Biodegradable PE wrapping film and processing technology thereof
By using a combination of composite polyol ester and cubic nanometer calcium carbonate and polyvinyl ester in PE stretch film, the problems of poor biodegradability and mechanical properties of traditional PE stretch film are solved, achieving higher environmental friendliness and Mechanical properties, reducing environmental pollution.
Patent Information
- Application Number
- CN202410742377.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional PE stretch film has poor biodegradability and mechanical properties, leading to environmental pollution problems.
A combination of composite polyol ester, cubic nanometer calcium carbonate and polyvinyl ester is used to prepare composite materials through esterification and polycondensation reactions. Silane coupling agents and defoaming agents are added to the processing process to form a composite material with excellent biodegradability. and mechanical properties of PE stretch film.
It improves the biodegradability and mechanical properties of PE stretch film, enhances its thermal stability and impact resistance at high temperatures, and reduces environmental pollution.
Smart Images

Figure BDA0004885250890000031 
Figure BDA0004885250890000141 
Figure BDA0004885250890000142
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PE stretch films, and in particular relates to a biodegradable PE stretch film and a processing technology thereof. Background Art
[0002] PE stretch film is a kind of plastic film. PE stretch film has high tensile strength, tear strength, and good self-adhesion, so it can wrap objects into a whole to prevent them from scattering and collapsing during transportation; PE stretch film has excellent transparency, making the wrapped objects beautiful and elegant, and can make the objects waterproof, dustproof, and damage-proof; PE stretch film is widely used in various fields, but traditional PE stretch film has poor biodegradability, is not easy to decompose, and is easy to cause environmental pollution. With the improvement of environmental awareness, the environmental protection of PE stretch film needs to be improved.
[0003] Patent CN 112708247 A discloses a resin modification and preparation method for producing a stretch film using biodegradable materials. The invention uses degradable materials to produce degradable stretch films for industrial applications, solving the technical difficulties of producing stretch films using fully biodegradable materials and the production process difficulties, and also solving the environmental pollution problems caused by the use of stretch films. The materials used in the invention include the following components, by weight: 2-10 parts of polylactic acid; 90-98 parts of polybutylene adipate / terephthalate; 2-5 parts of nano-calcium carbonate; 0.2-0.5 parts of octadecyl acrylate-maleic anhydride; 0.2-0.6 parts of chain extender; 0.2-0.8 parts of antioxidant; 0.2-0.5 parts of lubricant. The raw materials used are fully biodegradable materials, which are environmentally friendly. Part of the materials are modified, and butylene terephthalate does not need to be modified again for direct production, which reduces the damage to the molecular structure of the raw materials. However, the biodegradability and mechanical properties of the obtained stretch film still have room for improvement. Summary of the invention
[0004] The object of the present invention is to provide a PE stretch film with strong stretchability and a preparation method thereof, so as to solve the technical problems of poor biodegradability and mechanical properties of the PE stretch film in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention provides a biodegradable PE wrapping film, which is prepared from the following components in parts by weight: 12-18 parts of polyethylene ester, 15-20 parts of composite polyol ester, 2-4 parts of cubic nano calcium carbonate, 1-3 parts of silane coupling agent, and 1-2 parts of defoamer; wherein the composite polyol ester is obtained by reacting phenolphthalein-succinic acid, 2-butyl-1,3-propylene glycol and succinic anhydride, and the cubic nano calcium carbonate is obtained by multiphase reaction in a microemulsion system.
[0007] Preferably, the preparation method of the composite polyol ester comprises the following steps:
[0008] Q1: Add succinic anhydride, phenolphthalein and p-toluenesulfonic acid monohydrate into a three-necked flask, replace with nitrogen, and then heat. After the solid in the flask melts, stir vigorously and heat to carry out esterification reaction. After the reaction is completed, phenolphthalein-succinic acid is obtained;
[0009] Q2: Add 2-butyl-1,3-propanediol and phenolphthalein-succinic acid into a three-necked flask, add succinic anhydride and p-toluenesulfonic acid monohydrate at the same time, and replace with argon. After the replacement, heat and react after the succinic anhydride melts. After the reaction is completed, heat and carry out esterification reaction;
[0010] Q3: After the esterification reaction is completed, the temperature is lowered, and the vacuum distillation device is replaced. The catalysts tetrabutyl titanate and p-toluenesulfonic acid monohydrate are added. Under the protection of argon, the temperature is raised, and the vacuum is drawn to carry out the polycondensation reaction. After the reaction is completed, the temperature is lowered, chloroform is added to dissolve the polycondensation product, and then the product is poured into high-speed stirred anhydrous methanol to precipitate the final product. After filtration, it is dried to obtain a composite polyol ester.
