polyols, and a hard segment of a diisocyanate and a chain extender. The hard segment and the soft segment are arranged alternately to form a repeating structural unit. In addition to containing urethane groups, hydrogen bonds can be formed within and between polyurethane molecules, and the soft segment and the hard segment can form a microphase region and produce microscopic phase separation.
[0003] Polyurethane elastomers prepared from 1,5-naphthalene diisocyanate (referred to as "NDI") have incomparable performance advantages, such as excellent dynamic compression performance, extremely high mechanical properties, and wear and temperature resistance. Currently, NDI polyurethane elastomers are widely used in automobile shock absorbers, forklift load-bearing wheels, bridge construction buffer blocks, military industry, etc. NDI is a hard segment raw material for polyurethane and can be used to manufacture polyurethane elastomers with high elasticity and high hardness. However, in some extreme environments (high damping, high vibration scenarios), the material needs to have stronger impact resistance, hardness, mechanical properties, and shock absorption and energy absorption effects. It is very rare to find isocyanate monomers on the market that are suitable for such extremely harsh conditions. Summary of the invention
[0004] The purpose of the present invention is to address the existing technical problems and propose a No. 5 binaphthyl diisocyanate and its synthesis method and its application in the preparation of binaphthyl polyurethane materials. The No. 5 binaphthyl diisocyanate provided by the present invention, as an important organic synthesis intermediate, is a new raw material for the manufacture of polyurethane elastomers with high elasticity and high hardness by reacting with macromolecular diols and polyols. The generated carbamate is suitable for the fields of new energy vehicle battery shock absorption, bridges, military industry, etc., and is also suitable for extreme environments such as high strength, high hardness, wear resistance and high temperature resistance. At the same time, the No. 5 binaphthyl diisocyanate provided by the present invention has a stable chemical bond and a dense molecular structure, has excellent thermal stability and tensile resistance, and the generated polybinaphthyl carbamate has a high cohesive energy and impact modulus, and is particularly suitable for high damping and high vibration scenes. Therefore, the polybinaphthyl carbamate provided by the present invention is a polymer material with excellent performance and wide application, and its synthesis method and technical application are of great value.
[0005] The technical solution of the present invention is achieved in this way:
[0006] A 5-binaphthyl diisocyanate is prepared by acylation reaction of naphthylamine, Ullmann coupling reaction with metal or its salt as catalyst in the presence of ligand and inorganic base and under the protection of inert gas, amide hydrolysis and subsequent carbonylation reaction with carbonylation agent.
[0007] In the 5-position binaphthyl diisocyanate as described above, the structure of the naphthylamine is as shown in the following formula (I), wherein X is chlorine, bromine, iodine, trifluoromethanesulfonyloxy, p-toluenesulfonyloxy or phenolic hydroxyl group.
[0008] Preferably, X is chlorine or a phenolic hydroxyl group.
[0009]
[0010] The structure of the product of the 5-position binaphthyl diisocyanate after the acylation reaction of the naphthylamine is shown in the following formula (II), wherein R1 is C1-C 10 Straight or branched alkyl, C1~C 10 Alkoxy or C1~C 10 X is chlorine, bromine, iodine, trifluoromethanesulfonyloxy, p-toluenesulfonyloxy or phenolic hydroxyl.
[0011]
[0012] For the 5-binaphthyl diisocyanate as described above, the structure of the product generated by the Ullmann coupling reaction is as follows: 10 Straight or branched alkyl, C1~C 10 Alkoxy or C1~C 10 The alkylthio group,
[0013]
[0014] For the 5-binaphthyl diisocyanate described above, the structure of the product generated by the amide hydrolysis reaction is shown in the following formula (IV):
[0015]
[0016] For the 5-binaphthyl diisocyanate described above, the structure of the product generated by the carbonylation reaction is shown in the following formula (V):
[0017]
[0018] Based on the same inventive concept, the present invention also provides a method for synthesizing 5-binaphthyl diisocyanate, comprising the following steps:
[0019] Step 1: naphthylamine undergoes acylation reaction with an acylating agent to generate a halogenated acyl naphthylamine or a phenolic hydroxyl acyl naphthylamine.
