Water-based sand-containing colorful stone-like coating and preparation method thereof

Through the cross-linking reaction of functionalized acrylic emulsion and hydrazide-modified magnesium lithium silicate, a cross-linked network structure is formed, which solves the problem of poor stability of the protective gel system and poor emulsion compatibility in water-based sand-containing multi-colored coatings, and improves the coating's durability. Viscosity stability and film hardness enhance water resistance and durability.

CN118745308AActive Publication Date: 2024-10-08CARBON TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411120272.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-08
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The protective colloid system of existing water-based sand-containing multi-colored paints has poor stability and poor emulsion compatibility, resulting in unstable viscosity, poor water whitening resistance and poor particle stability of the finished paint. Moreover, the durability and protective performance of the paint film are reduced after the continuous phase is reduced.

Method used

Functionalized acrylic emulsion and hydrazide-modified magnesium lithium silicate are used as components of the base paint and granulation liquid, omitting the traditional continuous phase, and are formed through the cross-linking reaction of hydrazide-modified magnesium lithium silicate and functionalized acrylic emulsion. The cross-linked network structure improves the density and water resistance of the paint film.

Benefits of technology

It improves the viscosity stability, water whitening resistance and paint film hardness of the paint, enhances the durability and protective properties of the paint film, solves the problem of post-thickening and maintains the stability of the overall system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745308A_ABST
    Figure CN118745308A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sand-in-water colorful coatings, and particularly discloses a water-based sand-containing colorful stone-like coating and a preparation method thereof. The basic paint with specific raw material components and the granulation liquid are matched, in the drying process of a coating film, water is continuously volatilized, a neutralizing agent in a coating system is also continuously volatilized, so that the pH is reduced, latex particles start to deform, amino of hydrazide modified magnesium lithium silicate and ketone carbonyl of functionalized acrylic emulsion are subjected to a cross-linking reaction, and the functional acrylic emulsion is formed. A cross-linked network structure is quickly formed, so that the compactness and the water resistance of the colorful paint film are improved; hydrazide modified magnesium lithium silicate plays a role of anchoring points in the network structure, so that basic paint color points can be tightly connected together and cross-linked to form a film, continuous phase components are omitted, the post-thickening problem of the colorful stone-like coating is improved, the overall compactness, water white resistance and paint film hardness of a coating film are improved, and the color-like coating has a good color-like effect. And the defects of poor durability and protectiveness of the paint film after the continuous phase is reduced are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-based sand-containing multi-colored paint, and in particular to a water-based sand-containing multi-colored stone-imitation paint and a preparation method thereof. Background Art

[0002] Water-based sand-containing multi-color paint itself has the characteristics of rich colors and adjustable colors. With special shapes, it can achieve a very high degree of simulated stone effect, and can simulate the texture, color and texture of natural stone, thereby avoiding the further consumption of natural heavy material resources. In addition, water-based sand-containing multi-color paint is simple to construct, has strong designability, is light and safe, low-carbon and environmentally friendly, and relatively low in cost. It has the advantages of erosion resistance, waterproofness, and stain resistance. In recent years, it is expected to gradually replace traditional real stone paint. Existing water-based sand-containing multi-color paints generally consist of three parts: sand-containing base paint, granulation liquid and continuous phase. The sand-containing base paint is mixed with granulation liquid after color paste is adjusted, and mechanical cutting and granulation are used to form sand-containing base paint and granulation liquid mixtures with different color point sizes and colors, and then mixed with the continuous phase for thickening to form water-based sand-containing multi-color paint.

[0003] However, the stability of the protective colloid system in the current water-based sand-containing multi-color coating is poor, and the compatibility with the emulsion system is poor. It is very easy to cause post-thickening problems with the emulsion and cellulose in the coating, resulting in poor viscosity stability of the finished coating, poor water whitening resistance, poor particle stability, etc. In order to improve the above problems, the prior art uses an inert emulsion in the continuous phase emulsion, or cancels the continuous phase and only retains the base paint and granulation liquid. Although these operations can alleviate the post-thickening problem to a certain extent, they do not fundamentally solve the problem of poor stability of the protective colloid system. At the same time, since these operations reduce the protective effect of the continuous phase film formation, the durability and protective performance of the coating in the later stage are damaged to a certain extent. Summary of the invention

[0004] In view of the above problems, the present invention provides a water-based sand-containing colorful stone-like paint and a preparation method thereof, which improves the stability of the coating viscosity, while improving the post-thickening problem of the system, and improves the overall density, water whitening resistance and hardness of the coating film, thereby improving the durability and protectiveness of the paint film.

[0005] In order to solve the above technical problems, the technical solution provided by the present invention is: In a first aspect, the present invention provides a water-based sand-containing colorful stone-like paint, which is composed of a base paint and a granulation liquid; The base paint comprises a functionalized acrylic emulsion containing ketone carbonyl and carboxyl groups and hydrazide-modified lithium magnesium silicate containing amino groups; the granulation liquid comprises the hydrazide-modified lithium magnesium silicate; The components of the functionalized acrylic emulsion include the structural formula shown in Formula 1:

[0006] Formula 1; In the formula, R is selected from or ; R' is selected from -H or -CH 3 ; j, t, s, and q independently represent positive integers.

[0007] Compared with the prior art, the water-based sand-containing colorful stone-like paint provided by the present invention adopts a base paint and a granulation liquid of specific raw material components for combination, omitting the continuous phase part in the traditional colorful stone-like paint, which can effectively improve the post-thickening problem of the colorful stone-like paint on the one hand, and reduce the complexity of the preparation process on the other hand; hydrazide-modified lithium magnesium silicate is used as a protective glue system for the base paint and the granulation liquid, and can undergo a cross-linking reaction with the functionalized acrylic emulsion in the base paint during the drying process of the coating film, which not only improves the overall density, water whitening resistance and hardness of the coating film, but also makes up for the shortcomings of poor durability and protection of the paint film after reducing the continuous phase.