[0011] In the above process, phenolphthalein-succinic acid is first prepared, and then phenolphthalein-succinic acid is used as raw materials to replace 2-butyl-1,3-propanediol for copolymerization reaction to synthesize composite polyol ester. The reaction process is as follows:
[0012]
[0013] Preferably, in Q1, the molar ratio of succinic anhydride to phenolphthalein is 1:(0.8-1.2), the three-necked flask is equipped with a water separator and a condenser, the nitrogen replacement times are 3-5 times, the heating temperature is 140-160°C, the vigorous stirring time is 30-50min, the heating temperature is 180-200°C, and the esterification reaction time is 3-4h.
[0014] Preferably, in Q2, the molar ratio of 2-butyl-1,3-propanediol, phenolphthalein-succinic acid and succinic anhydride is (1.6-2.4):(0.8-1.3):(0.7-1.3), the three-necked flask is equipped with a water separator and a condenser, the argon replacement times are 3-5 times, the heating temperature is 120-140°C, the reaction time is 20-40min, the heating temperature is 170-190°C, and the esterification reaction time is 3-4h.
[0015] Preferably, in Q3, the heating temperature is 230-250°C, the polycondensation reaction time is 1-2h, the drying temperature is 50-60°C, and the drying time is 48-54h.
[0016] Preferably, the method for preparing the cubic nano calcium carbonate comprises the following steps:
[0017] S1: Sodium hydroxide and calcium chloride are placed in a beaker and stirred, distilled water is added for dilution and stirring to obtain a microemulsion, and then the microemulsion, hexadecyltrimethylammonium bromide, n-pentanol and cyclohexane are mixed and stirred to form a stable reverse microemulsion;
[0018] S2: Add sucrose to the reverse microemulsion, introduce carbon dioxide gas into the reverse microemulsion, continue to introduce and stir continuously until no precipitation is produced, stop introducing carbon dioxide, let it stand for aging, wash, centrifuge, and dry to obtain cubic nano-calcium carbonate.
[0019] In the above process, the synthesis of cubic nano-calcium carbonate is achieved through a multiphase reaction in a microemulsion system, and the reaction equation is:
[0020] CaCl2+2NaOH→Ca(OH)2+2NaCl; Ca(OH)2+CO2→CaCO3+H2O
[0021] Sucrose is added as a crystal shape controller. The hydroxyl groups in sucrose have high electronegativity and attract each other with calcium ions in the reverse microemulsion through electrostatic matching, making the local calcium ion concentration supersaturated and promoting its nucleation. The introduced carbon dioxide will react with the calcium ions in the aqueous phase in a multiphase manner to form a large number of small crystal nuclei that can exist stably. These small crystal nuclei have a large surface energy, which makes the system tend to grow into larger calcium carbonate crystals and reduces the crystal surface energy of calcium carbonate. Sucrose combines with calcium ions on the surface of calcium carbonate crystals through its hydroxyl groups. The sucrose molecular groups will guide the calcium carbonate to arrange in an orderly manner according to a specific orientation to form cubic nano-calcium carbonate in the form of calcite crystals.
[0022] Preferably, in S1, the volume ratio of the microemulsion, hexadecyltrimethylammonium bromide, n-pentanol and cyclohexane is (1-3): (45-55): (6-10): (13-17), and the stirring time is 20-40 min; in S2, the dosage ratio of sucrose and reverse microemulsion is 1 g: (95-105) mL, the flow rate of carbon dioxide gas is 300-320 mL / min, the standing aging time is 22-26 h, the drying temperature is 70-80°C, and the drying time is 20-24 h.
[0023] Preferably, the processing technology of the biodegradable PE stretch film comprises the following steps:
[0024] Step (1): mixing polyvinyl ester, composite polyol ester, cubic nano calcium carbonate, silane coupling agent and defoaming agent and performing dust removal treatment;
[0025] Step (2): adding the dust-removed mixture evenly into an extruder, mixing it thoroughly and heating it to melt it into a melt, transferring the melt from the extruder to a casting machine, and processing it into a film layer, and the film layer forms a PE wrapping film under the action of a cooling roller on the casting machine.