[0020] Optionally, the naphthylamine is a halogenated naphthylamine or a phenolic hydroxy naphthylamine; preferably, the naphthylamine is 1-amino-5-chloronaphthalene or 1-amino-5-naphthol; more preferably, the naphthylamine is 1-amino-5-chloronaphthalene.
[0021] Optionally, the acylating agent in step one is any one of carboxylic acid, carboxylic acid ester, acid anhydride and acid chloride; preferably, the acylating agent in step one is any one of acetic anhydride and acetic acid; more preferably, the acylating agent in step one is acetic anhydride.
[0022] Optionally, the molar ratio of the naphthylamine to the acylating agent is 4:(5-10); preferably, the molar ratio of the naphthylamine to the acylating agent is 4:5 or 4:10.
[0023] Optionally, an acylating agent is added to the halogenated naphthylamine or phenolic hydroxy naphthylamine, heated to 40-110°C, stirred for reaction for 60-120 minutes, cooled, filtered, and dried to obtain the halogenated acyl naphthylamine or phenolic hydroxy acyl naphthylamine. Preferably, the acylating agent is heated to 80°C and stirred for reaction for 60 minutes.
[0024] Step 2: The halogenated acyl naphthylamine or phenolic hydroxy acyl naphthylamine in step 1 is dissolved in an organic solvent, and an Ullmann reaction is carried out in the presence of a ligand and under the protection of an inert gas using a metal or a salt thereof as a catalyst to generate an alkyl acyl binaphthylamine.
[0025] Specifically, the halogenated acyl naphthylamine or phenolic hydroxy acyl naphthylamine in step 1 is dissolved in an organic solvent, stirred and dissolved, and an Ullmann reaction is carried out with a metal or a salt thereof as a catalyst in the presence of a ligand and an inorganic base and under the protection of an inert gas. The reaction time is 24 to 48 hours. After the reaction mixture is cooled, the solvent is filtered and evaporated, and column separation and purification are carried out with ethyl acetate and n-heptane in a volume ratio of 1:4 as an eluent to obtain a yellow solid product, namely, alkyl acyl binaphthylamine.
[0026] Optionally, the organic solvent is anhydrous N,N-dimethylformamide (hereinafter referred to as "anhydrous DMF") or dichloromethane. Preferably, the organic solvent is anhydrous DMF.
[0027] Optionally, the catalyst is any one of cuprous iodide, cuprous oxide, and nickel chloride. Preferably, the catalyst is cuprous iodide.
[0028] Optionally, the ligand is N,N-dimethylethylenediamine or triphenylphosphine. Preferably, the ligand is N,N-dimethylethylenediamine.
[0029] Preferably, the step 2 is carried out under alkaline conditions, and the alkaline conditions are adjusted using an inorganic base; optionally, the inorganic base is cesium carbonate.
[0030] Optionally, the molar ratio of the halogenated acyl naphthylamine or phenolic hydroxyl acyl naphthylamine to the catalyst is (8-12): 1. Preferably, the molar ratio of the halogenated acyl naphthylamine or phenolic hydroxyl acyl naphthylamine to the catalyst is 9:1.
[0031] Optionally, the molar ratio of the halogenated acyl naphthylamine or phenolic hydroxyl acyl naphthylamine to the ligand is 2:(1-2). Preferably, the molar ratio of the halogenated acyl naphthylamine or phenolic hydroxyl acyl naphthylamine to the ligand is 2:1.
[0032] Optionally, the molar ratio of the halogenated acyl naphthylamine or phenolic hydroxyl acyl naphthylamine to the inorganic base is 1:(1-3). Preferably, the molar ratio of the halogenated acyl naphthylamine or phenolic hydroxyl acyl naphthylamine to the inorganic base is 1:2.
[0033] Step 3: The alkyl acyl binaphthylamine in step 2 is heated to reflux with a small molecule alkyl alcohol solution under strong acid conditions to undergo a hydrolysis reaction to generate binaphthyl diamine.
