Preparation method of aminophenyl oligomeric silsesquioxane

By using diboron compounds as reducing agents to prepare aminophenyl oligomeric silsesquioxanes under catalyst-free conditions, the problem of silicon-oxygen bond breakage under alkaline conditions in the existing technology is solved, and structural stability and cost are achieved. Reduced, suitable for the preparation of high-performance polymer materials.

CN118745247AActive Publication Date: 2024-10-08BEIJING INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410725411.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-08
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

When preparing aminophenyl oligomeric silsesquioxane in the prior art, the silicon-oxygen bond is easily broken under alkaline conditions, destroying the cage structure and affecting its application in polymer materials.

Method used

Using a diboron compound as a reducing agent, the reduction reaction is carried out without a catalyst or a catalyst such as 4,4'-bipyridine to obtain structurally stable aminophenyl oligomeric silsesquioxane, simplifying the preparation process and reducing costs. and increase the reaction rate.

Benefits of technology

The structural stability of aminophenyl oligomeric silsesquioxane is achieved, which is suitable for the preparation of high-performance polymer materials, reduces the preparation cost, and improves the universality and environmental friendliness of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745247A_ABST
    Figure CN118745247A_ABST
Patent Text Reader

Abstract

The invention provides aminophenyl oligomeric silsesquioxane, a preparation method and application thereof and a polymer material, and belongs to the technical field of organic-inorganic hybrid materials. The invention provides a preparation method of aminophenyl oligomeric silsesquioxane, which comprises the following steps: mixing nitrophenyl oligomeric silsesquioxane, a reducing agent and a solvent, and carrying out reduction reaction in the absence of a catalyst or under the condition of taking at least one of 4, 4 '-dipyridyl, diphenylamine, 2, 2'-dipyridyl and pyridine as a catalyst, thereby obtaining the aminophenyl oligomeric silsesquioxane. The amino phenyl oligomeric silsesquioxane is obtained; the reducing agent is a diboron compound. The preparation method provided by the invention is high in yield, strong in universality, low in cost, environment-friendly and suitable for industrial production; the prepared aminophenyl oligomeric silsesquioxane is good in structural stability and can be used for preparing high-performance polymer materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic-inorganic hybrid materials, and specifically relates to an aminophenyl oligomeric silsesquioxane and a preparation method and application thereof, and a polymer material. Background Art

[0002] Polyhedral oligomeric silsesquioxane (POSS) is a nano-sized organic-inorganic hybrid material that has the advantages of both organic and inorganic materials. Among them, phenyl POSS is a class of 1.5 ) n Oligomeric silsesquioxanes contain cage-shaped rigid inorganic Si-O-Si cores. Phenyl POSS is prepared together with a polymer matrix to improve the thermal stability, flame retardancy, mechanical properties and dielectric properties of the obtained polymer material. However, due to the poor solubility of phenyl POSS, it is mostly dispersed in the polymer matrix in the form of microparticles, which is easy to be unevenly dispersed, affecting the performance of the polymer material. Amino compounds have good chemical reactivity and solubility and can react with a variety of groups. Therefore, phenyl is converted into aminophenyl by the side group conversion method, which can enhance the solubility and reactivity of phenyl POSS in the polymer matrix, so that it can be dispersed at the molecular level in the polymer matrix by physical mixing or chemical reaction. Therefore, the synthesis and preparation of aminophenyl POSS is of great significance.

[0003] At present, in the prior art, aminophenyl POSS is usually prepared by using hydrazine hydrate as a reducing agent in the presence of a catalyst. For example, a method for preparing aminophenyl silsesquioxane is disclosed in a patent with an authorization publication number of CN 100412077C, which uses Fe / C as a catalyst; a method for preparing octaaminophenyl cage-shaped silsesquioxane is disclosed in a patent with an authorization publication number of CN 100430406C, which uses an aluminum compound or a mixture of aluminum and iron compounds as a catalyst; and a method for preparing cage-type oligomeric octaaminophenyl oligomeric silsesquioxane is disclosed in a patent with a publication number of CN 102391303A, which uses ferric chloride and palladium on carbon as catalysts.