[0026] Preferably, in step (2), the temperature of the melt is 250-280°C.
[0027] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0028] 1. In the present invention, an environmentally friendly composite polyol ester is first prepared, and the composite polyol ester is composited with polyvinyl ester. Meanwhile, cubic nano-calcium carbonate and a silane coupling agent are added during the composite process. The addition of the cubic nano-calcium carbonate can improve the mechanical properties of the composite material, and the addition of the silane coupling agent can improve the compatibility of the composite polyol ester and polyvinyl ester, so that a more uniform and stable composite material is formed. The PE wrapping film obtained by the method has not only excellent biodegradability, but also excellent mechanical properties.
[0029] 2. In the present invention, phenolphthalein-succinic acid is prepared with succinic anhydride and phenolphthalein, and then the phenolphthalein-succinic acid is reacted with 2-butyl-1,3-propanediol and succinic anhydride to prepare a composite polyol ester. The polar groups such as hydroxyl and carbonyl contained in the substance can enhance the interaction between polymer chains, form a tighter molecular structure, and improve the barrier properties of the material. The benzene ring and carbonyl contained in the phenolphthalein structure have high thermal stability and can maintain the stability of the structure at high temperatures. This stability can be transferred to the composite polyol ester, so that it exhibits better thermal stability during high-temperature processing and use. At the same time, the ester bond contained in the prepared composite polyol ester can undergo a hydrolysis reaction under appropriate conditions, thereby degrading the polymer. Using it as the main material of the PE wrap film can reduce the pollution to the environment after use.
[0030] 3. In the present invention, sodium hydroxide, calcium chloride, hexadecyltrimethylammonium bromide, n-pentanol, cyclohexane, sucrose and carbon dioxide gas are used as raw materials to prepare cubic nano calcium carbonate. The substance has a large specific surface area and high surface energy. When it is added to the PE wrap film, the interface between it and the PE matrix is more tightly bonded, which helps to reduce stress concentration and crack propagation, thereby improving the mechanical properties and impact resistance of the PE wrap film. In addition, the cubic nano calcium carbonate can fill the vacancies and defects in the PE matrix to form a physical barrier to prevent the penetration of oxygen, moisture and other gases. At the same time, it can withstand high temperatures without decomposition or deterioration, thereby improving the thermal stability of the PE wrap film. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] This embodiment discloses a method for preparing a composite polyol ester, comprising the following steps:
[0034] Q1: Add 1g of succinic anhydride, 3.19g of phenolphthalein and p-toluenesulfonic acid monohydrate into a three-necked flask with a water separator and a condenser, replace with nitrogen three times, then heat to 140°C, wait for the solid in the flask to melt, stir vigorously for 30min, heat to 180°C, and esterify for 4h. After the reaction is completed, phenolphthalein-succinic acid is obtained;
[0035] Q2: 3.76g of 2-butyl-1,3-propanediol and 4.76g of phenolphthalein-succinic acid were added to a three-necked flask with a water separator and a condenser, and 1.43g of succinic anhydride and p-toluenesulfonic acid monohydrate were added at the same time. The argon gas was replaced 5 times. After the replacement, it was heated to 140°C and reacted for 30 minutes after the succinic anhydride melted. After the reaction was completed, the temperature was raised to 190°C and the esterification reaction was carried out for 4 hours;
[0036] Q3: After the esterification reaction, cool down, change to a vacuum distillation device, add catalysts tetrabutyl titanate and p-toluenesulfonic acid monohydrate, and raise the temperature to 240°C under argon protection. Vacuum and perform polycondensation for 2 hours. After the reaction, cool down, add chloroform to dissolve the polycondensation product, and then pour into high-speed stirred anhydrous methanol to precipitate the final product. After filtration, dry at 60°C for 48 hours to obtain a composite polyol ester.
[0037] This embodiment discloses a method for preparing cubic nano calcium carbonate, comprising the following steps:
[0038] S1: Sodium hydroxide and calcium chloride were placed in a beaker and stirred, and distilled water was added for dilution and stirring to obtain a microemulsion, and then 2 mL of the microemulsion, 50 mL of hexadecyltrimethylammonium bromide, 8 mL of n-pentanol and 15 mL of cyclohexane were mixed and stirred for 40 min to form a stable reverse microemulsion;
[0039] S2: Add 1 g of sucrose to 100 mL of reverse microemulsion, and introduce carbon dioxide gas into the reverse microemulsion at a flow rate of 300 mL / min. Continue to introduce and stir until no more precipitation is produced. Stop introducing carbon dioxide, let it stand for 24 hours, wash, centrifuge, and dry at 80°C for 24 hours to obtain cubic nano-calcium carbonate.