[0008] The present invention uses functionalized acrylic emulsion and hydrazide-modified lithium magnesium silicate as film-forming substances. The hydrazide-modified lithium magnesium silicate is composed of lithium magnesium silicate (its schematic diagram is shown in Figure 1 ) is obtained through organic modification. The spacing between the lithium magnesium silicate crystal lamellae increases, making it easier to react with latex molecules. Under the action of the carboxyl group of the functionalized acrylic emulsion, it is also easier to form a house-of-cards structure. With the volatilization of water and the decrease in pH, at room temperature, the amino groups of the hydrazide-modified lithium magnesium silicate and the ketone carbonyl groups of the functionalized acrylic emulsion can undergo a dehydration condensation reaction to cross-link. Therefore, during the drying process of the coating film, water continues to evaporate, and the ammonia water (neutralizer) in the coating system also continues to evaporate, causing the pH to drop, and the latex particles begin to deform. At the same time, the cross-linking reaction occurs, so that the hydrazide-modified lithium magnesium silicate in the base paint and granulation liquid can quickly form a cross-linked network structure with the functionalized acrylic emulsion in the base paint. The reaction diagram is shown in the figure. Figure 2 As shown. The formation of the cross-linked structure improves the density and water resistance of the colorful paint film. At the same time, the hydrazide-modified lithium magnesium silicate plays the role of an "anchor point" in the network structure, so that the color dots of the basic paint can be closely connected together, not only assuming the function of the color of the color dots, but also achieving the role of cross-linking film formation, omitting the traditional continuous phase component. The surface structure of the basic paint of the present invention can promote the formation of the "card house" structure of the protective glue to a certain extent, maintain the viscosity of the finished product, but will not have an adverse effect on the post-thickening viscosity of the overall system.

[0009] Preferably, the functionalized acrylic emulsion is polymerized from a ketocarbonyl-containing acrylic monomer, methyl methacrylate, methacrylic acid and butyl acrylate; The ketone carbonyl-containing acrylic monomer is selected from at least one of diacetone acrylamide and acetoacetoxyethyl methacrylate.

[0010] The present invention uses diacetone acrylamide (DAAM) and / or acetoacetoxyethyl methacrylate (AAEM) as the main functional monomers, and uses methyl methacrylate (MMA), methacrylic acid (MAA) and butyl acrylate (BA) as the main polymerization monomers. After the polymerization reaction, ketocarbonyl and carboxyl groups can be introduced into the functionalized acrylic emulsion. The ketocarbonyl group can undergo a dehydration condensation reaction with the amino group of hydrazide-modified lithium magnesium silicate to crosslink, thereby replacing the traditional continuous phase component and improving the density and water resistance of the paint film. Methacrylic acid contains carboxyl groups, which can be modified on the surface of the functionalized acrylic emulsion after the polymerization reaction. The carboxyl groups in the finished emulsion molecules can promote the swelling of the protective glue molecules (including hydrazide-modified lithium magnesium silicate) in the system and the formation of the house-of-cards structure.

[0011] Preferably, the raw materials of the functionalized acrylic emulsion include the following components in parts by mass: 4 to 5.2 parts of ketocarbonyl-containing acrylic monomer, 17.5 to 19 parts of methyl methacrylate, 0.5 to 0.8 parts of methacrylic acid, 9.5 to 11 parts of butyl acrylate, 1.28 to 1.58 parts of emulsifier, 0.12 to 0.15 parts of buffer, 0.1 to 0.12 parts of initiator and 61 to 68 parts of water.

[0012] The present invention has found through a large number of tests that the Tg (glass transition temperature) of homopolymerized polymethyl methacrylate (PMMA) is about 100°C, the Tg of homopolymerized polymethacrylic acid (PMAA) is about 105°C, the Tg of homopolymerized polybutyl acrylate (PBA) is about -55°C, and the Tg of homopolymerized ketone carbonyl-containing acrylic acid is about 80°C to 120°C. The present invention limits the dosage ratio of the main polymerized monomers so that the Tg of the functionalized acrylic emulsion is about 5°C to 10°C, which can ensure the film-forming properties of the finished paint film, thereby further balancing the flexibility and water whitening resistance of the colorful imitation stone paint and improving the comprehensive properties of the colorful imitation stone paint.

[0013] In addition, the functionalized acrylic emulsion is modified with a specific amount of methacrylic acid, and the introduced carboxyl group and the protective glue system can synergistically thicken without causing the post-thickening problem of the system. The present invention has found through a large number of experiments that when the carboxyl concentration exceeds the specified range of the present invention, the post-thickening of the system will increase sharply due to the excessively strong promotion effect on the protective glue; when the carboxyl concentration is lower than the specified range of the present invention, the viscosity of the system cannot be well maintained and stable, resulting in water separation problems in the coating.

[0014] Preferably, the raw material components of the functionalized acrylic emulsion further include a neutralizer, and the pH of the functionalized acrylic emulsion is 8-9.

[0015] In the present invention, the weakly alkaline environment is more likely to maintain the stability of the anionic emulsifier. In addition, during the (persulfate) initiation process, the pH of the system will decrease. The alkaline environment can maintain the stability of the polymerization reaction, and will not produce the phenomenon of polymerization acceleration, so that the polymerization reaction can proceed more fully.

[0016] More preferably, the emulsifier is selected from anionic reactive emulsifiers. More preferably, the emulsifier is SR-10.

[0017] In the present invention, the preferred emulsifier can reduce the surface tension of the functionalized acrylic emulsion, emulsify the monomer into small droplets, and further form micelles, which is conducive to the occurrence and progress of the subsequent polymerization reaction. The reactive emulsifier contains a polymerizable double bond, which can also participate in the copolymerization reaction of acrylic monomers during the polymerization reaction, thereby improving the stability of the latex particles. In addition, the migration of emulsifier molecules will be reduced during the drying process of the paint film, thereby improving the water whitening resistance of the paint film.

[0018] Further preferably, the buffer is sodium bicarbonate.

[0019] More preferably, the initiator is ammonium persulfate.

[0020] More preferably, the neutralizing agent is aqueous ammonia.

[0021] The present invention uses ammonia water as a neutralizing agent. During the drying process of the paint film, the ammonia water will continuously volatilize to reduce the pH value of the system, thereby enabling the hydrazide-modified lithium magnesium silicate in the base paint and the granulation liquid to quickly form a cross-linked network structure with the functionalized acrylic emulsion.