[0004] The above three existing solutions all use hydrazine hydrate with strong alkalinity as a reducing agent, but the silicon-oxygen bond is easily broken under alkaline conditions, and the cage structure of the resulting cage-shaped octaaminophenyl oligomeric silsesquioxane may be destroyed, which is not conducive to its application in polymer materials. Summary of the invention

[0005] The purpose of the present invention is to provide an aminophenyl oligomeric silsesquioxane and its preparation method and application, and polymer material. The aminophenyl oligomeric silsesquioxane obtained according to the preparation method provided by the present invention has good structural stability and can be used to prepare high-performance polymer materials.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing aminophenyl oligomeric silsesquioxane, comprising the following steps:

[0008] Nitrophenyl oligomeric silsesquioxane, a reducing agent and a solvent are mixed, and a reduction reaction is carried out in the absence of a catalyst or with at least one of 4,4'-bipyridine, diphenylamine, 2,2'-bipyridine and pyridine as a catalyst to obtain aminophenyl oligomeric silsesquioxane; the reducing agent is a diboron compound.

[0009] Preferably, the nitrophenyl oligomeric silsesquioxane includes at least one of T8 cage-shaped nitrophenyl oligomeric silsesquioxane, T12 cage-shaped nitrophenyl oligomeric silsesquioxane and Tn ring ladder nitrophenyl oligomeric silsesquioxane.

[0010] Preferably, the diboron compound comprises at least one of tetrahydroxydiboron, neopentyl glycol diborate, pinacol diborate and bis(bis(diphenyl))boric acid; and the molar ratio of the nitro functional group of the nitrophenyl oligomeric silsesquioxane to the reducing agent is 1:1-6.

[0011] Preferably, the solvent comprises at least one of ethanol, ethyl acetate, dichloromethane, tetrahydrofuran and N,N-dimethylformamide; and the solid-liquid ratio of the nitrophenyl oligomeric silsesquioxane to the solvent is 1 g: 1 to 40 mL.

[0012] Preferably, the amount of substance of the catalyst does not exceed 5% of the amount of substance of the nitro functional groups of the nitrophenyl oligomeric silsesquioxane.

[0013] Preferably, the reduction reaction is carried out in an inert atmosphere; the inert atmosphere comprises at least one of nitrogen and argon.

[0014] Preferably, the reduction reaction is carried out at a temperature of 20 to 80° C. and for a time of 2 to 24 hours.

[0015] The present invention provides aminophenyl oligomeric silsesquioxane prepared by the preparation method described in the above technical scheme.

[0016] The present invention provides application of the aminophenyl oligomeric silsesquioxane described in the above technical solution in polymer materials.

[0017] The present invention provides a polymer material, comprising the aminophenyl oligomeric silsesquioxane described in the above technical solution and a polymer matrix; the polymer matrix comprises at least one of epoxy resin and polyimide.

[0018] The present invention provides a method for preparing aminophenyl oligomeric silsesquioxane, comprising the following steps: mixing nitrophenyl oligomeric silsesquioxane, a reducing agent and a solvent, and performing a reduction reaction in the absence of a catalyst or with at least one of 4,4'-bipyridine, diphenylamine, 2,2'-bipyridine and pyridine as a catalyst to obtain aminophenyl oligomeric silsesquioxane; the reducing agent is a diboron compound. The present invention adopts a diboron compound as a reducing agent, which can achieve reduction without expensive catalysts on the one hand, simplify the preparation process and reduce the preparation cost; on the other hand, the diboron compound is used in combination with a catalyst such as 4,4'-bipyridine to construct an efficient catalytic system, which greatly improves the reaction rate. The preparation method of the present invention has mild and stable reaction conditions and is suitable for the reduction of different nitrophenyl oligomeric silsesquioxanes; the process has good repetition and strong universality, and also has the characteristics of low cost, environmental friendliness and simple operation, and is suitable for industrial production. At the same time, the preparation method provided by the present invention has high yield, good structural stability of the obtained aminophenyl oligomeric silsesquioxane, and is suitable for expanded production.