[0040] The present embodiment discloses a biodegradable PE wrapping film, which is prepared from the following ingredients in parts by weight: 15 parts of polyethylene ester, 17 parts of composite polyol ester, 3 parts of cubic nano calcium carbonate, 2 parts of silane coupling agent, and 1.5 parts of defoaming agent.
[0041] This embodiment discloses a processing technology for a biodegradable PE wrapping film, comprising the following steps:
[0042] Step (1): mixing polyvinyl ester, composite polyol ester, cubic nano calcium carbonate, silane coupling agent and defoaming agent and performing dust removal treatment;
[0043] Step (2): adding the dust-removed mixture evenly into an extruder, mixing it thoroughly and heating it to melt it into a melt, wherein the temperature of the melt is 260° C., transferring the melt from the extruder to a casting machine, and processing it into a film layer, wherein the film layer forms a PE wrapping film under the action of a cooling roller on the casting machine.
[0044] Example 2
[0045] This embodiment discloses a method for preparing a composite polyol ester, comprising the following steps:
[0046] Q1: Add 1g of succinic anhydride, 3.80g of phenolphthalein and p-toluenesulfonic acid monohydrate into a three-necked flask with a water separator and a condenser, replace with nitrogen three times, then heat to 140°C, wait for the solid in the flask to melt, stir vigorously for 30min, heat to 180°C, and esterify for 4h. After the reaction is completed, phenolphthalein-succinic acid is obtained;
[0047] Q2: 4.48g of 2-butyl-1,3-propanediol and 5.87g of phenolphthalein-succinic acid were added to a three-necked flask with a water separator and a condenser, and 1.80g of succinic anhydride and p-toluenesulfonic acid monohydrate were added at the same time. The argon gas was replaced 5 times. After the replacement, it was heated to 140°C and reacted for 30 minutes after the succinic anhydride melted. After the reaction was completed, the temperature was raised to 190°C and the esterification reaction was carried out for 4 hours;
[0048] Q3: After the esterification reaction, cool down, change to a vacuum distillation device, add catalysts tetrabutyl titanate and p-toluenesulfonic acid monohydrate, and raise the temperature to 240°C under argon protection. Vacuum and perform polycondensation for 2 hours. After the reaction, cool down, add chloroform to dissolve the polycondensation product, and then pour into high-speed stirred anhydrous methanol to precipitate the final product. After filtration, dry at 60°C for 48 hours to obtain a composite polyol ester.
[0049] This embodiment discloses a method for preparing cubic nano calcium carbonate, comprising the following steps:
[0050] S1: Sodium hydroxide and calcium chloride were placed in a beaker and stirred, and distilled water was added for dilution and stirring to obtain a microemulsion, and then 3 mL of the microemulsion, 55 mL of hexadecyltrimethylammonium bromide, 10 mL of n-pentanol and 17 mL of cyclohexane were mixed and stirred for 40 min to form a stable reverse microemulsion;
[0051] S2: Add 1 g of sucrose to 105 mL of reverse microemulsion, and introduce carbon dioxide gas into the reverse microemulsion at a flow rate of 300 mL / min. Continue to introduce and stir until no more precipitation is produced. Stop introducing carbon dioxide, let it stand for 24 hours, wash, centrifuge, and dry at 80°C for 24 hours to obtain cubic nano-calcium carbonate.
[0052] This embodiment discloses a biodegradable PE wrapping film, which is prepared from the following ingredients in parts by weight: 18 parts of polyethylene ester, 20 parts of composite polyol ester, 4 parts of cubic nano calcium carbonate, 3 parts of silane coupling agent, and 2 parts of defoaming agent.
[0053] This embodiment discloses a processing technology for a biodegradable PE wrapping film, comprising the following steps:
[0054] Step (1): mixing polyvinyl ester, composite polyol ester, cubic nano calcium carbonate, silane coupling agent and defoaming agent and performing dust removal treatment;
[0055] Step (2): adding the dust-removed mixture evenly into an extruder, mixing it thoroughly and heating it to melt it into a melt, wherein the temperature of the melt is 260° C., transferring the melt from the extruder to a casting machine, and processing it into a film layer, wherein the film layer forms a PE wrapping film under the action of a cooling roller on the casting machine.