[0022] Preferably, the method for preparing the functionalized acrylic emulsion comprises the following steps: Sa, weighing each raw material component according to the designed ratio, and uniformly mixing the ketone carbonyl-containing acrylic acid monomer, methyl methacrylate, methacrylic acid, butyl acrylate, the first part of the emulsifier and the first part of the water to obtain a pre-emulsion; Sb, the remaining emulsifier, buffer and the remaining water are mixed evenly, the pre-emulsion and initiator are added at 80° C. to 85° C. to carry out polymerization reaction, and the pH of the obtained reaction solution is adjusted to 8 to 9 to obtain a functionalized acrylic emulsion.

[0023] Further preferably, the mass ratio of the first part of emulsifier to the remaining part of emulsifier is 0.9:1~1.1:1.

[0024] Further preferably, the mass ratio of the first part of water to the remaining part of water is (27~30):(34~38).

[0025] For example, the pre-emulsion and the initiator are added dropwise for 2 h to 3 h.

[0026] More preferably, the polymerization reaction temperature is 80° C. to 85° C., and the insulation reaction time is 1.5 h to 2 h.

[0027] Preferably, the preparation method of the hydrazide-modified lithium magnesium silicate comprises the following steps: S1, adding lithium magnesium silicate and a silane coupling agent into a first solvent, heating to reflux, and performing a substitution reaction to obtain silane-modified lithium magnesium silicate; S2, adding the silane-modified lithium magnesium silicate and methyl acrylate to a second solvent under a protective atmosphere and light-proof conditions to carry out a Michael addition reaction to obtain methyl acrylate-terminated lithium magnesium silicate; S3, adding the methyl acrylate-terminated lithium magnesium silicate to hydrazine hydrate, and carrying out a condensation reaction at 75° C. to 78° C. under a protective atmosphere to obtain hydrazide-modified lithium magnesium silicate.

[0028] In the present invention, the hydrazide-modified lithium magnesium silicate and the ketone carbonyl of the functionalized acrylic emulsion can be cross-linked at room temperature, thereby improving the density of the paint film and making the originally separated basic color dots tightly cross-linked, in which the hydrazide-modified lithium magnesium silicate structure plays the role of an "anchor point". The reaction equation in the preparation process of the hydrazide-modified lithium magnesium silicate of the present invention can be found in Figure 3 .

[0029] Further preferably, in S1, the silane coupling agent is aminopropyltrimethoxysilane.

[0030] Further preferably, in S1, the first solvent is toluene.

[0031] Further preferably, in S1, the mass volume ratio of the lithium magnesium silicate, the silane coupling agent and the first solvent is (4.8-5.2) g: (10.2-12.8) mL: (150-180) mL.

[0032] Further preferably, in S1, the substitution reaction time is 7h~8h.

[0033] For example, in S1, after the substitution reaction is completed, the obtained reaction solution is further stirred at room temperature for 12h~14h, filtered, and the filter cake is washed with a Soxhlet extractor for 16h~18h, and dried to obtain silane-modified lithium magnesium silicate. The drying method can be vacuum freeze drying.

[0034] In the present invention, the silane coupling agent can undergo a substitution reaction with the lithium magnesium silicate to graft the amino group onto the lithium magnesium silicate, and by limiting the amount of the silane coupling agent and the lithium magnesium silicate and the reaction conditions, it is convenient to subsequently end-cap the lithium magnesium silicate with the corresponding substance. In addition, the preferred silane coupling agent contains an amino group, has strong activity and aggressiveness, and can directly perform the subsequent Michael addition reaction without adding a base.

[0035] Further preferably, in S2, the second solvent is selected from methanol, ethanol or N,N-dimethylformamide.

[0036] Further preferably, in S2, the mass volume ratio of the silane-modified lithium magnesium silicate, the methyl acrylate and the second solvent is (5.2-5.7) g: (4.2-4.8) mL: (48-55) mL.

[0037] Further preferably, in S2, the temperature of the Michael addition reaction is 10°C to 40°C, and the reaction time is 48h to 56h.

[0038] For example, after the Michael addition reaction is completed, the obtained reaction solution is subjected to reduced pressure distillation to remove the second solvent.

[0039] For example, the protective atmosphere is a nitrogen atmosphere.

[0040] Further preferably, in S3, the volume concentration of the hydrazine hydrate is 70% to 80%.

[0041] Further preferably, in S3, the mass volume ratio of the methyl acrylate-capped lithium magnesium silicate and the hydrazine hydrate is (6-6.5) g: (18-21) mL.

[0042] Further preferably, in S3, the condensation reaction time is 22h~24h.

[0043] For example, in S3, after the condensation reaction is completed, the obtained reaction solution is concentrated, diluted with a third solvent (selected from chloroform, benzene or toluene), washed with brine, dried over anhydrous sodium sulfate, and then concentrated under reduced pressure to remove the third solvent to obtain hydrazide-modified lithium magnesium silicate.

[0044] The present invention sequentially uses methyl acrylate and hydrazine hydrate to react with silane-modified lithium magnesium silicate, amplifies the number of hydrazide amino groups that can react with ketocarbonyl groups, and controls the amount of each reactant and the reaction conditions to obtain hydrazide-modified lithium magnesium silicate that can achieve optimal crosslinking with the ketocarbonyl groups of a functionalized acrylic emulsion.

[0045] Preferably, the base paint and the granulation liquid both include lithium magnesium silicate.

[0046] The present invention uses lithium magnesium silicate and hydrazide-modified lithium magnesium silicate as the protective colloid system of the base paint and granulation liquid. Compared with lithium magnesium silicate, the hydrophilicity of hydrazide-modified lithium magnesium silicate is reduced. The addition of lithium magnesium silicate can promote the dispersion and swelling of hydrazide-modified lithium magnesium silicate in the aqueous phase, and under the action of the carboxyl group of the functionalized acrylic emulsion, it is also easier to form a house-of-cards structure. During the drying process of the coating film, the protective colloid system of lithium magnesium silicate and hydrazide-modified lithium magnesium silicate can undergo a cross-linking reaction with the functionalized acrylic emulsion in the base paint, which not only improves the overall density, water whitening resistance and hardness of the coating film, but also makes up for the shortcomings of poor durability and protection of the coating film after reducing the continuous phase.

[0047] Preferably, the mass ratio of the base paint to the granulation liquid is 7:3 to 8:2.