[0019] Furthermore, the aminophenyl oligomeric silsesquioxane obtained according to the preparation method of the present invention can be further reacted to obtain POSS containing different functional groups, and can also be introduced into polymer matrices such as epoxy resins and polyimides through various means such as grafting, crosslinking and copolymerization, thereby improving the flame retardant, dielectric, mechanical and other properties of the obtained polymer material. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0021] Figure 1 FTIR spectrum of T8 cage-shaped aminophenyl oligomeric silsesquioxane prepared in Example 1;

[0022] Figure 2 The T8 cage-shaped aminophenyl oligomeric silsesquioxane prepared in Example 1 1 H NMR spectrum;

[0023] Figure 3 This is the mass spectrum of T8 cage-shaped aminophenyl oligomeric silsesquioxane prepared in Example 1. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing aminophenyl oligomeric silsesquioxane, comprising the following steps:

[0025] Nitrophenyl oligomeric silsesquioxane, a reducing agent and a solvent are mixed, and a reduction reaction is carried out in the absence of a catalyst or with at least one of 4,4'-bipyridine, diphenylamine, 2,2'-bipyridine and pyridine as a catalyst to obtain aminophenyl oligomeric silsesquioxane; the reducing agent is a diboron compound.

[0026] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art or are prepared by methods well known to those skilled in the art.

[0027] The invention mixes nitrophenyl oligomeric silsesquioxane, a reducing agent and a solvent, and performs a reduction reaction in the absence of a catalyst or with 4,4'-bipyridine as a catalyst to obtain aminophenyl oligomeric silsesquioxane.

[0028] In the present invention, the nitrophenyl oligomeric silsesquioxane preferably includes at least one of T8 cage-shaped nitrophenyl oligomeric silsesquioxane, T12 cage-shaped nitrophenyl oligomeric silsesquioxane and Tn ring ladder nitrophenyl oligomeric silsesquioxane, more preferably T8 cage-shaped nitrophenyl oligomeric silsesquioxane, T12 cage-shaped nitrophenyl oligomeric silsesquioxane or Tn ring ladder nitrophenyl oligomeric silsesquioxane. The T8 cage-shaped nitrophenyl oligomeric silsesquioxane (nitro functionality is 1 to 8) of the present invention is preferably T8 cage-shaped low nitro functionality phenyl cage-shaped silsesquioxane (nitro functionality is 1 to 7); the T12 cage-shaped nitrophenyl oligomeric silsesquioxane (nitro functionality is 1 to 12) preferably includes T12 cage-shaped low nitro functionality phenyl oligomeric silsesquioxane (nitro functionality is 1 to 11).

[0029] In the present invention, the reducing agent is a diboron compound; the diboron compound preferably includes at least one of tetrahydroxydiboron, neopentyl glycol diborate, pinacol diborate and bis-dipyrocatechol boric acid, and is more preferably tetrahydroxydiboron or neopentyl glycol diborate. The molar ratio of the nitro functional group of the nitrophenyl oligomeric silsesquioxane of the present invention to the reducing agent is preferably 1:1-6, more preferably 1:2-5.

[0030] In the present invention, the solvent preferably includes at least one of ethanol, ethyl acetate, dichloromethane, tetrahydrofuran and N,N-dimethylformamide, more preferably dichloromethane or N,N-dimethylformamide. The material-liquid ratio of the nitrophenyl oligomeric silsesquioxane of the present invention to the solvent is preferably 1g: 1-40mL, more preferably 1g: 10-30mL.

