Wear-resistant leather fabric and preparation method thereof
By using a combination of low-temperature plasma treatment and a specific retanning agent in the preparation of leather fabrics, the problem of poor mechanical properties of leather fabrics caused by cumbersome coating and high-temperature baking in the existing technology is solved, and the wear resistance and softness of leather fabrics are achieved. The improvement extends the service life.
Patent Information
- Application Number
- CN202411033326.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-30
AI Technical Summary
In the existing preparation methods of wear-resistant leather fabrics, the coating process is cumbersome and high-temperature baking results in poor mechanical properties and softness of the leather fabric, making it difficult to use it for a long time.
Animal rawhide is used for degreasing, washing, low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquing, dyeing, and color fixation in sequence. The retanning agent is ricinoleic acid modified polyurethane and polyhedral oligomeric sesqui-silica. The combination of oxane, fibrous soy protein and zirconium oxide composite graphene oxide improves the retanning and fatliquoring effects through low-temperature plasma treatment and maintains the softness of the leather.
It achieves excellent wear resistance and good softness of leather fabrics, extends its service life, and avoids the problem of reduced wear resistance after the coating peels off.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fabric preparation, and in particular relates to a wear-resistant leather fabric and a preparation method thereof. Background Art
[0002] Leather fabrics are made by bonding animal leather with base fabric after degreasing and tanning. People subject raw hides such as cowhide, pigskin, and sheepskin to a series of physical and chemical treatments. After degreasing, liming, deliming and softening, pickling, tanning, neutralization, retanning, filling and fatliquoring, and dyeing, all other components in the raw hide are destroyed and removed, leaving only the collagen fibers and the basic organizational structure composed of collagen fibers that are needed for leather manufacturing. Leather fabrics are widely used in many industries such as the clothing industry, the shoe and bag industry, and the daily necessities industry. Compared with synthetic leather, animal leather has the advantages of high strength, durability, waterproofness, breathability, and good appearance.
[0003] With the improvement of national economic level, people's demand for animal leather products is getting higher and higher. However, animal leather products usually need careful care. With the long-term use of animal leather products, small molecules in animal leather migrate, the original texture and elasticity will disappear, and it will become brittle, aged, and cracked on the surface. However, the current pace of life is getting faster and faster, and people have limited energy to care for animal leather products. Therefore, improving the wear resistance of animal leather can play a certain protective role and extend the service life of animal leather products.
[0004] Patent CN103525957B discloses a method for producing wear-resistant leather, which takes a full leather material, and sequentially goes through primer, embossing, mid-coating, top-coating, tumbling, and color repair to obtain a finished leather product. This patented technology uses different coatings for finishing, layer by layer protection, and embosses the leather embryo with an embossing machine after the primer process, which effectively enhances the density of the leather embryo, and then improves the peel strength and wear resistance through special processes of mid-coating and top-coating. However, the coating process of this patented technology is cumbersome, and each layer of coating must be baked at 100°C or close to 100°C after completion. The baking temperature is high, resulting in poor mechanical properties of the product and poor softness. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a wear-resistant leather fabric and a preparation method thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical solution: A method for preparing wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is obtained by mixing ricinoleic acid-modified polyurethane, polyhedral oligomeric silsesquioxane, fibrous soy protein and zirconium oxide composite graphene oxide in a mass ratio of 1:0.1-0.2:0.2-0.3:0.1-0.2.
[0007] Preferably, the animal hide is selected from any one of cow hide, pig hide and sheep hide.
[0008] Preferably, the ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, toluene diisocyanate and polytetrahydrofuran diether alcohol are uniformly mixed at 70-80°C, dibutyltin dilaurate is added, and the mixture is polymerized for 2-3 hours at a temperature of 90-100°C, 2,2-dihydroxymethylpropionic acid and N-methyldiethanolamine are added, and the mixture is reacted for 2-3 hours at a temperature of 2-3 hours, ricinoleic acid is added, and the mixture is reacted for 2-3 hours at a temperature of 2-3 hours, and ricinoleic acid is added and the mixture is reacted for 2-3 hours at a temperature of 2-3 hours, and the mixture is naturally cooled to below 45°C, and triethylamine is used for neutralization, and distilled water is used for emulsification to obtain a ricinoleic acid modified polyurethane having a mass solid content of 35-40%; wherein the mass ratio of toluene diisocyanate, polytetrahydrofuran diether alcohol, dibutyltin dilaurate, 2,2-dihydroxymethylpropionic acid, N-methyldiethanolamine, and ricinoleic acid is 16:5:0.5-0.8:3-4:3-4:2-3.
[0009] Preferably, the polyhedral oligomeric silsesquioxane is prepared by the following method: first, γ-aminopropyltriethoxysilane and cyclohexane are mixed evenly, then a hydrochloric acid solution with a mass concentration of 30-40% is added, heated to 60-70°C, kept warm for reaction for 55-60 hours, and the solvent is evaporated under reduced pressure to obtain the polyhedral oligomeric silsesquioxane; wherein the dosage ratio of γ-aminopropyltriethoxysilane, cyclohexane, and hydrochloric acid solution is 5-6g:20-30mL:3-4mL.
[0010] Preferably, the fibrous soy protein is prepared by the following method: first, ultrasonically disperse the soy protein in 25 to 30 times its weight of water, adjust the pH to 11 to 12 using 1 to 2 mol / L sodium hydroxide solution, heat at 80 to 90°C for 10 to 12 minutes, centrifuge and take the supernatant to obtain a soy protein solution; then mix the soy protein solution with an equal volume of 0.6 to 1 mol / L tartaric acid solution, stir at 60 to 70°C for 40 to 50 minutes, irradiate with 300 to 500W microwaves for 2 to 3 minutes, adjust the pH to neutral using 1 to 2 mol / L sodium hydroxide solution, dialyze with a 10000 to 12000Da dialysis bag, dry, and crush to less than 500 mesh to obtain the fibrous soy protein.