[0048] Preferably, the base paint includes the following components in percentage by weight: 22% to 25% functionalized acrylic emulsion, 0.38% to 0.42% lithium magnesium silicate, 0.19% to 0.21% hydrazide-modified lithium magnesium silicate, 0.6% to 1% cellulose, 0.08% to 0.12% dispersant, 0.2% to 0.4% defoamer, 0.7% to 1.2% antifreeze, 1.2% to 1.8% film-forming aid, 0.3% to 0.6% bactericide, 4.5% to 5.8% color filler, 0.08% to 0.12% neutralizer, 32% to 38% quartz sand, 0 to 2% color paste and 25% to 30% water.

[0049] Preferably, the granulation liquid comprises the following components in percentage by weight: 2% to 3.5% lithium magnesium silicate, 2.2% to 3.5% hydrazide-modified lithium magnesium silicate, 0.35% to 0.5% anti-settling agent, 0.3% to 0.5% bactericide, and 92% to 95% water. Further preferably, the granulation liquid comprises the following raw material components in percentage by weight: 2.2% to 3.5% lithium magnesium silicate, 2.2% to 3.5% hydrazide-modified lithium magnesium silicate, 0.36% to 0.42% anti-settling agent, 0.32% to 0.42% bactericide, and 92.5% to 94.5% water.

[0050] The present invention limits the components and contents of the base paint and the granulation liquid, so as to better exert the synergistic effect of the components, effectively control the crosslinking degree of the protective glue system and the functionalized acrylic emulsion during the coating film drying process, ensure that the water-based sand-containing colorful stone-like paint has stable viscosity, water whitening resistance and hardness, and will not have an adverse effect on the post-thickening viscosity of the overall system, so that the comprehensive performance of the water-based sand-containing colorful stone-like paint reaches the best state.

[0051] Preferably, the cellulose is hydroxyethyl cellulose.

[0052] More preferably, the hydroxyethyl cellulose is selected from at least one of 250HBR, 250HHBR or HE-10K.

[0053] Preferably, the pigment filler is selected from at least one of calcined kaolin or rutile titanium dioxide.

[0054] Preferably, the dispersant is a polycarboxylate sodium salt type dispersant.

[0055] Further preferably, the dispersant is SN-5040.

[0056] Preferably, the defoaming agent is a mineral oil defoaming agent.

[0057] Further preferably, the defoaming agent is NXZ.

[0058] Preferably, the antifreeze liquid is selected from at least one of ethylene glycol or propylene glycol.

[0059] Preferably, the film-forming aid is alcohol ester dodecaned.

[0060] Preferably, the fungicide is an isothiazolinone fungicide.

[0061] Further preferably, the fungicide is selected from at least one of CMIT (5-chloro-2-methyl-4-isothiazoline-3-one), MIT (2-methyl-4-isothiazoline-3-one) or BIT (1,2-benzisothiazolin-3-one).

[0062] Preferably, the anti-settling agent is xanthan gum.

[0063] Preferably, the color paste is selected from at least one of iron red, iron yellow or carbon black.

[0064] The present invention can further improve the comprehensive performance of the water-based sand-containing colorful stone-like paint by limiting the corresponding auxiliary materials in the base paint and the granulation liquid.

[0065] In a second aspect, the present invention provides a method for preparing a water-based sand-containing colorful stone-like paint, comprising the following steps: SI, preparation of base paint: Weigh each raw material component according to the designed ratio, mix cellulose, dispersant, the first portion of defoamer and the first portion of water evenly, add pigments and fillers and neutralizers, mix evenly, then add antifreeze, film-forming aid, functionalized acrylic emulsion, the remaining portion of defoamer and fungicide, mix evenly to obtain a mixed system; Adding lithium magnesium silicate and hydrazide-modified lithium magnesium silicate into the remaining water to obtain a protective colloid solution; Adding the protective glue solution into the mixed system, and then adding quartz sand and color paste to obtain a base paint; SII, Preparation of Granulation Solution: Mixing lithium magnesium silicate, hydrazide-modified lithium magnesium silicate, an anti-settling agent, a bactericide and water uniformly to obtain a granulation liquid; SIII, preparation of water-based sand-containing colorful stone-like paint: The base paint is added into the granulation liquid, mixed and granulated to obtain a water-based sand-containing colorful stone-like paint.

[0066] The preparation method of the water-based sand-containing colorful stone-like paint provided by the present invention is simple and easy to operate, suitable for large-scale production, and has high market application value. It should be noted that the present invention does not limit the order of SI and SII.

[0067] Further preferably, in SI, the mass ratio of the first defoamer to the remaining defoamer is 0.9:1~1.1:1.

[0068] Preferably, in SI, the mass ratio of the first portion of water to the remaining portion of water is (20~23):(5~7). BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 Schematic diagram of the charge structure of lithium magnesium silicate in the present invention; Figure 2 It is a schematic diagram of the dehydration condensation reaction between the hydrazide amino group of the hydrazide-modified lithium magnesium silicate and the ketone carbonyl group of the functionalized acrylic emulsion in the present invention; Figure 3 Schematic diagram of the reaction equation in the preparation process of hydrazide-modified lithium magnesium silicate of the present invention; Wherein, k, m, n and p represent positive integers respectively, and R represents a methyl group or an ethyl group. DETAILED DESCRIPTION

[0070] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0071] Example 1 The present embodiment provides a water-based sand-containing colorful stone-like paint, which is composed of a base paint and a granulation liquid in a mass ratio of 8:2. The specific raw material composition and proportion are shown in Tables 1 and 2.

[0072] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint comprises the following steps: S1, preparation of functionalized acrylic emulsion: S1-1, weigh the raw material components according to the designed ratio, and evenly mix the ketone carbonyl-containing acrylic acid monomer, methyl methacrylate, methacrylic acid, butyl acrylate, 0.75 parts of emulsifier and 30 parts of water to obtain a pre-emulsion.

[0073] S1-2, 0.83 parts of emulsifier, buffer and 35 parts of water are mixed evenly, and the pre-emulsion and initiator are added dropwise at 83°C. After 2.5 hours of addition, the polymerization reaction is continued at 83°C and kept warm for 1.8 hours. The pH value of the obtained reaction solution is adjusted to 8.5 with a neutralizer to obtain a functionalized acrylic emulsion.