[0031] The present invention performs a reduction reaction without a catalyst or with at least one of 4,4'-bipyridine, diphenylamine, 2,2'-bipyridine and pyridine as a catalyst. In the present invention, when a catalyst is used for the reduction reaction, the catalyst is preferably 4,4'-bipyridine. In the present invention, the amount of the catalyst is preferably not more than 5% of the amount of the nitro functional group of the nitrophenyl oligomeric silsesquioxane, and more preferably not more than 4% of the amount of the nitro functional group of the nitrophenyl oligomeric silsesquioxane. In one embodiment of the present invention, the amount of the catalyst is 0. In another embodiment of the present invention, the amount of the catalyst is 0.1 to 3% of the amount of the nitro functional group of the nitrophenyl oligomeric silsesquioxane.

[0032] The reduction reaction of the present invention is preferably carried out in an inert atmosphere; the inert atmosphere preferably includes at least one of nitrogen and argon, more preferably nitrogen. The temperature of the reduction reaction of the present invention is preferably 20 to 80°C, more preferably 30 to 50°C, and the time is preferably 2 to 24 hours, more preferably 10 to 24 hours. The reduction reaction of the present invention is preferably carried out under stirring.

[0033] After the reduction reaction, the present invention preferably mixes the obtained material with ethyl acetate, washes with saturated brine, separates the liquids, mixes the obtained organic phase with a precipitant, and precipitates; collects the precipitate by solid-liquid separation, and dries the precipitate to obtain aminophenyl oligomeric silsesquioxane. In the present invention, the number of washings is preferably 2 to 3 times, more preferably 3 times. In the present invention, the precipitant is preferably at least one of n-hexane, petroleum ether, benzene, water and cyclohexane, more preferably n-hexane or petroleum ether; the volume ratio of the organic phase to the precipitant is preferably 1:1 to 20, more preferably 1:5 to 15. The solid-liquid separation of the present invention is preferably suction filtration; the drying is preferably vacuum drying.

[0034] The present invention also provides an aminophenyl oligomeric silsesquioxane prepared by the preparation method described in the above technical solution. The aminophenyl oligomeric silsesquioxane described in the present invention preferably includes at least one of T8 cage-type aminophenyl oligomeric silsesquioxane, T12 cage-type aminophenyl oligomeric silsesquioxane and Tn ring ladder aminophenyl oligomeric silsesquioxane, and more preferably T8 cage-type aminophenyl oligomeric silsesquioxane, T12 cage-type aminophenyl oligomeric silsesquioxane or Tn ring ladder aminophenyl oligomeric silsesquioxane.

[0035] In the present invention, when the nitrophenyl oligomeric silsesquioxane is T8 cage-type nitrophenyl oligomeric silsesquioxane, the obtained aminophenyl oligomeric silsesquioxane is preferably T8 cage-type aminophenyl oligomeric silsesquioxane. The T8 cage-type aminophenyl oligomeric silsesquioxane of the present invention preferably has a structure shown in Formula I:

[0036]

[0037] In formula I, each R is independently phenyl or aminophenyl, and at least one R is aminophenyl.

[0038] In the present invention, when the nitrophenyl oligomeric silsesquioxane is a T8 cage-type low-nitro-functionality phenyl cage-type silsesquioxane, the obtained aminophenyl oligomeric silsesquioxane is preferably a T8 cage-type aminophenyl oligomeric silsesquioxane.

[0039] In the present invention, when the nitrophenyl oligomeric silsesquioxane is T12 cage-shaped nitrophenyl oligomeric silsesquioxane, the obtained aminophenyl oligomeric silsesquioxane is preferably T12 cage-shaped aminophenyl oligomeric silsesquioxane. The T12 cage-shaped aminophenyl oligomeric silsesquioxane of the present invention preferably has a structure shown in Formula II:

[0040]

[0041] In formula II, each R is independently phenyl or aminophenyl, and at least one R is amino.

[0042] In the present invention, when the nitrophenyl oligomeric silsesquioxane is a T12 cage-shaped low-nitro-functionality phenyl cage-shaped silsesquioxane, the obtained aminophenyl oligomeric silsesquioxane is preferably a T12 cage-shaped aminophenyl oligomeric silsesquioxane.