[0034] Optionally, the alkyl acyl binaphthylamine in step 2 is added to a mixed solution of 36% concentrated hydrochloric acid and anhydrous ethanol, heated to 75-95° C., heated under reflux for 2-4 hours, filtered and dried after cooling to obtain a yellow solid product, namely binaphthyl diamine;
[0035] Step 4: The dinaphthyl diamine in step 3 is subjected to carbonylation reaction to generate 5-position dinaphthyl diisocyanate.
[0036] Optionally, the mass ratio of the binaphthyl diamine to the carbonylating agent is (3-5):(8-10). Most preferably, the mass ratio of the binaphthyl diamine to the carbonylating agent is 4.27:10.
[0037] Optionally, the dinaphthylene diamine in the step three is dissolved in 1,2-dichlorobenzene solvent, stirred and heated to 120°C, and the 1,2-dichlorobenzene solution of triphosgene is slowly dripped into the dinaphthylene diamine, and the dripping time in the 1,2-dichlorobenzene solution is 48 hours. After the dripping is completed, continue to heat and reflux for 3 to 6 hours until the reaction system is clear and transparent, and remove the organic solvent by separation to obtain a crude product of p-phenylene diisocyanate. The crude product is recrystallized in xylene to obtain a yellow solid product, i.e., No. 5 dinaphthylene diisocyanate.
[0038]
[0039] Based on the same inventive concept, the present invention also provides an application of No. 5 binaphthyl diisocyanate in the preparation of urethane rubber and elastomer, urethane fiber, cast urethane rubber, urethane emulsion and coating, urethane adhesive, shock-absorbing foam material, energy-absorbing foam material, and damping foam material.
[0040] Based on the same inventive concept, the present invention also provides a carbamate material, which is prepared using a No. 5-binaphthalene diisocyanate as described above or a No. 5-binaphthalene diisocyanate synthesized by the synthesis method described above.
[0041] The beneficial effects of the invention are:
[0042] 1. The present invention provides a 5-position binaphthyl diisocyanate, which has four ring structures with high covalent bond stability, excellent chemical stability and high strength. At the same time, the naphthalene rings are connected by CC bonds, and there is a very strong rigidity feature in its molecular structure. This rigid structure makes the carbamate material have outstanding mechanical strength, and the material has the advantages of high hardness, good resilience, excellent shock absorption and energy absorption performance, etc.
[0043] 2. The 5-binaphthyl diisocyanate provided by the present invention has a large conjugated structure and a stable chemical bond. The obtained binaphthyl polyurethane material has a higher loss factor, indicating that the viscosity of the material is greater. DETAILED DESCRIPTION
[0044] The following will combine the contents in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in this specification includes any and all combinations of one or more of the related listed items.
[0046] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0047] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0048] In the following examples, the 1-amino-5-chloronaphthalene was purchased from Shanghai Yuanye Biotechnology Co., Ltd., with a CAS number of 2750-80-3 and a density of 1.289 g / cm 3 , molecular weight 177.63. The 1-amino-5-naphthol was purchased from
[0049] Embodiment 1:
[0050] This embodiment provides a 5-binaphthyl diisocyanate, and its synthesis method includes the following specific steps:
[0051] Step 1, weigh 7.1 g of 1-amino-5-chloronaphthalene, add 4.7 mL of acetic anhydride, add 0.02 g of zinc powder, heat to 80 ° C, stir and react for 60 min, pour the hot reaction solution into 200 mL of water, precipitate white crystals, cool, filter and dry to obtain 7.99 g of N-(5-chloro-1-naphthalene)-acetamide, with a yield of 91%;
[0052] Step 2: Dissolve 7.99 g of N-(5-chloro-1-naphthalene)-acetamide obtained in step 1 in 50 mL of anhydrous DMF and stir to dissolve, add 0.8 g of cuprous iodide, 2 mL of N,N-dimethylethylenediamine, and 23.5 g of cesium carbonate, slowly heat to 120 ° C. under nitrogen protection, react for 24 hours, and after the reaction is completed, cool and filter to evaporate the solvent, and use ethyl acetate and n-heptane in a volume ratio of 1:4 as an eluent for column separation and purification to obtain 5.7 g of a yellow solid product, that is, alkyl acyl dinaphthylamine, with a yield of 86%.