[0011] Preferably, the zirconium oxide composite graphene oxide is prepared by the following method: first, zirconium oxide, graphene oxide and sodium bromide are crushed to 500 meshes according to a mass ratio of 30-40:170-180:9-10 and mixed to obtain a mixed powder; then, in a nitrogen atmosphere, the temperature is raised to 1200-1300°C at 3-5°C / min, and the mixture is kept warm and calcined for 6-7 hours, and naturally cooled to room temperature to obtain a calcined powder; finally, the calcined powder is mixed with an equal mass of water, subjected to ultrasonic oscillation treatment at 500-600W for 30-40 minutes, centrifuged to obtain a precipitate, dried, and crushed to less than 500 meshes to obtain the obtained product.
[0012] Preferably, the specific method of degreasing is: after washing the animal hide, completely immerse it in a degreasing agent solution of 12 to 15 times its weight, let it stand for 2 to 3 hours, adjust the pH to 2 to 3 with a 20 to 30% mass concentration of formic acid aqueous solution, rotate the drum for 2 to 3 hours, and drain the liquid.
[0013] Further preferably, the degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract in a mass ratio of 12 to 15:100; wherein, the animal fur waste extract is prepared by the following method: first, add the animal fur waste into 1 to 2 mol / L sodium hydroxide solution, stir and heat at 95 to 100°C for 6 to 8 hours, filter and take the filtrate while hot, naturally cool to 60 to 65°C, add lauroyl chloride dropwise to the filtrate, use 1 to 2 mol / L sodium hydroxide solution to control pH=9 to 10, stir for 3 to 4 hours after the addition is completed, and obtain the animal fur waste extract; wherein, the amount ratio of animal fur waste, sodium hydroxide solution, and lauroyl chloride is 3 to 4 kg: 2 to 3 kg: 0.2 to 0.3 mL.
[0014] Preferably, the specific method of washing is: first, wash the defatted leather material 2 to 3 times with water of 2 to 3 times its mass to obtain pre-washed leather; then add the pre-washed leather into water of 2 to 3 times its mass, adjust the pH to 7, stir at 35 to 40° C. for 1 to 2 hours, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather 2 to 3 times with water of 2 to 3 times its mass.
[0015] Preferably, the process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 20-30 Pa, power is 200-300 W, and treatment time is 30-40 s.
[0016] Preferably, the specific method of retanning is: soak the leather treated with low-temperature plasma in 40-50°C water which is 2-3 times its weight for 40-50 minutes, add the retanning agent, rotate the drum for 2-3 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:0.8-1.
[0017] Preferably, the process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.3-0.5, the air pressure is 100-120 Pa, the power is 300-400 W, and the treatment time is 2-3 minutes.
[0018] Preferably, the specific method of fatliquor is: soak the leather after retanning in 60-65°C water of 2-3 times its weight for 20-30 minutes, add fatliquor, rotate the drum for 2-3 hours, and discharge the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.3-0.4. Further preferably, the fatliquor is obtained by mixing castor oil phosphate, neatsfoot oil, animal fur waste extract, and polyethylene glycol 400 dioleate in a mass ratio of 1:1:0.1-0.2:0.3-0.4.
[0019] Further preferably, the animal fur waste extract is prepared by the following method: first add the animal fur waste into 1-2 mol / L sodium hydroxide solution, stir and heat at 95-100°C for 6-8 hours, filter and collect the filtrate while hot, and vacuum freeze-dry to obtain the extract; the mass ratio of animal fur waste to sodium hydroxide solution is 3-4:2-3.
[0020] A wear-resistant leather fabric is obtained by the above-mentioned preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial effects: The present invention sequentially degreases, washes, performs a first low-temperature plasma treatment, performs retanning, performs a second low-temperature plasma treatment, performs fatliquoring, dyes, and performs color fixation treatment on animal hides to obtain a leather fabric; wherein the retanning agent used in the retanning is obtained by mixing ricinoleic acid-modified polyurethane, polyhedral oligomeric silsesquioxane, fibrous soy protein, and zirconium oxide composite graphene oxide. The leather fabric obtained by the present invention has excellent wear resistance, prolongs the service life of the leather fabric, maintains good softness, and is more comfortable to use.
[0022] The present invention does not improve the wear resistance by forming a wear-resistant coating, which can avoid affecting the softness of the leather fabric on the one hand and avoid the loss of wear resistance after the coating falls off on the other hand.
[0023] The technical key of the present invention lies in the selection of retanning agent, with ricinoleic acid modified polyurethane as the main component, supplemented by polyhedral oligomeric silsesquioxane, fibrous soy protein, zirconium oxide composite graphene oxide. The hydroxyl group and double bond in ricinoleic acid are introduced into polyurethane to improve the retanning effect; polyhedral oligomeric silsesquioxane, fibrous soy protein, zirconium oxide composite graphene oxide further strengthen the retanning effect, and fully enter the interior of the leather fabric to improve the wear resistance of the product.
[0024] Low-temperature plasma treatment was carried out before retanning and fatliquoring, which was beneficial to the improvement of retanning and fatliquoring effects, ensuring the softness of the leather fabric and improving its wear resistance.
[0025] The fatliquor of the invention is prepared by mixing castor oil phosphate, neatsfoot oil, animal fur waste extract and polyethylene glycol 400 dioleate, and the softness is improved through the synergistic effect of the components. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Unless otherwise specified, all commodities in this invention are purchased through market channels.
[0028] For the convenience of comparison, the animal hides in the embodiments and comparative examples are all cow hides from the same source.
[0029] Example 1 A method for preparing wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is obtained by mixing 1kg of ricinoleic acid modified polyurethane, 0.1kg of polyhedral oligomeric silsesquioxane, 0.2kg of fibrous soy protein and 0.1kg of zirconium oxide composite graphene oxide.