[0056] Example 3
[0057] This embodiment discloses a method for preparing a composite polyol ester, comprising the following steps:
[0058] Q1: Add 1g of succinic anhydride, 2.66g of phenolphthalein and p-toluenesulfonic acid monohydrate into a three-necked flask with a water separator and a condenser, replace with nitrogen three times, then heat to 140°C, wait for the solid in the flask to melt, stir vigorously for 30min, heat to 180°C, and esterify for 4h. After the reaction is completed, phenolphthalein-succinic acid is obtained;
[0059] Q2: 3.21 g of 2-butyl-1,3-propanediol and 3.74 g of phenolphthalein-succinic acid were added to a three-necked flask with a water separator and a condenser, and 1.21 g of succinic anhydride and p-toluenesulfonic acid monohydrate were added at the same time. The argon gas was replaced 5 times. After the replacement, it was heated to 140°C and reacted for 30 minutes after the succinic anhydride melted. After the reaction was completed, the temperature was raised to 190°C and the esterification reaction was carried out for 4 hours;
[0060] Q3: After the esterification reaction, cool down, change to a vacuum distillation device, add catalysts tetrabutyl titanate and p-toluenesulfonic acid monohydrate, and raise the temperature to 240°C under argon protection. Vacuum and perform polycondensation for 2 hours. After the reaction, cool down, add chloroform to dissolve the polycondensation product, and then pour into high-speed stirred anhydrous methanol to precipitate the final product. After filtration, dry at 60°C for 48 hours to obtain a composite polyol ester.
[0061] This embodiment discloses a method for preparing cubic nano calcium carbonate, comprising the following steps:
[0062] S1: Sodium hydroxide and calcium chloride were placed in a beaker and stirred, and distilled water was added for dilution and stirring to obtain a microemulsion, and then 1 mL of the microemulsion, 45 mL of hexadecyltrimethylammonium bromide, 6 mL of n-pentanol and 13 mL of cyclohexane were mixed and stirred for 40 min to form a stable reverse microemulsion;
[0063] S2: Add 1 g of sucrose to 95 mL of reverse microemulsion, and introduce carbon dioxide gas into the reverse microemulsion at a flow rate of 300 mL / min. Continue to introduce and stir until no more precipitation is produced. Stop introducing carbon dioxide, let it stand for 24 hours, wash, centrifuge, and dry at 80°C for 24 hours to obtain cubic nano-calcium carbonate.
[0064] This embodiment discloses a biodegradable PE wrapping film, which is prepared from the following ingredients in parts by weight: 12 parts of polyethylene ester, 15 parts of composite polyol ester, 2 parts of cubic nano calcium carbonate, 1 part of silane coupling agent, and 1 part of defoaming agent.
[0065] This embodiment discloses a processing technology for a biodegradable PE wrapping film, comprising the following steps:
[0066] Step (1): mixing polyvinyl ester, composite polyol ester, cubic nano calcium carbonate, silane coupling agent and defoaming agent and performing dust removal treatment;
[0067] Step (2): adding the dust-removed mixture evenly into an extruder, mixing it thoroughly and heating it to melt it into a melt, wherein the temperature of the melt is 260° C., transferring the melt from the extruder to a casting machine, and processing it into a film layer, wherein the film layer forms a PE wrapping film under the action of a cooling roller on the casting machine.
[0068] Example 4
[0069] This embodiment discloses a method for preparing a composite polyol ester, comprising the following steps:
[0070] Q1: Add 1g of succinic anhydride, 2.83g of phenolphthalein and p-toluenesulfonic acid monohydrate into a three-necked flask with a water separator and a condenser, replace with nitrogen three times, then heat to 140°C, wait for the solid in the flask to melt, stir vigorously for 30min, heat to 180°C, and esterify for 4h. After the reaction is completed, phenolphthalein-succinic acid is obtained;
[0071] Q2: 4.25 g of 2-butyl-1,3-propanediol and 5.17 g of phenolphthalein-succinic acid were added to a three-necked flask with a water separator and a condenser, and 1.58 g of succinic anhydride and p-toluenesulfonic acid monohydrate were added at the same time. The argon gas was replaced 5 times. After the replacement, the mixture was heated to 140°C and reacted for 30 minutes after the succinic anhydride melted. After the reaction was completed, the temperature was raised to 190°C and the esterification reaction was carried out for 4 hours.