[0053] Step 3: Add 5.7 g of the yellow solid product obtained in step 2 to a mixed solution of 50 mL of 36% concentrated hydrochloric acid and 50 mL of ethanol, heat to 85°C and reflux for 3 h, filter and dry after cooling to obtain 4.27 g of a yellow solid product, namely, dinaphthylene diamine, with a yield of 97%.
[0054] Step 4: Dissolve 4.27 g of the dried yellow solid dinaphthyl diamine in step 3 in 1,2-dichlorobenzene solvent, stir and heat to 120 ° C, slowly drop 50 g of triphosgene in 1,2-dichlorobenzene solution into the diphenyl diamine solution, wherein the mass concentration of triphosgene in 1,2-dichlorobenzene solution is 20%, and the dropping time is 48 h. After the dropwise addition is completed, continue to heat and reflux for 4 h until the reaction system is clear and transparent, remove the organic solvent by separation, and obtain a crude product of p-phenylene diisocyanate. The crude product is recrystallized in xylene to obtain 4.64 g of a yellow solid product, that is, 5-position dinaphthyl diisocyanate, with a yield of 92%.
[0055] The product identification data are as follows:
[0056] GC-MS: 336.09;
[0057] Determination by nuclear magnetic resonance: 1H NMR (400MHz, DMSO-d6) δ: 8.77 (d, 2H, Ar-H), 8.55 (d, 2H, Ar-H), 8.41 (d, 2H, Ar-H), 7.78 (t, 2H, Ar-H), 7.74 (d, 2H, Ar-H), 7.37 (t, 2H, Ar-H);
[0058] 13C NMR(101MHz,DMSO-d6)δ:135.0,134.2,132.3,131.4,131.1,128.4,127.9,127.7,127.2,125.5,118.0
[0059] Embodiment 2:
[0060] This embodiment provides a 5-binaphthyl diisocyanate, and its synthesis method includes the following specific steps:
[0061] Step 1, weigh 7.1 g of 1-amino-5-chloronaphthalene, add 5.7 mL of acetic acid, add 0.05 g of zinc powder, stir and heat to 105 ° C, react and reflux for 60 min, pour the hot reaction solution into 200 mL of cold water in a thin stream, precipitate white crystals, cool, filter and dry to obtain 7.82 g of N-(5-chloro-1-naphthalene)-acetamide, with a yield of 89%;
[0062] Step 2: Dissolve 7.82 g of N-(5-chloro-1-naphthalene)-acetamide obtained in step 1 in 50 mL of anhydrous DMF and stir to dissolve, add 0.8 g of cuprous iodide, 4 mL of N,N-dimethylethylenediamine, and 23.5 g of cesium carbonate, slowly heat to 120 ° C. under nitrogen protection, react for 24 hours, and after the reaction is completed, cool and filter to evaporate the solvent, and use ethyl acetate and n-heptane in a volume ratio of 1:4 as an eluent for column separation and purification to obtain 5.51 g of a yellow solid product, that is, alkyl acyl dinaphthylamine, with a yield of 84%.
[0063] Step 3: Add the yellow solid product obtained in step 2 to a mixed solution of 50 mL of 36% concentrated hydrochloric acid and 50 mL of ethanol, heat to 75°C and reflux for 2 h, filter and dry after cooling to obtain 4.04 g of a yellow solid product, namely, dinaphthylene diamine, with a yield of 95%.
[0064] Step 4: Dissolve 4.04 g of the dried yellow solid dinaphthyl diamine in step 3 in 1,2-dichlorobenzene solvent, stir and heat to 120°C, slowly drop 50 g of triphosgene in 1,2-dichlorobenzene solution into the diphenyl diamine solution, wherein the mass concentration of triphosgene in 1,2-dichlorobenzene solution is 20%. After the dropwise addition is completed for 48 hours, continue to heat and reflux for 4 hours until the reaction system is clear and transparent, remove the organic solvent by liquid separation, and obtain a crude product of p-phenylene diisocyanate. The crude product is recrystallized in xylene to obtain 4.44 g of a yellow solid product, that is, 5-position dinaphthyl diisocyanate, with a yield of 93%.