[0030] The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, 1.6 kg of toluene diisocyanate and 0.5 kg of polytetramethylene glycol are uniformly mixed at 70° C., 0.05 kg of dibutyltin dilaurate is added, and the mixture is polymerized for 2 hours under heat preservation, heated to 90° C., 0.3 kg of 2,2-dihydroxymethylpropionic acid and 0.3 kg of N-methyldiethanolamine are added, and the mixture is reacted for 2 hours under heat preservation, 0.2 kg of ricinoleic acid is added, and the mixture is reacted for 2 hours under heat preservation, naturally cooled to below 45° C., neutralized with triethylamine, and emulsified with distilled water to obtain a ricinoleic acid modified polyurethane with a mass solid content of 35%.
[0031] Polyhedral oligomeric silsesquioxane is prepared by the following method: first, 0.5 kg of γ-aminopropyltriethoxysilane is uniformly mixed with 2 L of cyclohexane, then 0.3 L of 30% hydrochloric acid solution is added, heated to 60° C., kept warm for 55 hours, and the solvent is evaporated under reduced pressure to obtain the polyhedral oligomeric silsesquioxane.
[0032] The fibrous soy protein is prepared by the following method: first, the soy protein is ultrasonically dispersed in 25 times its weight of water, the pH is adjusted to 11 with a 1 mol / L sodium hydroxide solution, heated at 80°C for 10 minutes, and the supernatant is taken by centrifugation to obtain a soy protein solution; then, the soy protein solution is mixed with an equal volume of a 0.6 mol / L tartaric acid solution, stirred at 60°C for 40 minutes, irradiated with a 300 W microwave for 2 minutes, the pH is adjusted to neutral with a 1 mol / L sodium hydroxide solution, dialyzed with a 10000 Da dialysis bag, dried, and crushed to less than 500 meshes to obtain the fibrous soy protein.
[0033] The zirconium oxide composite graphene oxide is prepared by the following method: firstly, zirconium oxide, graphene oxide and sodium bromide are crushed to 500 meshes according to a mass ratio of 30:170:9 and mixed to obtain mixed powder; then, the temperature is raised to 1200°C at 3°C / min in a nitrogen atmosphere, and the mixture is kept warm and calcined for 6 hours, and naturally cooled to room temperature to obtain calcined powder; finally, the calcined powder is mixed with water of equal mass, subjected to 500W ultrasonic oscillation treatment for 30 minutes, centrifuged to obtain a precipitate, dried, and crushed to less than 500 meshes to obtain the obtained product.
[0034] The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 12 times its weight, let it stand for 2 hours, adjust the pH to 2 with a 20% mass concentration of formic acid aqueous solution, rotate the drum for 2 hours, and drain the liquid.
[0035] The degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract at a mass ratio of 12:100; wherein, the animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 0.2 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 9 with 1 mol / L sodium hydroxide solution. After the addition is completed, the mixture is stirred for 3 hours to obtain the animal fur waste extract.
[0036] The specific method of washing is: first wash the degreased leather twice with twice its mass of water to obtain pre-washed leather; then add the pre-washed leather into twice its mass of water, adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather twice with twice its mass of water.
[0037] The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 20Pa, power is 200W, and treatment time is 30s.
[0038] The specific method of retanning is: soak the leather treated with low-temperature plasma in 40°C water twice its weight for 40 minutes, add the retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:0.8.
[0039] The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.3, the gas pressure is 100Pa, the power is 300W, and the treatment time is 2 minutes.
[0040] The specific method of fatliquoring is: soak the leather after retanning in 60°C water twice its weight for 20 minutes, add fatliquor, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.3. The fatliquor is prepared by mixing 1 kg of castor oil phosphate, 1 kg of neat's foot oil, 0.1 kg of animal fur waste extract, and 0.3 kg of polyethylene glycol 400 dioleate.
[0041] The animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated at 95° C. with stirring for 6 hours, the filtrate is filtered while hot, and vacuum freeze-dried to obtain the extract.
[0042] Example 2 A method for preparing a wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is obtained by mixing 1kg of ricinoleic acid-modified polyurethane, 0.2kg of polyhedral oligomeric silsesquioxane, 0.3kg of fibrous soy protein and 0.2kg of zirconium oxide composite graphene oxide.
[0043] The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, 1.6 kg of toluene diisocyanate and 0.5 kg of polytetramethylene glycol are uniformly mixed at 80° C., 0.08 kg of dibutyltin dilaurate is added, and the mixture is polymerized for 3 hours under heat preservation, and the mixture is heated to 100° C., 0.4 kg of 2,2-dihydroxymethylpropionic acid and 0.4 kg of N-methyldiethanolamine are added, and the mixture is reacted for 3 hours under heat preservation, 0.3 kg of ricinoleic acid is added, and the mixture is reacted for 3 hours under heat preservation, and the mixture is naturally cooled to below 45° C., triethylamine is used for neutralization, and distilled water is used for emulsification to obtain a ricinoleic acid modified polyurethane with a mass solid content of 40%.
[0044] Polyhedral oligomeric silsesquioxane is prepared by the following method: first, 0.6 kg of γ-aminopropyltriethoxysilane is uniformly mixed with 3 L of cyclohexane, then 0.4 L of 40% hydrochloric acid solution is added, heated to 70° C., kept warm for 60 hours, and the solvent is evaporated under reduced pressure to obtain the polyhedral oligomeric silsesquioxane.
[0045] The fibrous soy protein is prepared by the following method: first, the soy protein is ultrasonically dispersed in 30 times its weight of water, the pH is adjusted to 12 with a 2mol / L sodium hydroxide solution, heated at 90°C for 12 minutes, and the supernatant is centrifuged to obtain a soy protein solution; then the soy protein solution is mixed with an equal volume of a 1mol / L tartaric acid solution, stirred at 70°C for 50 minutes, irradiated with a 500W microwave for 3 minutes, the pH is adjusted to neutral with a 2mol / L sodium hydroxide solution, dialyzed with a 12000Da dialysis bag, dried, and crushed to less than 500 meshes to obtain the fibrous soy protein.