[0043] In the present invention, when the nitrophenyl oligomeric silsesquioxane is a Tn ring ladder nitrophenyl oligomeric silsesquioxane, the obtained aminophenyl oligomeric silsesquioxane is preferably a Tn ring ladder aminophenyl oligomeric silsesquioxane. The Tn ring ladder aminophenyl oligomeric silsesquioxane of the present invention preferably has a structure shown in Formula III:

[0044]

[0045] In formula III, n≥2 (preferably n=30) and n is an integer; each R is independently a phenyl group or an aminophenyl group, and at least one R is an amino group.

[0046] The present invention also provides application of the aminophenyl oligomeric silsesquioxane described in the above technical solution in polymer materials.

[0047] The present invention also provides a polymer material, comprising the aminophenyl oligomeric silsesquioxane described in the above technical solution and a polymer matrix; the polymer matrix comprises at least one of epoxy resin and polyimide, preferably epoxy resin or polyimide.

[0048] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] The three-necked flask used in the examples is provided with a reflux condenser, a constant pressure dropping funnel, a temperature control device, a nitrogen protection device and a magnetic stirring device.

[0050] Example 1

[0051] 1) 5 g of T8 cage-shaped nitrophenyl oligomeric silsesquioxane, 0.023 g of 4,4'-bipyridine and 100 mL of N,N-dimethylformamide were added to a three-necked flask to obtain a mixed solution; 50 mL of N,N-dimethylformamide solution containing 8 g of tetrahydroxydiboron was added dropwise to the mixed solution under stirring and nitrogen protection, and after the addition was completed, the mixture was reacted at 30° C. for 10 h, and a reaction solution was obtained after the reaction was completed;

[0052] 2) 100 mL of ethyl acetate was added to the reaction solution, and the mixture was washed three times with saturated brine. The organic phase was poured into 200 mL of n-hexane to precipitate a precipitate (light brown); the precipitate was filtered and the obtained solid material was vacuum dried to obtain T8 cage-shaped aminophenyl oligomeric silsesquioxane with a yield of 88.7%.

[0053] The T8 cage-shaped aminophenyl oligomeric silsesquioxane obtained in Example 1 was subjected to infrared spectroscopy, nuclear magnetic resonance hydrogen spectrum detection and mass spectrometry detection, and the results were as follows: Figure 1 , 2 and 3.

[0054] Depend on Figure 1 It can be seen that at 3500cm -1 The characteristic absorption peak of the -OH group nearby, 1080 cm -1 The absorption peak at 3480.2 cm is attributed to the vibration of Si-O-Si bonds, which preliminarily indicates that most or all of the siloxane cage structures remain intact. -1 、3360.6cm -1 and 3220.3cm -1 The characteristic absorption peak of the amino group is not present at 1530 cm -1 、1350cm -1 It can be preliminarily determined that the cage-shaped octanonitrophenyl oligomeric silsesquioxane is quantitatively converted into the cage-shaped octanaminophenyl oligomeric silsesquioxane.

[0055] Figure 2 In T8 cage-shaped aminophenyl oligosilsesquioxane, H is located on the amino group and the benzene ring, respectively, among which 6.0-8.0 ppm is the peak of the hydrogen atom on the phenyl group, 4.0-6.0 ppm is the peak of the hydrogen atom on the amino group, and the ratio of the integrated area of ​​the amino hydrogen atom peak to the integrated area of ​​the phenyl hydrogen atom peak is close to the theoretical value of 0.5:1, indicating that the nitro groups connected to the benzene ring are successfully reduced to amino groups.