[0065] The product identification data are as follows:
[0066] GC-MS: 336.09NMR determination: 1H NMR (400MHz, DMSO-d6) δ: 8.77 (d, 2H, Ar-H), 8.55 (d, 2H, Ar-H), 8.41 (d, 2H, Ar-H), 7.78 (t, 2H, Ar-H), 7.74 (d, 2H, Ar-H), 7.37 (t, 2H, Ar-H);
[0067] 13C NMR(101MHz,DMSO-d6)δ:135.0,134.2,132.3,131.4,131.1,128.4,127.9,127.7,127.2,125.5,118.0
[0068] Embodiment 3:
[0069] This embodiment provides a 5-binaphthyl diisocyanate, and its synthesis method includes the following specific steps:
[0070] Step 1, weigh 6.36 g of 1-amino-5-naphthol, add 4.7 mL of acetic anhydride, add 0.02 g of zinc powder, stir and heat to 80 ° C, react for 60 minutes, and pour the reaction solution into 200 mL of water after cooling to precipitate white crystals, cool, filter and dry to obtain 7.48 g of N-(5-hydroxy-1-naphthalene)-acetamide, with a yield of 93%;
[0071] Step 2: Dissolve 7.48 g of N-(5-hydroxy-1-naphthalene)-acetamide obtained in step 1 and 6.9 mL of triethylamine, an acid binding agent, in 50 mL of dichloromethane, cool to 0 ° C in an ice-water bath, and stir to dissolve. Add 4.7 mL of trifluoromethanesulfonyl chloride, slowly warm to room temperature, react for 2 h, wash with water, separate the lower layer, add anhydrous sodium sulfate to dry, and evaporate the solvent to obtain 10.85 g of a yellow solid product, namely, N-(5-trifluoromethanesulfonic acid oxo-1-naphthalene)-acetamide, with a yield of 88%.
[0072] Step 3: Dissolve 10.85 g of N-(5-trifluoromethanesulfonic acid oxo-1-naphthalene)-acetamide obtained in step 2 in 50 mL of anhydrous DMF and stir to dissolve, add 0.43 g of nickel chloride and 8.66 g of triphenylphosphine. Slowly heat to 120° C. under nitrogen protection, react for 24 hours, and after the reaction is completed, filter and evaporate the solvent after cooling, and use ethyl acetate and n-heptane in a volume ratio of 1:4 as an eluent for column separation and purification to obtain 5.17 g of a yellow solid product, that is, alkyl acyl binaphthylamine, with a yield of 85%.
[0073] Step 4: Add 5.17 g of the yellow solid product obtained in step 3 to a mixed solution of 50 mL of 36% concentrated hydrochloric acid and 50 mL of ethanol, heat to 75°C and reflux for 3 h, filter and dry after cooling to obtain 3.79 g of a yellow solid product, namely, dinaphthylene diamine, with a yield of 95%.
[0074] Step 5: Dissolve 3.79 g of the dried dinaphthyl diamine in 20 mL of 1,2-dichlorobenzene, stir and heat to 120°C, slowly drop 45 g of triphosgene 1,2-dichlorobenzene solution into the diphenyl diamine solution, wherein the mass concentration of triphosgene 1,2-dichlorobenzene solution is 20%. The dropping time is 48 hours. After the dropping is completed, continue to heat and reflux for 4 hours until the reaction system is clear and transparent, remove the organic solvent by liquid separation, and obtain a crude product of p-phenylene diisocyanate. The crude product is recrystallized in xylene to obtain 4.08 g of a yellow solid product, that is, 5-position dinaphthyl diisocyanate, with a yield of 91%.