[0046] The zirconium oxide composite graphene oxide is prepared by the following method: firstly, zirconium oxide, graphene oxide and sodium bromide are crushed to 500 meshes according to a mass ratio of 40:180:10 and mixed to obtain mixed powder; then, the temperature is raised to 1300°C at 5°C / min in a nitrogen atmosphere, and the mixture is kept warm and calcined for 7 hours, and naturally cooled to room temperature to obtain calcined powder; finally, the calcined powder is mixed with water of equal mass, subjected to 600W ultrasonic oscillation treatment for 40 minutes, centrifuged to obtain a precipitate, dried, and crushed to less than 500 meshes to obtain the composite.
[0047] The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 15 times its weight, let it stand for 3 hours, adjust the pH to 3 with a 30% mass concentration of formic acid aqueous solution, rotate the drum for 3 hours, and drain the liquid.
[0048] The degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract at a mass ratio of 15:100; wherein, the animal fur waste extract is prepared by the following method: first, 4 kg of animal fur waste is added to 3 kg of 2 mol / L sodium hydroxide solution, heated with stirring at 100°C for 8 hours, the filtrate is filtered while hot, naturally cooled to 65°C, 0.3 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 10 with 2 mol / L sodium hydroxide solution. After the addition is completed, the mixture is stirred for 4 hours to obtain the animal fur waste extract.
[0049] The specific method of washing is: first wash the degreased leather with 3 times its mass of water for 3 times to obtain pre-washed leather; then add the pre-washed leather into 3 times its mass of water, adjust the pH to 7, stir at 40°C for 2 hours, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather with 3 times its mass of water for 3 times.
[0050] The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 30Pa, power is 300W, and treatment time is 40s.
[0051] The specific method of retanning is: soak the leather treated with low-temperature plasma in 50°C water three times its weight for 50 minutes, add the retanning agent, rotate the drum for 3 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:1.
[0052] The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.5, the gas pressure is 120Pa, the power is 400W, and the treatment time is 3 minutes.
[0053] The specific method of fatliquoring is: soak the leather after retanning in 65°C water three times its weight for 30 minutes, add fatliquor, rotate the drum for 3 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.4. The fatliquor is prepared by mixing 1 kg of castor oil phosphate, 1 kg of neat's foot oil, 0.2 kg of animal fur waste extract, and 0.4 kg of polyethylene glycol 400 dioleate.
[0054] The animal fur waste extract is prepared by the following method: first, 4 kg of animal fur waste is added into 3 kg of 2 mol / L sodium hydroxide solution, heated with stirring at 100° C. for 8 hours, filtered while hot to obtain the filtrate, and vacuum freeze-dried to obtain the extract.
[0055] Example 3 A method for preparing a wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is obtained by mixing 1kg of ricinoleic acid-modified polyurethane, 0.15kg of polyhedral oligomeric silsesquioxane, 0.25kg of fibrous soy protein and 0.15kg of zirconium oxide composite graphene oxide.
[0056] The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, 1.6 kg of toluene diisocyanate and 0.5 kg of polytetramethylene glycol are uniformly mixed at 75° C., 0.07 kg of dibutyltin dilaurate is added, and the mixture is polymerized for 2.5 hours under heat preservation, heated to 95° C., 0.35 kg of 2,2-dihydroxymethylpropionic acid and 0.35 kg of N-methyldiethanolamine are added, and the mixture is reacted for 2.5 hours under heat preservation, 0.25 kg of ricinoleic acid is added, and the mixture is reacted for 2.5 hours under heat preservation, and naturally cooled to below 45° C., neutralized with triethylamine, and emulsified with distilled water to obtain a ricinoleic acid modified polyurethane with a mass solid content of 37%.
[0057] Polyhedral oligomeric silsesquioxane is prepared by the following method: first, 0.55 kg of γ-aminopropyltriethoxysilane is uniformly mixed with 2.5 L of cyclohexane, then 0.35 L of 35% hydrochloric acid solution is added, heated to 65° C., kept warm for 57 hours, and the solvent is evaporated under reduced pressure to obtain the polyhedral oligomeric silsesquioxane.
[0058] The fibrous soy protein is prepared by the following method: first, the soy protein is ultrasonically dispersed in 28 times its weight of water, the pH is adjusted to 11 with a 1.5 mol / L sodium hydroxide solution, heated at 85°C for 11 minutes, and the supernatant is taken by centrifugation to obtain a soy protein solution; then, the soy protein solution is mixed with an equal volume of a 0.8 mol / L tartaric acid solution, stirred at 65°C for 45 minutes, irradiated with a 450 W microwave for 2 minutes, the pH is adjusted to neutral with a 1 mol / L sodium hydroxide solution, dialyzed with a 12000 Da dialysis bag, dried, and crushed to less than 500 meshes to obtain the fibrous soy protein.
[0059] The zirconium oxide composite graphene oxide is prepared by the following method: firstly, zirconium oxide, graphene oxide and sodium bromide are crushed to 500 meshes according to a mass ratio of 35:175:9 and mixed to obtain mixed powder; then, the temperature is raised to 1250°C at 4°C / min in a nitrogen atmosphere, and the mixture is calcined for 6 hours at the temperature, and naturally cooled to room temperature to obtain calcined powder; finally, the calcined powder is mixed with water of equal mass, subjected to 600W ultrasonic oscillation treatment for 35 minutes, centrifuged to obtain a precipitate, dried, and crushed to less than 500 meshes to obtain the obtained product.
[0060] The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 13 times its weight, let it stand for 2 hours, adjust the pH to 2 with a 25% mass concentration of formic acid aqueous solution, rotate the drum for 3 hours, and drain the liquid.