[0056] Finally, the characterization method commonly used to measure the molecular weight of octaaminophenyl oligomeric silsesquioxane is GPC. The present invention introduces MALDI TOF MS to characterize the molecular weight. Figure 3 It can be seen that the T8 cage-shaped aminophenyl oligomeric silsesquioxane prepared by the present invention has a stable structure. The results show that the present invention synthesizes a structurally complete octaaminophenyl oligomeric silsesquioxane, further illustrating the mildness and effectiveness of the preparation method of the present invention.

[0057] Example 2

[0058] 1) adding 10 g of T8 cage-shaped nitrophenyl oligomeric silsesquioxane and 100 mL of N,N-dimethylformamide into a three-necked flask to obtain a mixed solution; adding 100 mL of N,N-dimethylformamide solution containing 15 g of tetrahydroxydiboron to the mixed solution under stirring and nitrogen protection, and reacting at 60° C. for 24 h to obtain a reaction solution after completion;

[0059] 2) 200 mL of ethyl acetate was added to the reaction solution, and the mixture was washed three times with saturated brine. The organic phase was poured into 400 mL of n-hexane to precipitate a precipitate (light brown); the precipitate was filtered and the obtained solid material was vacuum dried to obtain T8 cage-shaped aminophenyl oligomeric silsesquioxane with a yield of 85.7%.

[0060] Example 3

[0061] 1) 5 g of T8 cage-shaped low-nitro-functionality phenyl cage-shaped silsesquioxane, 0.023 g of 4,4'-bipyridine and 100 mL of N,N-dimethylformamide were added to a three-necked flask to obtain a mixed solution; 50 mL of N,N-dimethylformamide solution containing 8 g of tetrahydroxydiboron was added dropwise to the mixed solution under stirring and nitrogen protection. After the addition was completed, the mixture was reacted at 30° C. for 10 h, and a reaction solution was obtained after the reaction was completed;

[0062] 2) 200 mL of ethyl acetate was added to the reaction solution, and the mixture was washed three times with saturated brine. The organic phase was poured into 200 mL of n-hexane to precipitate a precipitate (light brown); the precipitate was filtered and the obtained solid material was vacuum dried to obtain T8 cage-shaped low-amino-functional phenyl oligomeric silsesquioxane with a yield of 82.6%.

[0063] Example 4

[0064] 1) 5 g of T12 cage-shaped nitrophenyl oligomeric silsesquioxane, 0.025 g of 4,4'-bipyridine and 100 mL of N,N-dimethylformamide were added to a three-necked flask to obtain a mixed solution; 50 mL of N,N-dimethylformamide solution containing 12 g of tetrahydroxydiboron was added dropwise to the mixed solution under stirring and nitrogen protection. After the addition was completed, the mixture was reacted at 30° C. for 24 h, and a reaction solution was obtained after the reaction was completed;

[0065] 2) 200 mL of ethyl acetate was added to the reaction solution, and the mixture was washed three times with saturated brine. The organic phase was poured into 400 mL of n-hexane to precipitate a precipitate (light brown); the precipitate was filtered and the obtained solid material was vacuum dried to obtain T12 cage-shaped aminophenyl oligomeric silsesquioxane with a yield of 80.5%.

[0066] Example 5

[0067] 1) 5 g of T12 cage-shaped low-nitro-functional phenyl oligomeric silsesquioxane, 0.025 g of 4,4'-bipyridine and 100 mL of N,N-dimethylformamide were added to a three-necked flask to obtain a mixed solution; 75 mL of N,N-dimethylformamide solution containing 12 g of tetrahydroxydiboron was added dropwise to the mixed solution under stirring and nitrogen protection. After the addition was completed, the mixture was reacted at 25° C. for 24 h, and a reaction solution was obtained after the reaction was completed;

[0068] 2) 200 mL of ethyl acetate was added to the reaction solution, and the mixture was washed three times with saturated brine. The organic phase was poured into 400 mL of n-hexane to precipitate a precipitate (light brown); the precipitate was filtered and the obtained solid material was vacuum dried to obtain T12 cage-shaped low-amino-functional phenyl oligomeric silsesquioxane in a yield of 78.5%.