[0074] S2, preparation of hydrazide-modified lithium magnesium silicate: S2-1, 5 g of lithium magnesium silicate and 11 mL of KH-540 were added to 160 mL of toluene, heated to reflux, and the substitution reaction was carried out for 7.5 h. After the reaction was completed, the resulting reaction solution was stirred at room temperature for 13 h, filtered, and the filter cake was washed with a Soxhlet extractor for 17 h, and vacuum freeze-dried to obtain silane-modified lithium magnesium silicate.

[0075] S2-2, 5.5 g of silane-modified lithium magnesium silicate and 52 mL of methanol were mixed under N 2 The mixture was mixed and stirred for 35 min to 40 min under air flow for deoxygenation, and then 4.5 mL of methyl acrylate was added, and Michael addition reaction was carried out for 52 h at room temperature in the dark. After the reaction, the obtained reaction solution was subjected to reduced pressure distillation to remove methanol to obtain methyl acrylate-capped lithium magnesium silicate.

[0076] S2-3, 6.3 g of methyl acrylate-terminated lithium magnesium silicate and 20 mL of 75% hydrazine hydrate were mixed in N 2 The mixture was mixed and stirred for 35 min to 40 min under air flow for deoxygenation, and then the condensation reaction was carried out at 76° C. for 23 h. After the reaction, the obtained reaction solution was concentrated, diluted with chloroform, washed with brine, dried over anhydrous sodium sulfate, and then concentrated under reduced pressure to remove chloroform to obtain hydrazide-modified lithium magnesium silicate.

[0077] S3, preparing base paint: Weigh each component according to the designed ratio, mix cellulose, dispersant, half of the defoamer and the first portion of water evenly, add pigments, fillers and neutralizers, mix evenly, then add antifreeze, film-forming aid, functionalized acrylic emulsion, the remaining defoamer and fungicide, mix evenly to obtain a mixed system.

[0078] Add lithium magnesium silicate and hydrazide-modified lithium magnesium silicate into the remaining water to obtain a protective glue solution. The mass ratio of the first water to the remaining water is 4:1.

[0079] Add the protective glue solution into the mixed system, then add quartz sand and color paste to obtain the basic paint.

[0080] S4, prepare granulation liquid: Weigh each component according to the designed ratio, mix lithium magnesium silicate, hydrazide-modified lithium magnesium silicate, anti-settling agent, bactericide and water evenly to obtain granulation liquid.

[0081] S5, preparing water-based sand-containing colorful stone-like paint: The base paint is added into the granulation liquid, mixed and granulated to obtain a water-based sand-containing colorful stone-like paint.

[0082] It should be noted that the present invention does not limit the sequence of S1 and S2, nor does it limit the sequence of S3 and S4.

[0083] Example 2 The present embodiment provides a water-based sand-containing colorful stone-like paint, which is composed of a base paint and a granulation liquid in a mass ratio of 7:3. The specific raw material composition and proportion are shown in Table 1 to Table 2.

[0084] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint comprises the following steps: S1, preparation of functionalized acrylic emulsion: S1-1, weigh the raw material components according to the designed ratio, and evenly mix the ketone carbonyl-containing acrylic monomer, methyl methacrylate, methacrylic acid, butyl acrylate, 0.64 parts of emulsifier and 29 parts of water to obtain a pre-emulsion.

[0085] S1-2, 0.64 parts of emulsifier, buffer and 34 parts of water are mixed evenly, and the pre-emulsion and initiator are added dropwise at 80°C. After 3 hours of addition, the polymerization reaction is continued at 80°C and kept warm for 2 hours; the pH value of the obtained reaction solution is adjusted to 8 with a neutralizer to obtain a functionalized acrylic emulsion.

[0086] S2, preparation of hydrazide-modified lithium magnesium silicate: S2-1, 4.8 g of lithium magnesium silicate and 10.2 mL of KH-540 were added to 150 mL of toluene, heated to reflux, and the substitution reaction was carried out for 7 hours; after the reaction was completed, the resulting reaction solution was stirred at room temperature for 14 hours, filtered, and the filter cake was washed with a Soxhlet extractor for 16 hours, and vacuum freeze-dried to obtain silane-modified lithium magnesium silicate.

[0087] S2-2, 5.2 g of silane-modified lithium magnesium silicate and 48 mL of ethanol were mixed in N 2 The mixture was mixed and stirred for 35 min to 40 min under air flow for deoxygenation, and then 4.2 mL of methyl acrylate was added, and Michael addition reaction was carried out for 48 h at room temperature in the dark. After the reaction, the obtained reaction solution was subjected to reduced pressure distillation to remove ethanol to obtain methyl acrylate-capped lithium magnesium silicate.

[0088] S2-3, 6 g of methyl acrylate-terminated lithium magnesium silicate and 18 mL of 80% hydrazine hydrate were mixed in N 2The mixture was mixed and stirred for 35 min to 40 min under air flow for deoxygenation, and then the condensation reaction was carried out at 75° C. for 24 h. After the reaction, the obtained reaction solution was concentrated, diluted with benzene, washed with brine, dried with anhydrous sodium sulfate, and then concentrated under reduced pressure to remove benzene to obtain hydrazide-modified lithium magnesium silicate.

[0089] S3, preparing base paint: Weigh each component according to the designed ratio, mix cellulose, dispersant, half of the defoamer and the first portion of water evenly, add pigments, fillers and neutralizers, mix evenly, then add antifreeze, film-forming aid, functionalized acrylic emulsion, the remaining defoamer and fungicide, mix evenly to obtain a mixed system.

[0090] Add lithium magnesium silicate and hydrazide-modified lithium magnesium silicate into the remaining water to obtain a protective glue solution. The mass ratio of the first water to the remaining water is 23:5.

[0091] Add the protective glue solution into the mixed system, then add quartz sand and color paste to obtain the basic paint.

[0092] S4, prepare granulation liquid: Weigh each component according to the designed ratio, mix lithium magnesium silicate, hydrazide-modified lithium magnesium silicate, anti-settling agent, bactericide and water evenly to obtain granulation liquid.

[0093] S5, preparing water-based sand-containing colorful stone-like paint: The base paint is added into the granulation liquid, mixed and granulated to obtain a water-based sand-containing colorful stone-like paint.