[0061] The degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract at a mass ratio of 13:100; wherein, the animal fur waste extract is prepared by the following method: first, 3.5 kg of animal fur waste is added to 2.5 kg of 1 mol / L sodium hydroxide solution, and heated with stirring at 98°C for 7 hours, and the filtrate is filtered while hot, and naturally cooled to 62°C, and 0.2 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 10 with 1 mol / L sodium hydroxide solution. After the addition is completed, the mixture is stirred for 3 hours to obtain the animal fur waste extract.
[0062] The specific method of washing is: first wash the degreased leather twice with 3 times its mass of water to obtain pre-washed leather; then add the pre-washed leather into 2 times its mass of water, adjust the pH to 7, stir at 38°C for 1.5 hours, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather twice with 2.5 times its mass of water.
[0063] The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 25Pa, power is 300W, and treatment time is 40s.
[0064] The specific method of retanning is: soak the leather treated with low-temperature plasma in 50°C water twice its weight for 45 minutes, add the retanning agent, rotate the drum for 2.5 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:1.
[0065] The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.5, the gas pressure is 120Pa, the power is 400W, and the treatment time is 2 minutes.
[0066] The specific method of fatliquoring is: soak the leather after retanning in 65°C water three times its weight for 30 minutes, add fatliquoring agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquoring agent is 100:0.3.
[0067] The fatliquor is prepared by mixing 1 kg of castor oil phosphate, 1 kg of neat's foot oil, 0.1 kg of animal fur waste extract, and 0.3 kg of polyethylene glycol 400 dioleate.
[0068] The animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added into 2 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 100° C. for 7 hours, filtered while hot to obtain the filtrate, and vacuum freeze-dried to obtain the extract.
[0069] Comparative Example 1 A method for preparing wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is obtained by mixing 1 kg of ricinoleic acid modified polyurethane, 0.1 kg of polyhedral oligomeric silsesquioxane and 0.1 kg of zirconium oxide composite graphene oxide.
[0070] The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, 1.6 kg of toluene diisocyanate and 0.5 kg of polytetramethylene glycol are uniformly mixed at 70° C., 0.05 kg of dibutyltin dilaurate is added, and the mixture is polymerized for 2 hours under heat preservation, heated to 90° C., 0.3 kg of 2,2-dihydroxymethylpropionic acid and 0.3 kg of N-methyldiethanolamine are added, and the mixture is reacted for 2 hours under heat preservation, 0.2 kg of ricinoleic acid is added, and the mixture is reacted for 2 hours under heat preservation, naturally cooled to below 45° C., neutralized with triethylamine, and emulsified with distilled water to obtain a ricinoleic acid modified polyurethane with a mass solid content of 35%.
[0071] Polyhedral oligomeric silsesquioxane is prepared by the following method: first, 0.5 kg of γ-aminopropyltriethoxysilane is uniformly mixed with 2 L of cyclohexane, then 0.3 L of 30% hydrochloric acid solution is added, heated to 60° C., kept warm for 55 hours, and the solvent is evaporated under reduced pressure to obtain the polyhedral oligomeric silsesquioxane.
[0072] The zirconium oxide composite graphene oxide is prepared by the following method: firstly, zirconium oxide, graphene oxide and sodium bromide are crushed to 500 meshes according to a mass ratio of 30:170:9 and mixed to obtain mixed powder; then, the temperature is raised to 1200°C at 3°C / min in a nitrogen atmosphere, and the mixture is kept warm and calcined for 6 hours, and naturally cooled to room temperature to obtain calcined powder; finally, the calcined powder is mixed with water of equal mass, subjected to 500W ultrasonic oscillation treatment for 30 minutes, centrifuged to obtain a precipitate, dried, and crushed to less than 500 meshes to obtain the obtained product.
[0073] The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 12 times its weight, let it stand for 2 hours, adjust the pH to 2 with a 20% mass concentration of formic acid aqueous solution, rotate the drum for 2 hours, and drain the liquid.
[0074] The degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract at a mass ratio of 12:100; wherein, the animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 0.2 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 9 with 1 mol / L sodium hydroxide solution. After the addition is completed, the mixture is stirred for 3 hours to obtain the animal fur waste extract.
[0075] The specific method of washing is: first wash the degreased leather twice with twice its mass of water to obtain pre-washed leather; then add the pre-washed leather into twice its mass of water, adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather twice with twice its mass of water.
[0076] The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 20Pa, power is 200W, and treatment time is 30s.
[0077] The specific method of retanning is: soak the leather treated with low-temperature plasma in 40°C water twice its weight for 40 minutes, add the retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:0.8.
[0078] The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.3, the gas pressure is 100Pa, the power is 300W, and the treatment time is 2 minutes.
[0079] The specific method of fatliquoring is: soak the leather after retanning in 60°C water twice its weight for 20 minutes, add fatliquor, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.3. The fatliquor is prepared by mixing 1 kg of castor oil phosphate, 1 kg of neat's foot oil, 0.1 kg of animal fur waste extract, and 0.3 kg of polyethylene glycol 400 dioleate.
[0080] The animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated at 95° C. with stirring for 6 hours, the filtrate is filtered while hot, and vacuum freeze-dried to obtain the extract.
[0081] Comparative Example 2 A method for preparing wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is obtained by mixing 1kg of ricinoleic acid modified polyurethane, 0.2kg of fibrous soy protein and 0.1kg of zirconium oxide composite graphene oxide.
[0082] The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, 1.6 kg of toluene diisocyanate and 0.5 kg of polytetramethylene glycol are uniformly mixed at 70° C., 0.05 kg of dibutyltin dilaurate is added, and the mixture is polymerized for 2 hours under heat preservation, heated to 90° C., 0.3 kg of 2,2-dihydroxymethylpropionic acid and 0.3 kg of N-methyldiethanolamine are added, and the mixture is reacted for 2 hours under heat preservation, 0.2 kg of ricinoleic acid is added, and the mixture is reacted for 2 hours under heat preservation, naturally cooled to below 45° C., neutralized with triethylamine, and emulsified with distilled water to obtain a ricinoleic acid modified polyurethane with a mass solid content of 35%.