[0075] The product identification data are as follows:
[0076] GC-MS: 336.09;
[0077] Determination by nuclear magnetic resonance: 1H NMR (400MHz, DMSO-d6) δ: 8.77 (d, 2H, Ar-H), 8.55 (d, 2H, Ar-H), 8.41 (d, 2H, Ar-H), 7.78 (t, 2H, Ar-H), 7.74 (d, 2H, Ar-H), 7.37 (t, 2H, Ar-H);
[0078] 13C NMR(101MHz,DMSO-d6)δ:135.0,134.2,132.3,131.4,131.1,128.4,127.9,127.7,127.2,125.5,118.0
[0079] Comparative Example 1:
[0080] 1,5-Naphthalene diisocyanate (hereinafter referred to as NDI) was purchased from Qingdao Dexin Chemical Co., Ltd., with CAS number: 3173-72-6.
[0081] The performance test was conducted on the urethane prepared by the prepolymerization method using the No. 5 binaphthyl diisocyanate described in Example 1 and the NDI described in Comparative Example 1.
[0082] In the following Application Examples 1 and 2, the No. 5 binaphthyl diisocyanate prepared in Example 1 has an NCO (isocyanate) content of 21.88%; the NDI in Comparative Example 1 has an NCO (isocyanate) content of 40.0%; polyether triol EP-3600 was purchased from Shandong Bluestar Dongda Chemical Co., Ltd., with a molecular weight of 5000, a hydroxyl value of 26 to 30 mgKOH / g, and a moisture content of ≤0.05%; pentafluorobutane HFC-365MFC was purchased from Shandong Orilon Chemical Co., Ltd., CAS No.: 406-58-6, and a general-purpose silicone surfactant SH-493 was purchased from Hubei Longsheng Sihai New Materials Co., Ltd.
[0083] Application Example 1:
[0084] A method for preparing binaphthyl polyurethane by a prepolymer method comprises the following steps:
[0085] (1) reacting an excess of the 5-binaphthyl diisocyanate of Example 1 with polyether triol EP-3600 at 85° C. to form a prepolymer having a terminal -NCO group content of 8.5%;
[0086] (2) Casting: The prepolymer and the chain extender component are mixed in a mass ratio of 100:11.5, the mixing speed is 2000 r / min, and the mixture is stirred for 30 seconds. The reaction liquid is injected into a mold at a temperature of 90° C., and demolded after pre-aging; wherein the chain extender component comprises the following components in parts by weight: 60 parts of chain extender 1,4-butanediol, 30 parts of catalyst triethylenediamine, 5 parts of foaming agent pentafluorobutane HFC-365MFC, and 5 parts of surfactant SH-493;
[0087] (3) Post-curing: The demoulded product was cured in an oven at 110°C for 12 hours and then placed at room temperature for 5 days to obtain binaphthyl polyurethane.
[0088] Application Example 2:
[0089] The difference from Application Example 1 is that the 5-position binaphthyl diisocyanate in Example 1 is replaced by NDI in Comparative Example 1.
[0090] The properties of the polyurethane prepared in Application Example 1 and Application Example 2 were tested, and the results are shown in Table 1.
[0091] Table 1 Polyurethanes prepared by prepolymerization process
[0092] Test items unit Experimental methods Application Example 1 Application Example 2 density g / cm3 GB / T 1033.1-2008 1.07 1.05 Tensile Strength MPa GB / T 1040-2006 4.9 3.4 Tensile elongation % GB / T 528-2009 306 261 Shaw A HA GB T 2411-2008 82 73 Tear Strength kN / m GB / T 10808-2006 4.8 3.4 Loss Factor GB / T 18258-2000 0.43 0.35
[0093] According to Table 1, the binaphthyl polyurethane prepared by the prepolymerization method using the 5-position binaphthyl diisocyanate of the present invention has better tensile strength, tensile elongation and tear strength than the polyurethane prepared by the prepolymerization method using NDI in the same process, and has a higher loss factor. The above data illustrate that the carbamate product prepared by the method of the present invention has excellent performance and outstanding mechanical strength and shock absorption characteristics.