[0094] It should be noted that the present invention does not limit the sequence of S1 and S2, nor does it limit the sequence of S3 and S4.

[0095] Example 3 The present embodiment provides a water-based sand-containing colorful stone-like paint, which is composed of a base paint and a granulation liquid in a mass ratio of 7:3. The specific raw material composition and proportion are shown in Table 1 to Table 2.

[0096] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint comprises the following steps: S1, preparation of functionalized acrylic emulsion: S1-1, weigh the raw material components according to the designed ratio, and evenly mix the ketone carbonyl-containing acrylic monomer, methyl methacrylate, methacrylic acid, butyl acrylate, 0.73 parts of emulsifier and 28 parts of water to obtain a pre-emulsion.

[0097] S1-2, 0.67 parts of emulsifier, buffer and 35 parts of water are mixed evenly, and the pre-emulsion and initiator are added dropwise at 85°C. After 2 hours of addition, the polymerization reaction is continued at 85°C and kept warm for 1.5 hours. The pH value of the obtained reaction solution is adjusted to 9 with a neutralizer to obtain a functionalized acrylic emulsion.

[0098] S2, preparation of hydrazide-modified lithium magnesium silicate: S2-1, 5.2 g of lithium magnesium silicate and 12.8 mL of KH-540 were added to 180 mL of toluene, heated to reflux, and the substitution reaction was carried out for 8 hours; after the reaction was completed, the resulting reaction solution was stirred at room temperature for 12 hours, filtered, and the filter cake was washed with a Soxhlet extractor for 18 hours, and vacuum freeze-dried to obtain silane-modified lithium magnesium silicate.

[0099] S2-2, 5.7 g of silane-modified lithium magnesium silicate and 55 mL of N,N-dimethylformamide were mixed in N 2 The mixture was mixed and stirred for 35 min to 40 min under air flow for deoxygenation, and then 4.8 mL of methyl acrylate was added, and Michael addition reaction was carried out for 56 h at room temperature in the dark. After the reaction, the obtained reaction solution was subjected to reduced pressure distillation to remove N,N-dimethylformamide to obtain methyl acrylate-capped lithium magnesium silicate.

[0100] S2-3, 6.5 g of methyl acrylate-capped lithium magnesium silicate and 21 mL of 70% hydrazine hydrate were mixed in N 2 The mixture was mixed and stirred for 35 min to 40 min under air flow for deoxygenation, and then the condensation reaction was carried out at 78° C. for 22 h. After the reaction, the obtained reaction solution was concentrated, diluted with toluene, washed with brine, dried over anhydrous sodium sulfate, and then concentrated under reduced pressure to remove toluene to obtain hydrazide-modified lithium magnesium silicate.

[0101] S3, preparing base paint: Weigh each component according to the designed ratio, mix cellulose, dispersant, half of the defoamer and the first portion of water evenly, add pigments, fillers and neutralizers, mix evenly, then add antifreeze, film-forming aid, functionalized acrylic emulsion, the remaining defoamer and fungicide, mix evenly to obtain a mixed system.

[0102] Add lithium magnesium silicate and hydrazide-modified lithium magnesium silicate into the remaining water to obtain a protective glue solution. The mass ratio of the first water to the remaining water is 23:7.

[0103] Add the protective glue solution into the mixed system, and then add quartz sand to obtain the base paint.

[0104] S4, prepare granulation liquid: Weigh each component according to the designed ratio, mix lithium magnesium silicate, hydrazide-modified lithium magnesium silicate, anti-settling agent, bactericide and water evenly to obtain granulation liquid.

[0105] S5, preparing water-based sand-containing colorful stone-like paint: The base paint is added into the granulation liquid, mixed and granulated to obtain a water-based sand-containing colorful stone-like paint.

[0106] It should be noted that the present invention does not limit the sequence of S1 and S2, nor does it limit the sequence of S3 and S4.

[0107] Example 4 The present embodiment provides a water-based sand-containing colorful stone-like paint, which is composed of a base paint and a granulation liquid in a mass ratio of 75:25. The specific raw material composition and proportion are shown in Tables 1 and 2.

[0108] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint is the same as that of Example 1 (the mass ratio of the emulsifier in S1-1 to the emulsifier in S1-2 is 1:1, and the mass ratio of water in S1-1 to water in S1-2 is 27:34), which will not be repeated here.

[0109] Example 5 The present embodiment provides a water-based sand-containing colorful stone-like paint, which is composed of a base paint and a granulation liquid in a mass ratio of 75:25. The specific raw material composition and proportion are shown in Tables 1 and 2.

[0110] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint is the same as that of Example 1 (the mass ratio of the emulsifier in S1-1 to the emulsifier in S1-2 is 1:1, and the mass ratio of water in S1-1 to water in S1-2 is 30:38), which will not be repeated here.

[0111] Table 1 Raw material components and proportions of water-based sand-containing colorful stone-like coatings of Examples 1 to 5 (%)

[0112] Table 2 Raw material components and proportions of functionalized acrylic emulsions of Examples 1 to 5 (parts)

[0113] Example 6 The present embodiment provides a water-based sand-containing colorful stone-like paint, whose raw material components are exactly the same as those in Example 4, and the ratio of each raw material component is similar to that in Example 4, the only difference is that in the functionalized acrylic emulsion, the mass fraction of MAA is replaced from 0.8 parts to 1.8 parts, and the other ratios are the same as those in the embodiment and will not be repeated.

[0114] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint is the same as that of Example 4, which will not be repeated here.

[0115] Comparative Example 1 This comparative example provides a water-based sand-containing colorful stone-like paint, which consists of a base paint, a granulating liquid and a continuous phase in a mass ratio of 8:2:2.

[0116] The raw material components and proportions of the base paint and the granulation liquid are similar to those in Example 1, except that the functionalized acrylic emulsion in the base paint is replaced with an equal mass of commercially available acrylic emulsion Badfu RS-2788, and the hydrazide-modified lithium magnesium silicate in the base paint and the granulation liquid is replaced with an equal mass of lithium magnesium silicate. The remaining raw material components and proportions are the same as those in Example 1 and will not be repeated.