[0083] The fibrous soy protein is prepared by the following method: first, the soy protein is ultrasonically dispersed in 25 times its weight of water, the pH is adjusted to 11 with a 1 mol / L sodium hydroxide solution, heated at 80°C for 10 minutes, and the supernatant is taken by centrifugation to obtain a soy protein solution; then, the soy protein solution is mixed with an equal volume of a 0.6 mol / L tartaric acid solution, stirred at 60°C for 40 minutes, irradiated with a 300 W microwave for 2 minutes, the pH is adjusted to neutral with a 1 mol / L sodium hydroxide solution, dialyzed with a 10000 Da dialysis bag, dried, and crushed to less than 500 meshes to obtain the fibrous soy protein.
[0084] The zirconium oxide composite graphene oxide is prepared by the following method: firstly, zirconium oxide, graphene oxide and sodium bromide are crushed to 500 meshes according to a mass ratio of 30:170:9 and mixed to obtain mixed powder; then, the temperature is raised to 1200°C at 3°C / min in a nitrogen atmosphere, and the mixture is kept warm and calcined for 6 hours, and naturally cooled to room temperature to obtain calcined powder; finally, the calcined powder is mixed with water of equal mass, subjected to 500W ultrasonic oscillation treatment for 30 minutes, centrifuged to obtain a precipitate, dried, and crushed to less than 500 meshes to obtain the obtained product.
[0085] The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 12 times its weight, let it stand for 2 hours, adjust the pH to 2 with a 20% mass concentration of formic acid aqueous solution, rotate the drum for 2 hours, and drain the liquid.
[0086] The degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract at a mass ratio of 12:100; wherein, the animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 0.2 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 9 with 1 mol / L sodium hydroxide solution. After the addition is completed, the mixture is stirred for 3 hours to obtain the animal fur waste extract.
[0087] The specific method of washing is: first wash the degreased leather twice with twice its mass of water to obtain pre-washed leather; then add the pre-washed leather into twice its mass of water, adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather twice with twice its mass of water.
[0088] The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 20Pa, power is 200W, and treatment time is 30s.
[0089] The specific method of retanning is: soak the leather treated with low-temperature plasma in 40°C water twice its weight for 40 minutes, add the retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:0.8.
[0090] The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.3, the gas pressure is 100Pa, the power is 300W, and the treatment time is 2 minutes.
[0091] The specific method of fatliquoring is: soak the leather after retanning in 60°C water twice its weight for 20 minutes, add fatliquor, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.3. The fatliquor is prepared by mixing 1 kg of castor oil phosphate, 1 kg of neat's foot oil, 0.1 kg of animal fur waste extract, and 0.3 kg of polyethylene glycol 400 dioleate.
[0092] The animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated at 95° C. with stirring for 6 hours, the filtrate is filtered while hot, and vacuum freeze-dried to obtain the extract.
[0093] Comparative Example 3 A method for preparing wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is obtained by mixing 1kg of ricinoleic acid modified polyurethane, 0.1kg of polyhedral oligomeric silsesquioxane and 0.2kg of fibrous soy protein.
[0094] The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, 1.6 kg of toluene diisocyanate and 0.5 kg of polytetramethylene glycol are uniformly mixed at 70° C., 0.05 kg of dibutyltin dilaurate is added, and the mixture is polymerized for 2 hours under heat preservation, heated to 90° C., 0.3 kg of 2,2-dihydroxymethylpropionic acid and 0.3 kg of N-methyldiethanolamine are added, and the mixture is reacted for 2 hours under heat preservation, 0.2 kg of ricinoleic acid is added, and the mixture is reacted for 2 hours under heat preservation, naturally cooled to below 45° C., neutralized with triethylamine, and emulsified with distilled water to obtain a ricinoleic acid modified polyurethane with a mass solid content of 35%.
[0095] Polyhedral oligomeric silsesquioxane is prepared by the following method: first, 0.5 kg of γ-aminopropyltriethoxysilane is uniformly mixed with 2 L of cyclohexane, then 0.3 L of 30% hydrochloric acid solution is added, heated to 60° C., kept warm for 55 hours, and the solvent is evaporated under reduced pressure to obtain the polyhedral oligomeric silsesquioxane.
[0096] The fibrous soy protein is prepared by the following method: first, the soy protein is ultrasonically dispersed in 25 times its weight of water, the pH is adjusted to 11 with a 1 mol / L sodium hydroxide solution, heated at 80°C for 10 minutes, and the supernatant is taken by centrifugation to obtain a soy protein solution; then, the soy protein solution is mixed with an equal volume of a 0.6 mol / L tartaric acid solution, stirred at 60°C for 40 minutes, irradiated with a 300 W microwave for 2 minutes, the pH is adjusted to neutral with a 1 mol / L sodium hydroxide solution, dialyzed with a 10000 Da dialysis bag, dried, and crushed to less than 500 meshes to obtain the fibrous soy protein.
[0097] The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 12 times its weight, let it stand for 2 hours, adjust the pH to 2 with a 20% mass concentration of formic acid aqueous solution, rotate the drum for 2 hours, and drain the liquid.
[0098] The degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract at a mass ratio of 12:100; wherein, the animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 0.2 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 9 with 1 mol / L sodium hydroxide solution. After the addition is completed, the mixture is stirred for 3 hours to obtain the animal fur waste extract.
[0099] The specific method of washing is: first wash the degreased leather twice with twice its mass of water to obtain pre-washed leather; then add the pre-washed leather into twice its mass of water, adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather twice with twice its mass of water.