[0094] The description of the above embodiments is only for the convenience of understanding and use by technicians in this field. Those skilled in the art can select appropriate production processes according to product needs. Of course, the above description is only part of the embodiments of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A 5-binaphthyl diisocyanate, characterized in that: The invention is prepared by acylation reaction of naphthylamine, Ullmann coupling reaction with metal or its salt as catalyst in the presence of ligand and under the protection of inert gas, amide hydrolysis and subsequent carbonylation reaction with carbonylation agent.
2. A No. 5 binaphthyl diisocyanate according to claim 1, characterized in that: The structure of the naphthylamine is shown in the following formula (I), wherein X is chlorine, bromine, iodine, trifluoromethanesulfonyloxy, p-toluenesulfonyloxy or phenolic hydroxyl group.
3. A No. 5 binaphthyl diisocyanate according to claim 1, characterized in that: The structure of the product after the acylation reaction of naphthylamine is shown in the following formula (II), wherein R1 is C1~C 10 Straight or branched alkyl, C1~C 10 Alkoxy or C1~C 10 X is chlorine, bromine, iodine, trifluoromethanesulfonyloxy, p-toluenesulfonyloxy or phenolic hydroxyl.
4. A No. 5 binaphthyl diisocyanate according to claim 3, characterized in that: The structure of the product generated by the Ullmann coupling reaction is as follows: 10 Straight or branched alkyl, C1~C 10 Alkoxy or C1~C 10 The alkylthio group, 5. A No. 5 binaphthyl diisocyanate according to claim 1, characterized in that: The structure of the product generated by the amide hydrolysis reaction is shown in the following formula (IV):
6. A No. 5 binaphthyl diisocyanate according to claim 1, characterized in that: The structure of the product generated by the carbonylation reaction is shown in the following formula (V):
7. A method for synthesizing 5-binaphthyl diisocyanate according to any one of claims 1 to 6, characterized in that: The steps include: Step 1, naphthylamine, preferably halogenated naphthylamine or phenolic hydroxy naphthylamine, undergoes acylation reaction with an acylating agent to generate halogenated acyl naphthylamine or phenolic hydroxy acyl naphthylamine; Step 2: The halogenated acyl naphthylamine or phenolic hydroxyl acyl naphthylamine in step 1 is dissolved in an organic solvent, and an Ullmann reaction is carried out in the presence of a ligand and under the protection of an inert gas using a metal or a salt thereof as a catalyst to generate an alkyl acyl binaphthylamine; Step 3: The alkyl acyl binaphthylamine in step 2 is heated under reflux with a small molecule alkyl alcohol solution under strong acid conditions to undergo a hydrolysis reaction to generate binaphthyl diamine; Step 4: The dinaphthyl diamine in step 3 is subjected to carbonylation reaction to generate 5-position dinaphthyl diisocyanate.
8. A method for synthesizing No. 5 binaphthyl diisocyanate according to claim 7, characterized in that: The acylating agent in step 1 is any one of carboxylic acid, carboxylic acid ester, acid anhydride and acid chloride.
9. Use of a No. 5 binaphthyl diisocyanate according to any one of claims 1 to 8 or a No. 5 binaphthyl diisocyanate synthesized according to the synthesis method of claim 7 in the preparation of urethane rubber and elastomer, urethane fiber, cast urethane rubber, urethane emulsion and coating, urethane adhesive, shock-absorbing foam material, energy-absorbing foam material, and damping foam material.
10. A urethane material, characterized in that: The invention is prepared by using a No. 5 binaphthyl diisocyanate as described in any one of claims 1 to 6 or a No. 5 binaphthyl diisocyanate synthesized by the synthesis method as described in claims 7 to 8.
Citation Information
Patent Citations
Low-compression-deformation special microporous polyurethane elastomer and preparation method thereof
CN104262583A
1, 5-naphthalene diisocyanate prepolymer as well as preparation method and application thereof
CN114015009A
1, 6-pyrene diisocyanate, preparation method thereof and application of 1, 6-pyrene diisocyanate in modified polyurethane elastomer