[0117] The continuous phase is composed of the following raw material components in percentage: acrylic emulsion (Badford RS-3799) 60%, antifreeze (Runtai Chemical) 2%, Runtai Chemical C-123%, San Nopco NXZ 0.3%, Hoffman CMIT / MIT (1:1) 0.4%, ammonia (Jingxin Hongrun) 0.4%, thickener (Dow Chemical TT-935) 1% and deionized water 32.9%.

[0118] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint comprises the following steps: S1~S2, except that the functionalized acrylic emulsion is replaced by Badfu RS-2788 and the hydrazide-modified lithium magnesium silicate is replaced by lithium magnesium silicate, the remaining steps are the same as S3~S4 of Example 1, and will not be repeated here.

[0119] S3, mix Budford RS-3799, antifreeze, Runtai Chemical C-12, San Nopco NXZ, Hoffman CMIT / MIT (1:1), ammonia water, thickener and deionized water to obtain a continuous phase.

[0120] S4, mixing the base paint and the granulation liquid evenly, adding the continuous phase, mixing and granulating, and obtaining a water-based sand-containing colorful stone-like paint.

[0121] It should be noted that there is no order of precedence between S1~S3.

[0122] Comparative Example 2 This comparative example provides a water-based sand-containing colorful stone-like paint, whose raw material components and proportions are similar to those of Example 2, except that the functionalized acrylic emulsion in the base paint is replaced with commercially available acrylic emulsion Bader RS-2788 of equal mass, and the hydrazide-modified lithium magnesium silicate in the base paint and the granulation liquid is replaced with lithium magnesium silicate of equal mass, respectively. The remaining raw material components and proportions are the same as those of Example 2 and will not be repeated.

[0123] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint comprises the following steps: S1~S2 are the same as S1~S2 in Comparative Example 1 and will not be described in detail.

[0124] S3 is the same as S5 in Example 2 and will not be described in detail.

[0125] Comparative Example 3 This comparative example provides a water-based sand-containing colorful stone-like paint, whose raw material components and proportions are similar to those of Example 3, except that the hydrazide-modified lithium magnesium silicate in the base paint and the granulation liquid is replaced with lithium magnesium silicate of the same mass. The remaining raw material components and proportions are the same as those of Example 3 and are not described in detail.

[0126] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint comprises the following steps: S1 is the same as S1 in Example 3 and will not be described in detail.

[0127] S2~S3, except that the hydrazide-modified lithium magnesium silicate is replaced by lithium magnesium silicate, the remaining steps are the same as S3~S4 of Example 3, and will not be repeated here.

[0128] S4 is the same as S5 in Example 3 and will not be described in detail.

[0129] Comparative Example 4 This comparative example provides a water-based sand-containing colorful stone-like paint, whose raw material components and proportions are similar to those of Example 1, except that the functionalized acrylic emulsion in the base paint is replaced with a commercially available acrylic emulsion of the same quality, Bader RS-2788. The remaining raw material components and proportions are the same as those of Example 1 and will not be repeated.

[0130] The preparation method of the above-mentioned water-based sand-containing colorful stone-like paint comprises the following steps: S1 is the same as S2 in Example 1 and will not be described in detail.

[0131] S2, except that the functionalized acrylic emulsion is replaced by Badful RS-2788, the remaining steps are the same as S3 of Example 1, and will not be repeated here.

[0132] S3~S4 are the same as S4~S5 in Example 1 and will not be described in detail.

[0133] Comparative Example 5 This comparative example provides a water-based sand-containing colorful stone-like paint, whose raw material components and proportions are similar to those of Example 4, except that: MAA in the functionalized acrylic emulsion is omitted. The remaining raw material components and proportions are the same as those of Example 4 and will not be repeated.

[0134] Except for the above differences, the preparation method of the above water-based sand-containing colorful stone-like paint is the same as that of Example 4 and will not be repeated here.

[0135] Comparative Example 6 This comparative example provides a water-based sand-containing colorful stone-like paint, whose raw material components and proportions are similar to those of Example 5, except that the ketone carbonyl-containing acrylic monomer in the functionalized acrylic emulsion is omitted. The remaining raw material components and proportions are the same as those of Example 5 and are not described in detail.

[0136] Except for the above differences, the preparation method of the above water-based sand-containing colorful stone-like paint is the same as that of Example 5 and will not be described in detail.

[0137] Performance Testing According to the requirements of HG / T4343-2012 "Water-based Multicolor Architectural Coatings", the performance tests were conducted on the water-based sand-containing multicolor imitation stone coatings provided in Examples 1 to 6 of the present invention and Comparative Examples 1 to 5, respectively. The composite coating test was transparent primer + water-based sand-containing multicolor imitation stone coating midcoat + matte topcoat. The test results are shown in Table 3 (the states in the container are all normal).

[0138] Post-thickening test conditions include: Initial viscosity: Test the viscosity of the coating within 2 hours after preparation at 23℃±0.5℃, and record it as initial viscosity; Hot storage viscosity: After hot storage in a 50℃±5℃ oven for 3 days, take it out and keep the temperature at 23℃±0.5℃ to test the coating viscosity, which is recorded as hot storage viscosity; Post-thickening viscosity = thermal storage viscosity - initial viscosity.

[0139] Table 3 Comprehensive performance test results of water-based sand-containing colorful stone-like coatings of embodiments and comparative examples

[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based sand-containing colorful stone-like paint, It is characterized in that It is composed of base paint and granulating liquid; The base paint comprises a functionalized acrylic emulsion containing ketone carbonyl and carboxyl groups and hydrazide-modified lithium magnesium silicate containing amino groups; the granulation liquid comprises the hydrazide-modified lithium magnesium silicate; The components of the functionalized acrylic emulsion include the structural formula shown in Formula 1: Formula 1; In the formula, R is selected from or ; R' is selected from -H or -CH 3 ; j, t, s, and q independently represent positive integers.

2. The water-based sand-containing colorful stone-like paint according to claim 1, It is characterized in that The functionalized acrylic emulsion is polymerized from acrylic monomers containing ketocarbonyl groups, methyl methacrylate, methacrylic acid and butyl acrylate; The ketone carbonyl-containing acrylic monomer is selected from at least one of diacetone acrylamide and acetoacetoxyethyl methacrylate.