[0069] Comparative Example 1

[0070] The experiment was conducted with reference to the patent publication number CN 102391303A, and the specific operation is as follows:

[0071] 1) Weigh 15 g of T8 cage-shaped nitrophenyl oligomeric silsesquioxane into a three-necked flask, dissolve it with 120 mL of tetrahydrofuran, then add 1.83 g of 5% Pd / C catalyst and 0.69 of ferric chloride hexahydrate, heat to 60° C., slowly dropwise add 48 mL of 80% hydrazine hydrate under nitrogen protection, reflux for 12 h, and obtain a reaction solution after completion;

[0072] 2) 120 mL of ethyl acetate was added to the reaction solution, and the mixture was allowed to stand until the black catalyst Pd / C layer was separated from the organic layer. The organic layer was filtered, washed with 360 mL of saturated brine, dried over anhydrous sodium sulfate, poured into 1000 mL of n-hexane, and a white precipitate was precipitated. The precipitate was filtered and dried in a vacuum oven to obtain T8 cage-shaped low-amino-functional phenyl oligomeric silsesquioxane with a yield of 75.2%.

[0073] The product yield of Comparative Example 1 is significantly lower than that of Examples 1 to 3, and a noble metal catalyst is used in Comparative Example 1, which increases the cost and the complexity of post-processing.

[0074] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing aminophenyl oligomeric silsesquioxane, comprising the following steps: Nitrophenyl oligomeric silsesquioxane, a reducing agent and a solvent are mixed, and a reduction reaction is carried out in the absence of a catalyst or with at least one of 4,4'-bipyridine, diphenylamine, 2,2'-bipyridine and pyridine as a catalyst to obtain aminophenyl oligomeric silsesquioxane; the reducing agent is a diboron compound.

2. The preparation method according to claim 1, characterized in that: The nitrophenyl oligomeric silsesquioxane includes at least one of T8 cage-shaped nitrophenyl oligomeric silsesquioxane, T12 cage-shaped nitrophenyl oligomeric silsesquioxane and Tn ring ladder nitrophenyl oligomeric silsesquioxane.

3. The preparation method according to claim 1, characterized in that: The diboron compound comprises at least one of tetrahydroxydiboron, neopentyl glycol diborate, pinacol diborate and bis(bis(diphenyl)phenol)boric acid; the molar ratio of the nitro functional group of the nitrophenyl oligomeric silsesquioxane to the reducing agent is 1:1-6.

4. The preparation method according to claim 1, characterized in that: The solvent comprises at least one of ethanol, ethyl acetate, dichloromethane, tetrahydrofuran and N,N-dimethylformamide; the solid-liquid ratio of the nitrophenyl oligomeric silsesquioxane to the solvent is 1 g: 1-40 mL.

5. The preparation method according to claim 1, characterized in that: The amount of the catalyst does not exceed 5% of the amount of the nitro functional groups of the nitrophenyl oligomeric silsesquioxane.

6. The preparation method according to claim 1, characterized in that: The reduction reaction is carried out in an inert atmosphere; the inert atmosphere includes at least one of nitrogen and argon.

7. The preparation method according to claim 1 or 6, characterized in that: The temperature of the reduction reaction is 20-80° C. and the time is 2-24 hours.

8. Aminophenyl oligomeric silsesquioxane prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the aminophenyl oligomeric silsesquioxane according to claim 8 in polymer materials.

10. A polymer material comprising the aminophenyl oligomeric silsesquioxane of claim 8 and a polymer matrix; the polymer matrix comprises at least one of an epoxy resin and a polyimide.

Citation Information

Patent Citations

  • Process for preparing amino phenyl silsesquioxane

    CN100412077C

  • Method for preparing octamido phenyl silsesquixanes

    CN100430406C

  • Preparation method of cage-type oligomeric octa(aminophenyl) polyhedral silsesquioxane (OAPS)

    CN102391303A

  • Industrialized synthetic method of vismodegib

    CN104496889A