[0100] The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 20Pa, power is 200W, and treatment time is 30s.
[0101] The specific method of retanning is: soak the leather treated with low-temperature plasma in 40°C water twice its weight for 40 minutes, add the retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:0.8.
[0102] The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.3, the gas pressure is 100Pa, the power is 300W, and the treatment time is 2 minutes.
[0103] The specific method of fatliquoring is: soak the leather after retanning in 60°C water twice its weight for 20 minutes, add fatliquor, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.3. The fatliquor is prepared by mixing 1 kg of castor oil phosphate, 1 kg of neat's foot oil, 0.1 kg of animal fur waste extract, and 0.3 kg of polyethylene glycol 400 dioleate.
[0104] The animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated at 95° C. with stirring for 6 hours, the filtrate is filtered while hot, and vacuum freeze-dried to obtain the extract.
[0105] Comparative Example 4 A method for preparing wear-resistant leather fabric comprises the following steps: degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment of animal rawhide in sequence; wherein the retanning agent used in the retanning is ricinoleic acid modified polyurethane.
[0106] The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, 1.6 kg of toluene diisocyanate and 0.5 kg of polytetramethylene glycol are uniformly mixed at 70° C., 0.05 kg of dibutyltin dilaurate is added, and the mixture is polymerized for 2 hours under heat preservation, heated to 90° C., 0.3 kg of 2,2-dihydroxymethylpropionic acid and 0.3 kg of N-methyldiethanolamine are added, and the mixture is reacted for 2 hours under heat preservation, 0.2 kg of ricinoleic acid is added, and the mixture is reacted for 2 hours under heat preservation, naturally cooled to below 45° C., neutralized with triethylamine, and emulsified with distilled water to obtain a ricinoleic acid modified polyurethane with a mass solid content of 35%.
[0107] The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 12 times its weight, let it stand for 2 hours, adjust the pH to 2 with a 20% mass concentration of formic acid aqueous solution, rotate the drum for 2 hours, and drain the liquid.
[0108] The degreasing agent solution is obtained by uniformly mixing decyl glucoside and animal fur waste extract at a mass ratio of 12:100; wherein, the animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated with stirring at 95°C for 6 hours, the filtrate is filtered while hot, naturally cooled to 60°C, 0.2 mL of lauroyl chloride is added dropwise to the filtrate, and the pH is controlled to 9 with 1 mol / L sodium hydroxide solution. After the addition is completed, the mixture is stirred for 3 hours to obtain the animal fur waste extract.
[0109] The specific method of washing is: first wash the degreased leather twice with twice its mass of water to obtain pre-washed leather; then add the pre-washed leather into twice its mass of water, adjust the pH to 7, stir at 35°C for 1 hour, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather twice with twice its mass of water.
[0110] The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 20Pa, power is 200W, and treatment time is 30s.
[0111] The specific method of retanning is: soak the leather treated with low-temperature plasma in 40°C water twice its weight for 40 minutes, add the retanning agent, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:0.8.
[0112] The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.3, the gas pressure is 100Pa, the power is 300W, and the treatment time is 2 minutes.
[0113] The specific method of fatliquoring is: soak the leather after retanning in 60°C water twice its weight for 20 minutes, add fatliquor, rotate the drum for 2 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.3. The fatliquor is prepared by mixing 1 kg of castor oil phosphate, 1 kg of neat's foot oil, 0.1 kg of animal fur waste extract, and 0.3 kg of polyethylene glycol 400 dioleate.
[0114] The animal fur waste extract is prepared by the following method: first, 3 kg of animal fur waste is added to 2 kg of 1 mol / L sodium hydroxide solution, heated at 95° C. with stirring for 6 hours, the filtrate is filtered while hot, and vacuum freeze-dried to obtain the extract.
[0115] The performance tests were performed on the leather fabrics obtained in Examples 1 to 3 and Comparative Examples 1 to 4, respectively, and the specific methods are as follows: 1. Wear resistance: Martindale friction tester was used, referring to QB / T 2726-2005 "Determination of wear resistance of leather by physical and mechanical tests". The mass m1 of the sample was weighed before the test, and then the sample was fixed on the test instrument and pressed with a grinding wheel. The speed was set to 1000r / min. After the test, the mass m2 of the sample was weighed again, and the mass loss before and after wear was calculated, that is, the difference between m1 and m2.
[0116] 2. Softness: Refer to GB / T 39371-2020 "Determination of softness of leather - physical and mechanical tests" for softness test (the circular hole diameter is 25mm).
[0117] The performance test results are shown in Table 1.
[0118] Table 1. Performance test results
[0119] It can be seen from Table 1 that the leather fabrics obtained in Examples 1 to 3 have excellent wear resistance and good softness.
[0120] In Comparative Example 1, the fiberized soy protein was omitted, in Comparative Example 2, the polyhedral oligomeric silsesquioxane was omitted, in Comparative Example 3, the zirconium oxide composite graphene oxide was omitted, and in Comparative Example 4, the polyhedral oligomeric silsesquioxane, fiberized soy protein, and zirconium oxide composite graphene oxide were omitted. The wear resistance and softness were significantly deteriorated, indicating that the fiberized soy protein synergistically improves the wear resistance with the polyhedral oligomeric silsesquioxane, zirconium oxide composite graphene oxide, etc., and has good compatibility with animal skin components. It is cross-linked into a network structure through hydrogen bonding, etc., and the product has better softness.
[0121] The present invention illustrates the technical concept of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of individual raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a wear-resistant leather fabric, It is characterized in that The animal hides and skins are sequentially subjected to degreasing, washing, first low-temperature plasma treatment, retanning, second low-temperature plasma treatment, fatliquoring, dyeing and color fixing treatment; wherein the retanning agent used in the retanning is a mixture of ricinoleic acid-modified polyurethane, polyhedral oligomeric silsesquioxane, fibrous soy protein, and zirconium oxide composite graphene oxide in a mass ratio of 1:0.1-0.2:0.2-0.3:0.1-0.