3. The water-based sand-containing colorful stone-like paint according to claim 1 or 2, It is characterized in that The raw materials of the functionalized acrylic emulsion include the following components in parts by weight: 4-5.2 parts of ketocarbonyl-containing acrylic monomer, 17.5-19 parts of methyl methacrylate, 0.5-0.8 parts of methacrylic acid, 9.5-11 parts of butyl acrylate, 1.28-1.58 parts of emulsifier, 0.12-0.15 parts of buffer, 0.1-0.12 parts of initiator and 61-68 parts of water; The pH value of the functionalized acrylic emulsion is 8-9.

4. The water-based sand-containing colorful stone-like paint as claimed in claim 3, It is characterized in that The preparation method of the functionalized acrylic emulsion comprises the following steps: Sa, weighing each raw material component according to the designed ratio, and uniformly mixing the ketone carbonyl-containing acrylic acid monomer, methyl methacrylate, methacrylic acid, butyl acrylate, the first part of the emulsifier and the first part of the water to obtain a pre-emulsion; Sb, the remaining emulsifier, buffer and the remaining water are mixed evenly, the pre-emulsion and initiator are added at 80° C. to 85° C., the polymerization reaction is carried out for 1.5 h to 2 h, and the pH of the obtained reaction solution is adjusted to 8 to 9 to obtain a functionalized acrylic emulsion.

5. The water-based sand-containing colorful stone-like paint according to claim 1, It is characterized in that The preparation method of the hydrazide-modified lithium magnesium silicate comprises the following steps: S1, adding lithium magnesium silicate and a silane coupling agent into a first solvent, heating to reflux, and performing a substitution reaction to obtain silane-modified lithium magnesium silicate; S2, adding the silane-modified lithium magnesium silicate and methyl acrylate to a second solvent under a protective atmosphere and light-proof conditions to carry out a Michael addition reaction to obtain methyl acrylate-terminated lithium magnesium silicate; S3, adding the methyl acrylate-terminated lithium magnesium silicate to hydrazine hydrate, and carrying out a condensation reaction at 75° C. to 78° C. under a protective atmosphere to obtain hydrazide-modified lithium magnesium silicate.

6. The water-based sand-containing colorful stone-like paint according to claim 5, It is characterized in that In S1, the silane coupling agent is aminopropyltrimethoxysilane; and / or In S1, the first solvent is toluene; and / or In S1, the mass volume ratio of the lithium magnesium silicate, the silane coupling agent and the first solvent is (4.8-5.2) g: (10.2-12.8) mL: (150-180) mL; and / or In S2, the second solvent is selected from methanol, ethanol or N,N-dimethylformamide; and / or In S2, the mass volume ratio of the silane-modified lithium magnesium silicate, the methyl acrylate and the second solvent is (5.2-5.7) g: (4.2-4.8) mL: (48-55) mL; and / or In S3, the volume concentration of hydrazine hydrate is 70% to 80%; and / or In S3, the mass volume ratio of the methyl acrylate-capped lithium magnesium silicate to the hydrazine hydrate is (6-6.5) g: (18-21) mL.

7. The water-based sand-containing colorful stone-like paint according to claim 5, It is characterized in that In S1, the substitution reaction time is 7h~8h; and / or In S2, the temperature of the Michael addition reaction is 10°C to 40°C, and the reaction time is 48h to 56h; and / or In S3, the condensation reaction time is 22h~24h.

8. The water-based sand-containing colorful stone-like paint according to claim 1, It is characterized in that The base paint and the granulation liquid both include lithium magnesium silicate; and / or The mass ratio of the base paint to the granulation liquid is 7:3 to 8:

2.

9. The water-based sand-containing colorful stone-like paint according to claim 1 or 8, It is characterized in that The base paint comprises the following components in percentage by weight: 22% to 25% functionalized acrylic emulsion, 0.38% to 0.42% lithium magnesium silicate, 0.19% to 0.21% hydrazide-modified lithium magnesium silicate, 0.6% to 1% cellulose, 0.08% to 0.12% dispersant, 0.2% to 0.4% defoamer, 0.7% to 1.2% antifreeze, 1.2% to 1.8% film-forming aid, 0.3% to 0.6% fungicide, 4.5% to 5.8% pigment filler, 0.08% to 0.12% neutralizer, 32% to 38% quartz sand, 0% to 2% color paste and 25% to 30% water; and / or The granulation liquid comprises the following components in percentage by weight: 2% to 3.5% of lithium magnesium silicate, 2.2% to 3.5% of hydrazide-modified lithium magnesium silicate, 0.35% to 0.5% of an anti-settling agent, 0.3% to 0.5% of a bactericide, and 92% to 95% of water.

10. The method for preparing the water-based sand-containing colorful stone-like paint according to claim 9, It is characterized in that The following steps are involved: SI, preparation of base paint: Weigh each raw material component according to the designed ratio, mix cellulose, dispersant, the first portion of defoamer and the first portion of water evenly, add pigments and fillers and neutralizers, mix evenly, then add antifreeze, film-forming aid, functionalized acrylic emulsion, the remaining portion of defoamer and fungicide, mix evenly to obtain a mixed system; Adding lithium magnesium silicate and hydrazide-modified lithium magnesium silicate into the remaining water to obtain a protective colloid solution; Adding the protective glue solution into the mixed system, and then adding quartz sand and color paste to obtain a base paint; SII, Preparation of Granulation Solution: Mixing lithium magnesium silicate, hydrazide-modified lithium magnesium silicate, an anti-settling agent, a bactericide and water uniformly to obtain a granulation liquid; SIII, preparation of water-based sand-containing colorful stone-like paint: The base paint is added into the granulation liquid, mixed and granulated to obtain a water-based sand-containing colorful stone-like paint.

Citation Information

Patent Citations

  • Water white resistant particle crosslinking type water-in-water multicolor paint

    CN106634511A

  • Ketone-hydrazine crosslinking aqueous acrylic resin with film-forming-assisting function and preparation method and application thereof

    CN106674418A

  • Finish-coat-free matte water-based colored paint and preparation method thereof

    CN106675295A

  • Sand-in-sand multicolor coating, and preparation method and application thereof

    CN112010589A

  • Water-based emulsion, preparation method thereof and temperature-change-resistant construction real stone paint prepared from water-based emulsion