[0072] Q3: After the esterification reaction, cool down, change to a vacuum distillation device, add catalysts tetrabutyl titanate and p-toluenesulfonic acid monohydrate, and raise the temperature to 240°C under argon protection. Vacuum and perform polycondensation for 2 hours. After the reaction, cool down, add chloroform to dissolve the polycondensation product, and then pour into high-speed stirred anhydrous methanol to precipitate the final product. After filtration, dry at 60°C for 48 hours to obtain a composite polyol ester.
[0073] This embodiment discloses a method for preparing cubic nano calcium carbonate, comprising the following steps:
[0074] S1: Sodium hydroxide and calcium chloride were placed in a beaker and stirred, and distilled water was added for dilution and stirring to obtain a microemulsion, and then 1.5 mL of the microemulsion, 47 mL of hexadecyltrimethylammonium bromide, 7 mL of n-pentanol and 14 mL of cyclohexane were mixed and stirred for 40 min to form a stable reverse microemulsion;
[0075] S2: Add 1 g of sucrose to 98 mL of reverse microemulsion, and introduce carbon dioxide gas into the reverse microemulsion at a flow rate of 300 mL / min. Continue to introduce and stir until no more precipitation is produced. Stop introducing carbon dioxide, let it stand for 24 hours, wash, centrifuge, and dry at 80°C for 24 hours to obtain cubic nano-calcium carbonate.
[0076] This embodiment discloses a biodegradable PE wrapping film, which is prepared from the following ingredients in parts by weight: 13 parts of polyethylene ester, 18 parts of composite polyol ester, 2.5 parts of cubic nano-calcium carbonate, 1.5 parts of silane coupling agent, and 1 part of defoaming agent.
[0077] This embodiment discloses a processing technology for a biodegradable PE wrapping film, comprising the following steps:
[0078] Step (1): mixing polyvinyl ester, composite polyol ester, cubic nano calcium carbonate, silane coupling agent and defoaming agent and performing dust removal treatment;
[0079] Step (2): adding the dust-removed mixture evenly into an extruder, mixing it thoroughly and heating it to melt it into a melt, wherein the temperature of the melt is 260° C., transferring the melt from the extruder to a casting machine, and processing it into a film layer, wherein the film layer forms a PE wrapping film under the action of a cooling roller on the casting machine.
[0080] Example 5
[0081] This embodiment discloses a method for preparing a composite polyol ester, comprising the following steps:
[0082] Q1: Add 1g of succinic anhydride, 3.42g of phenolphthalein and p-toluenesulfonic acid monohydrate into a three-necked flask with a water separator and a condenser, replace with nitrogen three times, then heat to 140°C, wait for the solid in the flask to melt, stir vigorously for 30min, heat to 180°C, and esterify for 4h. After the reaction is completed, phenolphthalein-succinic acid is obtained;
[0083] Q2: 3.48g of 2-butyl-1,3-propanediol and 4.12g of phenolphthalein-succinic acid were added to a three-necked flask with a water separator and a condenser, and 1.07g of succinic anhydride and p-toluenesulfonic acid monohydrate were added at the same time. The argon gas was replaced 5 times. After the replacement, it was heated to 140°C and reacted for 30 minutes after the succinic anhydride melted. After the reaction was completed, the temperature was raised to 190°C and the esterification reaction was carried out for 4 hours;
[0084] Q3: After the esterification reaction, cool down, change to a vacuum distillation device, add catalysts tetrabutyl titanate and p-toluenesulfonic acid monohydrate, and raise the temperature to 240°C under argon protection. Vacuum and perform polycondensation for 2 hours. After the reaction, cool down, add chloroform to dissolve the polycondensation product, and then pour into high-speed stirred anhydrous methanol to precipitate the final product. After filtration, dry at 60°C for 48 hours to obtain a composite polyol ester.