2.
2. The preparation method according to claim 1, It is characterized in that The animal hide is selected from any one of cow hide, pig hide and sheep hide.
3. The preparation method according to claim 1, It is characterized in that The ricinoleic acid modified polyurethane is prepared by the following method: first, under nitrogen protection, toluene diisocyanate and polytetrahydrofuran diether alcohol are uniformly mixed at 70-80°C, dibutyltin dilaurate is added, heat preservation polymerization is carried out for 2-3 hours, heating is carried out to 90-100°C, 2,2-dihydroxymethylpropionic acid and N-methyldiethanolamine are added, heat preservation reaction is carried out for 2-3 hours, ricinoleic acid is added, heat preservation reaction is carried out for 2-3 hours, naturally cooled to below 45°C, neutralized with triethylamine, emulsified with distilled water, and ricinoleic acid modified polyurethane with a mass solid content of 35-40% is obtained; wherein the mass ratio of toluene diisocyanate, polytetrahydrofuran diether alcohol, dibutyltin dilaurate, 2,2-dihydroxymethylpropionic acid, N-methyldiethanolamine, and ricinoleic acid is 16:5:0.5-0.8:3-4:3-4:2-3.
4. The preparation method according to claim 1, It is characterized in that The polyhedral oligomeric silsesquioxane is prepared by the following method: firstly, γ-aminopropyltriethoxysilane and cyclohexane are uniformly mixed, then a hydrochloric acid solution with a mass concentration of 30-40% is added, heated to 60-70°C, kept warm for reaction for 55-60 hours, and the solvent is evaporated under reduced pressure to obtain the polyhedral oligomeric silsesquioxane; wherein the usage ratio of γ-aminopropyltriethoxysilane, cyclohexane and hydrochloric acid solution is 5-6g: 20-30mL: 3-4mL.
5. The preparation method according to claim 1, It is characterized in that The fibrous soybean protein is prepared by the following method: firstly, ultrasonically dispersing the soybean protein in water of 25 to 30 times its weight, adjusting the pH value to 11 to 12 with a 1 to 2 mol / L sodium hydroxide solution, heating at 80 to 90° C. for 10 to 12 minutes, centrifuging and taking the supernatant to obtain a soybean protein solution; then, mixing the soybean protein solution with an equal volume of a 0.6 to 1 mol / L tartaric acid solution, stirring at 60 to 70° C. for 40 to 50 minutes, irradiating with a 300 to 500W microwave for 2 to 3 minutes, adjusting the pH value to neutral with a 1 to 2 mol / L sodium hydroxide solution, dialyzing with a 10000 to 12000Da dialysis bag, drying, and crushing to less than 500 meshes to obtain the fibrous soybean protein.
6. The preparation method according to claim 1, It is characterized in that The zirconium oxide composite graphene oxide is prepared by the following method: firstly, zirconium oxide, graphene oxide and sodium bromide are crushed to 500 meshes according to a mass ratio of 30-40:170-180:9-10 and mixed to obtain mixed powder; then, in a nitrogen atmosphere, the temperature is raised to 1200-1300°C at 3-5°C / min, the mixture is kept warm and calcined for 6-7 hours, and naturally cooled to room temperature to obtain calcined powder; finally, the calcined powder is mixed with water of equal mass, subjected to 500-600W ultrasonic oscillation treatment for 30-40 minutes, centrifuged to obtain a precipitate, dried, and crushed to less than 500 meshes to obtain the obtained product.
7. The preparation method according to claim 1, It is characterized in that The specific method of degreasing is: after washing the animal rawhide, completely immerse it in a degreasing agent solution of 12 to 15 times its weight, let it stand for 2 to 3 hours, adjust the pH to 2 to 3 with a 20 to 30% mass concentration of formic acid aqueous solution, rotate the drum for 2 to 3 hours, and drain the liquid.
8. The preparation method according to claim 1, It is characterized in that The specific method of washing is: first wash the defatted leather with 2 to 3 times the weight of water for 2 to 3 times to obtain pre-washed leather; then add the pre-washed leather into 2 to 3 times the weight of water, adjust the pH to 7, stir at 35 to 40°C for 1 to 2 hours, drain, and obtain neutralized washed leather; finally, wash the neutralized washed leather with 2 to 3 times the weight of water for 2 to 3 times.
9. The preparation method according to claim 1, It is characterized in that The process conditions of the first low-temperature plasma treatment are: working atmosphere is oxygen, gas pressure is 20-30 Pa, power is 200-300 W, and treatment time is 30-40 s; The specific method of retanning is: soak the leather treated with low-temperature plasma in 40-50°C water of 2-3 times its weight for 40-50 minutes, add retanning agent, rotate the drum for 2-3 hours, and drain the liquid; the mass ratio of the leather treated with low-temperature plasma to the retanning agent is 1:0.8-1; The process conditions of the second low-temperature plasma treatment are: the working atmosphere is nitrogen and oxygen, the volume ratio of the two is 1:0.3-0.5, the gas pressure is 100-120Pa, the power is 300-400W, and the treatment time is 2-3 minutes; The specific method of fatliquoring is: soak the leather after retanning in 60-65°C water which is 2-3 times of its weight for 20-30 minutes, add fatliquor, rotate the drum for 2-3 hours, and drain the liquid; the mass ratio of the leather after retanning to the fatliquor is 100:0.3-0.
4.
10. A wear-resistant leather fabric, It is characterized in that The invention is obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Vegetable oil derivative modified amphoteric polyurethane retanning agent and preparation method thereof
CN111777738A
Preparation method of wear-resistant and tear-resistant finishing auxiliary agent for leather
CN115304991A
Processing technology for regulating soybean protein gel structure based on salt ion step-by-step induction
CN117502554A
Leather modifier
JP2007091864A