[0085] This embodiment discloses a method for preparing cubic nano calcium carbonate, comprising the following steps:
[0086] S1: Sodium hydroxide and calcium chloride were placed in a beaker and stirred, and distilled water was added for dilution and stirring to obtain a microemulsion, and then 2.5 mL of the microemulsion, 52 mL of hexadecyltrimethylammonium bromide, 9 mL of n-pentanol and 16 mL of cyclohexane were mixed and stirred for 40 min to form a stable reverse microemulsion;
[0087] S2: Add 1 g of sucrose to 103 mL of reverse microemulsion, and introduce carbon dioxide gas into the reverse microemulsion at a flow rate of 300 mL / min. Continue to introduce and stir until no more precipitation is produced. Stop introducing carbon dioxide, let it stand for 24 hours, wash, centrifuge, and dry at 80°C for 24 hours to obtain cubic nano-calcium carbonate.
[0088] This embodiment discloses a biodegradable PE wrapping film, which is prepared from the following ingredients in parts by weight: 17 parts of polyethylene ester, 16 parts of composite polyol ester, 3.5 parts of cubic nano calcium carbonate, 2.5 parts of silane coupling agent, and 2 parts of defoaming agent.
[0089] This embodiment discloses a processing technology for a biodegradable PE wrapping film, comprising the following steps:
[0090] Step (1): mixing polyvinyl ester, composite polyol ester, cubic nano calcium carbonate, silane coupling agent and defoaming agent and performing dust removal treatment;
[0091] Step (2): adding the dust-removed mixture evenly into an extruder, mixing it thoroughly and heating it to melt it into a melt, wherein the temperature of the melt is 260° C., transferring the melt from the extruder to a casting machine, and processing it into a film layer, wherein the film layer forms a PE wrapping film under the action of a cooling roller on the casting machine.
[0092] Comparative Example 1
[0093] Comparative Example 1 Compared with Example 1, in the process of preparing the composite polyol ester in Comparative Example 1, 2-butyl-1,3-propanediol was not added, and other conditions remained unchanged.
[0094] Comparative Example 2
[0095] Comparative Example 2 Compared with Example 1, in the process of preparing cubic nano-calcium carbonate in Comparative Example 2, no sucrose was added, and other conditions remained unchanged.
[0096] Comparative Example 3
[0097] Comparative Example 3 Compared with Example 1, in the process of preparing the PE stretch film in Comparative Example 3, no composite polyol ester is added, and other conditions remain unchanged.
[0098] Comparative Example 4
[0099] Comparative Example 4 Compared with Example 1, in the process of preparing the PE stretch film in Comparative Example 4, no cubic nano-calcium carbonate is added, and other conditions remain unchanged.
[0100] Experimental example
[0101] The properties of the biodegradable PE wrapping films prepared in Examples 1-5 and Comparative Examples 1-4 were tested.
[0102] 1. Biodegradability Test
[0103] The degradation performance of the samples was measured according to GB / T 35795-2017. The test results are shown in Table 1:
[0104] Table 1
[0105]
[0106] From the test results in Table 1, it can be seen that the PE wrapping films prepared in Examples 1-5 of the present invention have excellent biodegradability. From the comparison between Comparative Example 1 and Examples 1-5, it can be seen that the addition of 2-butyl-1,3-propanediol can effectively improve the biodegradability of the PE wrapping film; from the comparison between Comparative Example 3 and Examples 1-5, it can be seen that the addition of composite polyol ester can improve the biodegradability of the PE wrapping film.
[0107] 2. Mechanical properties test
[0108] The tensile properties of the samples were measured according to GB / T 1040.1-2018. The test results are shown in Table 2:
[0109] Table 2
[0110]
[0111] From the test results in Table 2, it can be seen that the PE wrapping films prepared in Examples 1-5 of the present invention have excellent mechanical properties. From the comparison between Comparative Example 2 and Examples 1-5, it can be seen that the addition of sucrose can promote the formation of cubic nano-calcium carbonate, thereby improving the mechanical properties of the PE wrapping film; from the comparison between Comparative Example 4 and Examples 1-5, it can be seen that the addition of cubic nano-calcium carbonate can effectively improve the mechanical properties of the PE wrapping film.
[0112] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0113] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A biodegradable PE stretch film, characterized in that: The invention is prepared from the following ingredients in parts by weight: 12-18 parts of polyethylene ester, 15-20 parts of composite polyol ester, 2-4 parts of cubic nano calcium carbonate, 1-3 parts of silane coupling agent and 1-2 parts of defoamer; wherein the composite polyol ester is obtained by reacting phenolphthalein-succinic acid, 2-butyl-1,3-propylene glycol and succinic anhydride, and the cubic nano calcium carbonate is obtained by multiphase reaction in a microemulsion system.
2. The biodegradable PE stretch film according to claim 1, characterized in that: The preparation method of the composite polyol ester comprises the following steps: Q1: Add succinic anhydride, phenolphthalein and p-toluenesulfonic acid monohydrate into a three-necked flask, replace with nitrogen, and then heat. After the solid in the flask melts, stir vigorously and heat to carry out esterification reaction. After the reaction is completed, phenolphthalein-succinic acid is obtained; Q2: Add 2-butyl-1,3-propanediol and phenolphthalein-succinic acid into a three-necked flask, add succinic anhydride and p-toluenesulfonic acid monohydrate at the same time, and replace with argon. After the replacement, heat and react after the succinic anhydride melts. After the reaction is completed, heat and carry out esterification reaction; Q3: After the esterification reaction is completed, the temperature is lowered, and the vacuum distillation device is replaced. The catalysts tetrabutyl titanate and p-toluenesulfonic acid monohydrate are added. Under the protection of argon, the temperature is raised, and the vacuum is drawn to carry out the polycondensation reaction. After the reaction is completed, the temperature is lowered, chloroform is added to dissolve the polycondensation product, and then the product is poured into high-speed stirred anhydrous methanol to precipitate the final product. After filtration, it is dried to obtain a composite polyol ester.
3. The biodegradable PE stretch film according to claim 2, characterized in that: In the Q1, the molar ratio of succinic anhydride to phenolphthalein is 1:(0.8-1.2), the three-necked flask is equipped with a water separator and a condenser, the nitrogen replacement times are 3-5 times, the heating temperature is 140-160°C, the vigorous stirring time is 30-50min, the heating temperature is 180-200°C, and the esterification reaction time is 3-4h.
4. The biodegradable PE stretch film according to claim 2, characterized in that: In Q2, the molar ratio of 2-butyl-1,3-propanediol, phenolphthalein-succinic acid and succinic anhydride is (1.6-2.4):(0.8-1.3):(0.7-1.3), the three-necked flask is equipped with a water separator and a condenser, the argon replacement times are 3-5 times, the heating temperature is 120-140°C, the reaction time is 20-40min, the heating temperature is 170-190°C, and the esterification reaction time is 3-4h.
5. The biodegradable PE stretch film according to claim 2, characterized in that: In the Q3, the heating temperature is 230-250°C, the polycondensation reaction time is 1-2h, the drying temperature is 50-60°C, and the drying time is 48-54h.
6. The biodegradable PE stretch film according to claim 1, characterized in that: The preparation method of the cubic nano calcium carbonate comprises the following steps: S1: Sodium hydroxide and calcium chloride are placed in a beaker and stirred, distilled water is added for dilution and stirring to obtain a microemulsion, and then the microemulsion, hexadecyltrimethylammonium bromide, n-pentanol and cyclohexane are mixed and stirred to form a stable reverse microemulsion; S2: Add sucrose to the reverse microemulsion, introduce carbon dioxide gas into the reverse microemulsion, continue to introduce and stir continuously until no precipitation is produced, stop introducing carbon dioxide, let it stand for aging, wash, centrifuge, and dry to obtain cubic nano-calcium carbonate.
7. The biodegradable PE stretch film according to claim 6, characterized in that: In the S1, the volume ratio of the microemulsion, hexadecyltrimethylammonium bromide, n-pentanol and cyclohexane is (1-3): (45-55): (6-10): (13-17), and the stirring time is 20-40 min. In the S2, the dosage ratio of sucrose and reverse microemulsion is 1 g: (95-105) mL, the flow rate of carbon dioxide gas is 300-320 mL / min, the standing aging time is 22-26 h, the drying temperature is 70-80° C., and the drying time is 20-24 h.
8. A processing technology for the biodegradable PE stretch film as claimed in claims 1 to 7, characterized in that: The following steps are involved: Step (1): mixing polyvinyl ester, composite polyol ester, cubic nano calcium carbonate, silane coupling agent and defoaming agent and performing dust removal treatment; Step (2): adding the dust-removed mixture evenly into an extruder, mixing it thoroughly and heating it to melt it into a melt, transferring the melt from the extruder to a casting machine, and processing it into a film layer, and the film layer forms a PE wrapping film under the action of a cooling roller on the casting machine.
9. The processing technology of the biodegradable PE stretch film according to claim 8, characterized in that: In the step (2), the temperature of the melt is 250-280°C.